Copper-tetracyano p-benzoquinone dimethane catalyst as well as preparation method and application thereof

Through the nanorod-like structure of the copper-tetracyano-p-benzoquinonedimethane catalyst, the problem of low efficiency of electrocatalytic nitrate reduction reaction is solved, and efficient ammonia product generation and catalyst stability are achieved.

CN118957679APending Publication Date: 2024-11-15SHANGHAI UNIV (JIAXING ZHEJIANG) EMERGING IND RES INST +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411179841.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The current electrocatalytic nitrate reduction reaction has low efficiency and is unfavorable thermodynamics, which leads to the overpotential of ammonia products being lower than that of nitrogen, making it difficult to effectively separate nitrate and hydrogen protons, affecting Faraday efficiency.

Method used

The nanorod-shaped catalyst is prepared by a mixed solvent method of acetonitrile, ethanol and water by using copper-tetracyanoparabenone dimethane catalyst to increase the active site, improve the stability and catalytic effect of the catalyst, and is used for electrocatalytic reduction of nitrates. reaction.

Benefits of technology

The conversion rate and ammonia yield of nitrate are significantly improved, and the ammonia Faraday efficiency reaches 98.57%, and the stability and catalytic effect of the catalyst are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957679A_ABST
    Figure CN118957679A_ABST
Patent Text Reader

Abstract

The invention provides a copper-tetracyano p-benzoquinone dimethane catalyst as well as a preparation method and application thereof, and belongs to the field of electrocatalysts. The method comprises the following steps: mixing acetonitrile, ethanol and water according to a set volume ratio to obtain a mixed solvent; dissolving tetracyano p-benzoquinone dimethane in the mixed solution to obtain a reaction solution; and porous foamy copper is added into the reaction liquid for a reaction, and the copper-tetracyano p-benzoquinone dimethane growing on at least part of the surface of the porous foamy copper is obtained. According to the copper-tetracyano-p-benzoquinone dimethane nanorod catalyst, the crystallization and dissolution balance of copper-tetracyano-p-benzoquinone dimethane can be effectively controlled through the reasonable proportion of acetonitrile, ethyl alcohol and water, the length of the prepared copper-tetracyano-p-benzoquinone dimethane nanorod catalyst is increased, the particle size of the prepared copper-tetracyano-p-benzoquinone dimethane nanorod catalyst is reduced, more active sites can be obviously exposed, and the catalytic effect of the catalyst can be effectively promoted. Therefore, the efficiency of the electro-catalysis nitrate reduction reaction is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of electrocatalysts, and in particular to a copper-tetracyano-p-benzoquinodimethane catalyst, a preparation method and an application thereof. Background Art

[0002] Ammonia is an indispensable substance in the development of modern industry and agriculture. It can be used in nitrogen fertilizer production, industrial product manufacturing, hydrogen storage medium, fuel cells, etc. It can also be used as an ideal carbon-neutral energy fuel. At present, the synthesis of ammonia mainly relies on the high-temperature and high-pressure Haber-Bosch process. This method is highly dependent on fossil energy and produces a large amount of carbon dioxide, which is contrary to the "dual carbon" goal proposed by my country. With the rapid development of clean energy projects such as high-power offshore wind power, high-efficiency photovoltaic power generation, and advanced nuclear power in our province, the use of green electricity for ammonia production has received more and more attention. Influenced by the Haber-Bosch process, nitrogen was selected as the nitrogen source for electrocatalytic ammonia production. Due to the high N≡N bond energy, the ammonia production rate is low. Nitrate is the main pollutant in environmental water bodies. With the development of social economy, human activities (such as: the combustion of fossil fuels, excessive use of nitrogen-rich fertilizers and wastewater discharge) have accelerated the accumulation of nitrates in water bodies. High concentrations of nitrates can lead to eutrophication of water bodies and damage the aquatic ecosystem. In addition, nitrates ingested by the human body can cause liver damage, methemoglobinemia and even cancer. The National Health Commission also attaches great importance to this. The latest "Sanitary Standards for Drinking Water" (GB5749-2022) stipulates that the maximum content in water sources shall not exceed 10 mg·L -1 . Safe drinking water is the basic guarantee for human health, and the removal of nitrates, a water pollutant, is a hot topic in environmental research. Traditional nitrate removal methods are mainly divided into physical methods and chemical methods. Physical methods (such as reverse osmosis, ion exchange, adsorption, electrodialysis, etc.) can only be used for nitrate separation and have low economic efficiency; chemical methods (such as biological denitrification, photo / electrocatalytic reduction) convert nitrates into other products by supplying electrons to nitrates. Electrocatalytic nitrate reduction can generate ammonia. This method is conducive to improving pollution control and waste resource utilization, achieving the effect of extending to high-end industries in the value chain, and enhancing the sustainability of economic growth and social development.

[0003] There are two difficulties in the electrocatalytic nitrate reduction reaction in aqueous media: one is the competition of hydrogen evolution reaction. When testing the catalytic nitrate reduction to produce ammonia, the protons in the electrolyte will compete with nitrates for adsorption on the catalytic active sites, and hydrogen evolution reaction will occur to produce hydrogen, consuming the supplied electrons, which will reduce the Faraday efficiency; the second is that the reaction thermodynamics is unfavorable. Nitrate reduction has two reaction pathways, eight electrons and five electrons. The product of the eight electron pathway is ammonia, and the electrochemical reaction overpotential is 1.20V. The product of the five electron pathway is nitrogen, and the electrochemical reaction overpotential is 1.25V. It can be seen that the overpotential for the production of ammonia is lower than that of nitrogen. Thermodynamically, the possibility of nitrate reduction to nitrogen is better than that of ammonia. Therefore, the constructed catalyst material is required to have a stronger adsorption effect on nitrate than hydrogen protons, and at the same time, the selectivity for the eight electron pathway of nitrate reduction is high, so as to finally achieve the generation of ammonia products. Therefore, it is urgent to develop a catalyst that can improve the efficiency of the electrocatalytic nitrate reduction reaction. Summary of the invention

[0004] The present application provides a copper-tetracyano-p-benzoquinodimethane catalyst and a preparation method and application thereof to solve the following technical problem: how to improve the efficiency of the electrocatalytic nitrate reduction reaction.

[0005] In a first aspect, the present application provides a method for preparing a copper-tetracyano-p-benzoquinodimethane catalyst, the method comprising:

[0006] Mixing acetonitrile, ethanol and water according to a set volume ratio to obtain a mixed solvent;

[0007] dissolving tetracyano-p-benzoquinodimethane in the mixed solution to obtain a reaction solution; and

[0008] The porous copper foam is added into the reaction solution to react and obtain copper-tetracyano-p-benzoquinodimethane grown on at least a portion of the surface of the porous copper foam.

[0009] Optionally, in the mixed solvent, the volume proportion of the acetonitrile is ≥70% and <100%, and the sum of the volume proportions of the ethanol and the water is >0 and ≤30%.

[0010] Optionally, in the reaction solution, the concentration of tetracyano-p-benzoquinodimethane is 0.25 g·L -1 ~1.0g·L -1 .

[0011] Optionally, the reaction temperature is room temperature, the reaction pressure is normal pressure, and the reaction time is 0.5h to 2h.

[0012] Optionally, before adding the porous copper foam to the reaction solution, the method includes:

[0013] The porous copper foam is sequentially immersed in acetone, dilute hydrochloric acid and ethanol solution to remove surface impurities of the porous copper foam.

[0014] In the second aspect, the present application provides a copper-tetracyanobenzoquinone dimethane catalyst prepared by the method described in any one of the embodiments of the first aspect, wherein the copper-tetracyanobenzoquinone dimethane catalyst is in the shape of a nanorod, and the diameter of the nanorod of the copper-tetracyanobenzoquinone dimethane catalyst is 50nm to 500nm.

[0015] In a third aspect, the present application provides an application of the copper-tetracyano-p-benzoquinodimethane catalyst as described in the embodiment of the second aspect in nitrate reduction to produce ammonia, the application comprising:

[0016] The copper-tetracyano-p-benzoquinodimethane catalyst is used as a working electrode to electrocatalytically reduce nitrate to obtain an ammonia product.

[0017] Optionally, the electrolyte used in the electrocatalytic reduction is a mixed solution of sodium nitrate and sodium sulfate, and the concentration of the sodium nitrate is 0.01 mol·L -1 ~0.5mol·L -1 The concentration of sodium sulfate is 0.1 mol·L -1 ~0.5mol·L -1 .

[0018] Optionally, the electrocatalytic reduction includes the following parameters: voltage is -0.6V to -1.3V, and time is 1h to 2h.

[0019] Optionally, the electrocatalytic reduction of nitrates satisfies at least one of the following properties: nitrate conversion rate ≥ 55%, ammonia yield ≥ 100 mmol·mg cat . -1 ·h -1 , ammonia Faraday efficiency ≥ 65%.

[0020] The above technical solution provided by the embodiment of the present application has the following advantages compared with the prior art:

[0021] The present application provides a method for preparing a copper-tetracyano-p-benzoquinone dimethane catalyst, comprising: mixing acetonitrile, ethanol and water according to a set volume ratio to obtain a mixed solvent; dissolving tetracyano-p-benzoquinone dimethane in the mixed solution to obtain a reaction solution; and adding porous copper foam to the reaction solution to react and obtain copper-tetracyano-p-benzoquinone dimethane grown on at least part of the surface of the porous copper foam. Through the reasonable ratio of acetonitrile, ethanol and water, due to the effect of multiple solvents, the crystallization and dissolution equilibrium of copper-tetracyano-p-benzoquinone dimethane can be effectively controlled, and the length of the prepared copper-tetracyano-p-benzoquinone dimethane nanorod catalyst increases and the particle size decreases, which can significantly expose more active sites and effectively promote the catalytic effect of the catalyst. Compared with the traditional pure acetonitrile solution method for synthesizing copper-tetracyano-p-benzoquinone dimethane catalyst, the stability of the copper-tetracyano-p-benzoquinone dimethane catalyst synthesized by the mixed solvent method is also improved, which can provide a better catalytic environment for the next step of catalyst application. Thereby improving the efficiency of the electrocatalytic nitrate reduction reaction. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.

[0023] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.

[0024] Figure 1 A schematic flow chart of a method for preparing a copper-tetracyano-p-benzoquinodimethane catalyst provided in an embodiment of the present application;

[0025] Figure 2 This is a scanning electron microscope image of the copper-tetracyano-p-benzoquinodimethane catalyst provided in Example 1 of the present application;

[0026] Figure 3 This is a scanning electron microscope image of the copper-tetracyano-p-benzoquinodimethane catalyst provided in Example 2 of the present application;

[0027] Figure 4 This is a scanning electron microscope image of the copper-tetracyano-p-benzoquinodimethane catalyst provided in Example 3 of the present application;

[0028] Figure 5 A scanning electron microscope image of the copper-tetracyano-p-benzoquinodimethane catalyst provided in Example 4 of the present application;

[0029] Figure 6A scanning electron microscope image of the copper-tetracyano-p-benzoquinodimethane catalyst provided in Example 5 of the present application;

[0030] Figure 7 A scanning electron microscope image of the copper-tetracyano-p-benzoquinodimethane catalyst provided in Example 6 of the present application;

[0031] Figure 8 A scanning electron microscope image of the copper-tetracyano-p-benzoquinodimethane catalyst provided in Example 7 of the present application;

[0032] Fig. 9 This is a scanning electron microscope image of the copper-tetracyano-p-benzoquinodimethane catalyst provided in Example 8 of the present application;

[0033] Fig.10 A scanning electron microscope image of the copper-tetracyano-p-benzoquinodimethane catalyst provided in Example 9 of the present application;

[0034] Fig.11 This is a scanning electron microscope image of the copper-tetracyanobenzoquinodimethane catalyst provided in Comparative Example 1 of the present application. DETAILED DESCRIPTION

[0035] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.

[0036] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present application; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values ​​within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.

[0037] In addition, in the description of the specification of the present application, the terms "including", "comprising", etc. mean "including but not limited to". In this article, relational terms such as "first" and "second", etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. In this article, "and / or" describes the association relationship of associated objects, indicating that three relationships may exist. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. Wherein A and B can be singular or plural. In this article, "at least one" means one or more, and "plurality" means two or more. "At least one", "the following at least one item (items)" or similar expressions refer to any combination of these items, including any combination of single items (items) or plural items (items). For example, "at least one of a, b, or c", or "at least one of a, b and c", can both mean: a, b, c, ab (i.e. a and b), ac, bc or abc, where a, b, c can be single or plural, respectively.

[0038] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.

[0039] Figure 1 A schematic flow chart of a method for preparing a copper-tetracyanoquinodimethane catalyst provided in an embodiment of the present application.

[0040] In a first aspect, the present application provides a method for preparing a copper-tetracyano-p-benzoquinodimethane catalyst, the method comprising:

[0041] S1, mixing acetonitrile, ethanol and water according to a set volume ratio to obtain a mixed solvent;

[0042] The present application uses a reasonable ratio of reaction solvents acetonitrile, ethanol and water, and due to the effect of multiple solvents, can effectively control crystallization and dissolution equilibrium, and the length of the prepared copper-tetracyano-p-benzoquinone dimethane nanorod catalyst is increased and the particle size is reduced, which can significantly expose more active sites and effectively promote the catalytic effect of the catalyst. Compared with the traditional pure acetonitrile solution method to synthesize copper-tetracyano-p-benzoquinone dimethane catalyst, the stability of the copper-tetracyano-p-benzoquinone dimethane catalyst synthesized by the mixed solvent method is also improved, which can provide a better catalytic environment for the next step of catalyst application.

[0043] It should be noted that the order of adding the mixed solvent is: first adding ethanol to the acetonitrile solvent, and then adding water to the mixed solvent.

[0044] In some embodiments, in the mixed solvent, the volume proportion of the acetonitrile is ≥70% and <100%, and the sum of the volume proportions of the ethanol and the water is >0 and ≤30%.

[0045] It should be noted that the sum of the volume percentages of ethanol and the water is >0 and ≤30%, which may be ethanol's volume percentage >0 and ≤30%, water's volume percentage >0 and ≤30%, or ethanol and water mixed in any proportion and the sum of the volume percentages >0 and ≤30%. In the above embodiment, by controlling the volume percentages of each solvent in the mixed solvent, the crystallization and dissolution equilibrium of the catalyst product can be effectively controlled while ensuring that tetracyano-p-benzoquinone dimethane is completely dissolved. Exemplarily, the volume percentage of acetonitrile can be 70%, 75%, 80%, 85%, 90%, 95%, etc., and the sum of the volume percentages of ethanol and water can be 5%, 10%, 15%, 20%, 25%, 30%, etc.

[0046] S2, dissolving tetracyano-p-benzoquinodimethane in the mixed solution to obtain a reaction solution;

[0047] In some embodiments, in the reaction solution, the concentration of tetracyano-p-benzoquinodimethane is 0.25 g·L -1 ~1.0g·L -1 .

[0048] In the above embodiment, controlling the concentration of tetracyano-p-benzoquinodimethane can ensure that tetracyano-p-benzoquinodimethane is completely dissolved and that the reaction of generating the copper-tetracyano-p-benzoquinodimethane catalyst proceeds smoothly. For example, the concentration of tetracyano-p-benzoquinodimethane can be 0.25 g·L -1 , 0.3g·L -1 , 0.4g·L -1 , 0.5g·L -1 , 0.7 g·L -1 , 0.9g·L -1 , 1.0g·L -1 wait.

[0049] S3, adding porous copper foam to the reaction solution to react and obtain copper-tetracyano-p-benzoquinodimethane grown on at least a portion of the surface of the porous copper foam.

[0050] In some embodiments, before adding the porous copper foam to the reaction solution, the method includes: soaking the porous copper foam in acetone, dilute hydrochloric acid, and ethanol solutions in sequence to remove surface impurities of the porous copper foam.

[0051] In some embodiments, the reaction temperature is room temperature, the reaction pressure is normal pressure, and the reaction time is 0.5 h to 2 h.

[0052] In the above embodiment, normal temperature is also called general temperature or room temperature, which is generally defined as about 25° C. The crystal growth of the catalyst tends to be balanced within this range. For example, the reaction time can be 0.5 h, 0.8 h, 1 h, 1.2 h, 1.5 h, 2 h, etc.

[0053] In some embodiments, the method further comprises: washing the copper-tetracyanobenzoquinodimethane catalyst grown on the surface of the porous copper foam with ethanol and water in sequence, and drying it in a vacuum oven at a temperature of 60°C to 80°C for a drying time of 12h to 24h.

[0054] Based on a general inventive concept, the present application provides a copper-tetracyanobenzoquinone dimethane catalyst prepared by the method described in any one of the above embodiments, wherein the copper-tetracyanobenzoquinone dimethane catalyst is in the shape of a nanorod, and the diameter of the nanorod of the copper-tetracyanobenzoquinone dimethane catalyst is 50nm to 500nm.

[0055] Compared with the traditional pure acetonitrile solution method for synthesizing copper-tetracyano-p-benzoquinodimethane catalyst, the copper-tetracyano-p-benzoquinodimethane nanorod catalyst prepared in the present application has an increased length and a reduced particle size, which can significantly expose more active sites and effectively promote the catalytic effect of the catalyst. Exemplarily, the diameter of the nanorod of the copper-tetracyano-p-benzoquinodimethane catalyst can be 50nm, 100nm, 200nm, 300nm, 400nm, 500nm, etc.

[0056] The copper-tetracyano-p-benzoquinone dimethane catalyst is realized based on the preparation method of the copper-tetracyano-p-benzoquinone dimethane catalyst. The specific steps of the preparation method of the copper-tetracyano-p-benzoquinone dimethane catalyst can refer to the above embodiment. Since the copper-tetracyano-p-benzoquinone dimethane catalyst adopts part or all of the technical solutions of the above embodiment, it at least has all the beneficial effects brought by the technical solutions of the above embodiment, which will not be repeated here one by one.

[0057] Based on a general inventive concept, the present application provides an application of a copper-tetracyano-p-benzoquinodimethane catalyst as described in the above embodiment in nitrate reduction to produce ammonia, the application comprising:

[0058] The copper-tetracyano-p-benzoquinodimethane catalyst is used as a working electrode to electrocatalytically reduce nitrate to obtain an ammonia product.

[0059] In some embodiments, the electrolyte used in the electrocatalytic reduction is a mixed solution of sodium nitrate and sodium sulfate, and the concentration of the sodium nitrate is 0.01 mol·L -1 ~0.5mol·L -1The concentration of sodium sulfate is 0.1 mol·L -1 ~0.5mol·L -1 .

[0060] In some embodiments, the electrocatalytic reduction includes the following parameters: voltage is -0.6V to -1.3V, and time is 1h to 2h.

[0061] In the above embodiment, when the voltage is higher than -0.6V, nitrate begins to undergo reduction reaction, and when the voltage is higher than -1.3V, the nitrate reduction process is inhibited by side reactions (such as hydrogen evolution reaction). At the same time, nitrate can be completely consumed within this time. Exemplarily, the voltage can be -0.6V, -0.7V, -0.9V, -1.0V, -1.2V, -1.3V, etc., and the time can be 1h, 1.2h, 1.4h, 1.6h, 1.8h, 2h, etc.

[0062] In some embodiments, the electrocatalytic reduction of nitrate satisfies at least one of the following properties: nitrate conversion rate ≥ 55%, ammonia yield ≥ 100 mmol·mg cat . -1 ·h -1 , ammonia Faraday efficiency ≥ 65%.

[0063] This application firstly applies copper-tetracyano-p-benzoquinodimethane nanorod catalyst to electrocatalytic nitrate reduction to produce ammonia, and obtains excellent catalytic performance. The conversion rate of nitrate can reach up to 99.87%, and the ammonia production rate can reach up to 309.6mmol·mg cat. -1 ·h -1 , the ammonia Faraday efficiency can reach up to 98.57%.

[0064] The present application will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are intended only to illustrate the present application and are not intended to limit the scope of the present application. The experimental methods for which specific conditions are not specified in the following examples are usually measured according to industry standards. If there is no corresponding industry standard, then the conditions recommended by the manufacturer are followed.

[0065] Example 1

[0066] A method for preparing a copper-tetracyano-p-benzoquinodimethane catalyst, exemplarily comprising the following steps:

[0067] (1) acetonitrile, ethanol and water are mixed in a certain proportion as a solvent, wherein the volumes of acetonitrile, ethanol and water are 9 mL, 0.5 mL and 0.5 mL respectively, and the order is that ethanol is first added to the acetonitrile solvent, and then water is added to the above mixed solvent;

[0068] (2) Dissolve 0.5 mg of tetracyano-p-benzoquinodimethane in the above solvent to prepare a reaction solution. The concentration of tetracyano-p-benzoquinodimethane is 0.05 g·L -1 ;

[0069] (3) soaking the porous copper foam in acetone, dilute hydrochloric acid and ethanol solutions in turn to remove surface impurities, then rinsing with water, and then placing it in the above reaction solution to react at room temperature and pressure for 1 hour. After the reaction is completed;

[0070] (4) The obtained product was washed with ethanol and water three times in sequence, and dried in a vacuum oven at a temperature of 60 degrees Celsius for 12 hours to obtain a copper-tetracyanobenzoquinone dimethane nanorod catalyst.

[0071] Based on the above scheme, 0.01 mol·L -1 of sodium nitrate and 0.1 mol·L -1 The sodium sulfate mixed solution was used as the electrolyte, the copper-tetracyano-p-benzoquinone dimethane catalyst was used as the working electrode, the carbon rod was used as the counter electrode, and the Ag / AgCl electrode was used as the reference electrode to form a three-electrode test system. The voltage required for the reaction was provided by the electrochemical workstation. The voltage parameter was set on the computer control system, and the voltage parameter was set to -0.6V. The constant potential test was performed for 1 hour. After the test, the electrolyte was collected to detect the remaining amount of nitrate reactants and the content of ammonia products. Then, the conversion rate of nitrate ions was calculated to be 56.63%, and the ammonia yield was 105.4mmol·mg cat. -1 ·h -1 , the ammonia Faraday efficiency is 67.42%.

[0072] Example 2

[0073] A method for preparing a copper-tetracyano-p-benzoquinodimethane catalyst, exemplarily comprising the following steps:

[0074] (1) acetonitrile, ethanol and water are mixed in a certain proportion as a solvent, wherein the volumes of the acetonitrile, ethanol and water are 8 mL, 1 mL and 1 mL respectively, and the order is that ethanol is first added to the acetonitrile solvent, and then water is added to the mixed solvent;

[0075] (2) Dissolve 1 mg of tetracyano-p-benzoquinodimethane in the above solvent to prepare a reaction solution. The concentration of tetracyano-p-benzoquinodimethane is 0.1 g·L -1 ;

[0076] (3) soaking the porous copper foam in acetone, dilute hydrochloric acid and ethanol solutions in turn to remove surface impurities, then rinsing with water, and then placing it in the above reaction solution to react at room temperature and pressure for 1 hour. After the reaction is completed;

[0077] (4) The obtained product was washed with ethanol and water three times in sequence, and dried in a vacuum oven at a temperature of 60 degrees Celsius for 12 hours to obtain a copper-tetracyanobenzoquinone dimethane nanorod catalyst.

[0078] Based on the above scheme, 0.01 mol·L -1 of sodium nitrate and 0.1 mol·L -1 The sodium sulfate mixed solution was used as the electrolyte, the copper-tetracyano-p-benzoquinone dimethane catalyst was used as the working electrode, the carbon rod was used as the counter electrode, and the Ag / AgCl electrode was used as the reference electrode to form a three-electrode test system. The voltage required for the reaction was provided by the electrochemical workstation. The voltage parameter was set on the computer control system, and the voltage parameter was set to -0.7V. The constant potential test was performed for 1 hour. After the test, the electrolyte was collected, and the residual amount of nitrate reactants and the content of ammonia products were detected. Then, the conversion rate of nitrate ions was calculated to be 64.28%, and the ammonia yield was 185.2mmol·mg cat. -1 ·h -1 , the ammonia Faraday efficiency is 72.45%.

[0079] Example 3

[0080] A method for preparing a copper-tetracyano-p-benzoquinodimethane catalyst, exemplarily comprising the following steps:

[0081] (1) acetonitrile, ethanol and water are mixed in a certain proportion as a solvent, wherein the volumes of acetonitrile, ethanol and water are 8 mL, 1.5 mL and 0.5 mL respectively, and the order is that ethanol is first added to the acetonitrile solvent, and then water is added to the above mixed solvent;

[0082] (2) Dissolve 2 mg of tetracyano-p-benzoquinodimethane in the above solvent to prepare a reaction solution. The concentration of tetracyano-p-benzoquinodimethane is 0.2 g·L -1 ;

[0083] (3) soaking the porous copper foam in acetone, dilute hydrochloric acid and ethanol solutions in turn to remove surface impurities, then rinsing with water, and then placing it in the above reaction solution to react at room temperature and pressure for 1 hour. After the reaction is completed;

[0084] (4) The obtained product was washed with ethanol and water three times in sequence, and dried in a vacuum oven at a temperature of 70 degrees Celsius for 12 hours to obtain a copper-tetracyanobenzoquinone dimethane nanorod catalyst.

[0085] Based on the above scheme, 0.05 mol·L -1 of sodium nitrate and 0.1 mol·L -1 The sodium sulfate mixed solution was used as the electrolyte, the copper-tetracyano-p-benzoquinone dimethane catalyst was used as the working electrode, the carbon rod was used as the counter electrode, and the Ag / AgCl electrode was used as the reference electrode to form a three-electrode test system. The voltage required for the reaction was provided by the electrochemical workstation. The voltage parameter was set on the computer control system, and the voltage parameter was set to -0.6V. The constant potential test was performed for 1 hour. After the test, the electrolyte was collected to detect the remaining amount of nitrate reactants and the content of ammonia products. Then, the conversion rate of nitrate ions was calculated to be 78.23%, and the ammonia yield was 203.6mmol·mg cat. -1 ·h -1 , the ammonia Faraday efficiency is 75.38%.

[0086] Example 4

[0087] A method for preparing a copper-tetracyano-p-benzoquinodimethane catalyst, exemplarily comprising the following steps:

[0088] (1) acetonitrile, ethanol and water are mixed in a certain proportion as a solvent, wherein the volumes of the acetonitrile, ethanol and water are 7 mL, 2 mL and 1 mL respectively, and the order is that ethanol is first added to the acetonitrile solvent, and then water is added to the mixed solvent;

[0089] (2) Dissolve 5 mg of tetracyano-p-benzoquinodimethane in the above solvent to prepare a reaction solution. The concentration of tetracyano-p-benzoquinodimethane is 0.5 g·L -1 ;

[0090] (3) soaking the porous copper foam in acetone, dilute hydrochloric acid and ethanol solutions in turn to remove surface impurities, then rinsing with water, and then placing it in the above reaction solution to react at room temperature and pressure for 1 hour. After the reaction is completed;

[0091] (4) The obtained product was washed with ethanol and water three times in sequence, and dried in a vacuum oven at a temperature of 60 degrees Celsius for 12 hours to obtain a copper-tetracyano-p-benzoquinone dimethane nanorod catalyst. -1 of sodium nitrate and 0.5 mol·L -1The sodium sulfate mixed solution was used as the electrolyte, the copper-tetracyano-p-benzoquinone dimethane catalyst was used as the working electrode, the carbon rod was used as the counter electrode, and the Ag / AgCl electrode was used as the reference electrode to form a three-electrode test system. The voltage required for the reaction was provided by the electrochemical workstation. The voltage parameter was set on the computer control system, and the voltage parameter was set to -0.9V. The constant potential test was performed for 2 hours. After the test, the electrolyte was collected, and the residual amount of nitrate reactants and the content of ammonia products were detected. Then, the conversion rate of nitrate ions was calculated to be 84.32%, and the ammonia yield was 235.7mmol·mg cat. -1 ·h -1 , the ammonia Faraday efficiency is 75.42%.

[0092] Example 5

[0093] A method for preparing a copper-tetracyano-p-benzoquinodimethane catalyst, exemplarily comprising the following steps:

[0094] (1) acetonitrile, ethanol and water are mixed in a certain proportion as a solvent, wherein the volumes of acetonitrile, ethanol and water are 8 mL, 0.5 mL and 1.5 mL respectively, and the order is that ethanol is first added to the acetonitrile solvent, and then water is added to the above mixed solvent;

[0095] (2) Dissolve 5 mg of tetracyano-p-benzoquinodimethane in the above solvent to prepare a reaction solution. The concentration of tetracyano-p-benzoquinodimethane is 0.5 g·L -1 ;

[0096] (3) soaking the porous copper foam in acetone, dilute hydrochloric acid and ethanol solutions in turn to remove surface impurities, then rinsing with water, and then placing it in the above reaction solution to react at room temperature and pressure for 1 hour. After the reaction is completed;

[0097] (4) The obtained product was washed with ethanol and water three times in sequence, and dried in a vacuum oven at a temperature of 60 degrees Celsius for 24 hours to obtain a copper-tetracyanobenzoquinone dimethane nanorod catalyst.

[0098] Based on the above scheme, 0.01 mol·L -1 of sodium nitrate and 0.1 mol·L -1The sodium sulfate mixed solution was used as the electrolyte, the copper-tetracyano-p-benzoquinone dimethane catalyst was used as the working electrode, the carbon rod was used as the counter electrode, and the Ag / AgCl electrode was used as the reference electrode to form a three-electrode test system. The voltage required for the reaction was provided by the electrochemical workstation. The voltage parameter was set on the computer control system, and the voltage parameter was set to -1.2V. The constant potential test was performed for 1 hour. After the test, the electrolyte was collected, and the residual amount of the nitrate reactant and the content of the ammonia product were detected. Then, the conversion rate of nitrate ion was calculated to be 99.87%, and the ammonia yield was 309.6mmol·mg cat. -1 ·h -1 , the ammonia Faraday efficiency is 98.57%.

[0099] Example 6

[0100] A method for preparing a copper-tetracyano-p-benzoquinodimethane catalyst, exemplarily comprising the following steps:

[0101] (1) acetonitrile, ethanol and water are mixed in a certain proportion as a solvent, wherein the volumes of the acetonitrile, ethanol and water are 7 mL, 1 mL and 2 mL respectively, and the order is that ethanol is first added to the acetonitrile solvent, and then water is added to the mixed solvent;

[0102] (2) Dissolve 10 mg of tetracyano-p-benzoquinodimethane in the above solvent to prepare a reaction solution. The concentration of tetracyano-p-benzoquinodimethane is 1 g·L -1 ;

[0103] (3) soaking the porous copper foam in acetone, dilute hydrochloric acid and ethanol solutions in turn to remove impurities on the surface, rinsing with water, and then placing it in the above reaction solution to react at room temperature and pressure for 2 hours. After the reaction is completed;

[0104] (4) The obtained product was washed with ethanol and water three times in sequence, and dried in a vacuum oven at a temperature of 80 degrees Celsius for 12 hours to obtain a copper-tetracyanobenzoquinone dimethane nanorod catalyst.

[0105] Based on the above scheme, 0.05 mol·L -1 of sodium nitrate and 0.5 mol·L -1The sodium sulfate mixed solution was used as the electrolyte, the copper-tetracyano-p-benzoquinone dimethane catalyst was used as the working electrode, the carbon rod was used as the counter electrode, and the Ag / AgCl electrode was used as the reference electrode to form a three-electrode test system. The voltage required for the reaction was provided by the electrochemical workstation. The voltage parameter was set on the computer control system, and the voltage parameter was set to -1.3V. The constant potential test was performed for 1 hour. After the test, the electrolyte was collected to detect the remaining amount of nitrate reactants and the content of ammonia products. Then, the conversion rate of nitrate ions was calculated to be 86.97%, and the ammonia yield was 298.9mmol·mg cat. -1 ·h -1 , the ammonia Faraday efficiency is 74.91%.

[0106] Example 7

[0107] A method for preparing a copper-tetracyano-p-benzoquinodimethane catalyst, exemplarily comprising the following steps:

[0108] (1) acetonitrile, ethanol and water are mixed in a certain proportion as a solvent, wherein the volumes of acetonitrile, ethanol and water are 7 mL, 1.5 mL and 1.5 mL respectively, and the order is that ethanol is first added to the acetonitrile solvent, and then water is added to the above mixed solvent;

[0109] (2) Dissolve 5 mg of tetracyano-p-benzoquinodimethane in the above solvent to prepare a reaction solution. The concentration of tetracyano-p-benzoquinodimethane is 0.5 g·L -1 ;

[0110] (3) soaking the porous copper foam in acetone, dilute hydrochloric acid and ethanol solutions in turn to remove surface impurities, then rinsing with water, and then placing it in the above reaction solution to react at room temperature and pressure for 1 hour. After the reaction is completed;

[0111] (4) The obtained product was washed with ethanol and water three times in sequence, and dried in a vacuum oven at a temperature of 70 degrees Celsius for 24 hours to obtain a copper-tetracyanobenzoquinone dimethane nanorod catalyst.

[0112] Based on the above scheme, 0.05 mol·L -1 of sodium nitrate and 0.1 mol·L -1The sodium sulfate mixed solution was used as the electrolyte, the copper-tetracyano-p-benzoquinone dimethane catalyst was used as the working electrode, the carbon rod was used as the counter electrode, and the Ag / AgCl electrode was used as the reference electrode to form a three-electrode test system. The voltage required for the reaction was provided by the electrochemical workstation. The voltage parameter was set on the computer control system, and the voltage parameter was set to -1.1V. The constant potential test was performed for 2 hours. After the test, the electrolyte was collected, and the residual amount of nitrate reactants and the content of ammonia products were detected. Then, the conversion rate of nitrate ions was calculated to be 97.64%, and the ammonia yield was 285.4mmol·mg cat. -1 ·h -1 , the ammonia Faraday efficiency is 89.76%.

[0113] Example 8

[0114] A method for preparing a copper-tetracyano-p-benzoquinodimethane catalyst, exemplarily comprising the following steps:

[0115] (1) acetonitrile, ethanol and water are mixed in a certain proportion as a solvent, wherein the volumes of acetonitrile, ethanol and water are 7 mL, 1.5 mL and 1.5 mL respectively, and the order is that ethanol is first added to the acetonitrile solvent, and then water is added to the above mixed solvent;

[0116] (2) Dissolve 5 mg of tetracyano-p-benzoquinodimethane in the above solvent to prepare a reaction solution. The concentration of tetracyano-p-benzoquinodimethane is 0.5 g·L -1 ;

[0117] (3) soaking the porous copper foam in acetone, dilute hydrochloric acid and ethanol solutions in turn to remove surface impurities, then rinsing with water, and then placing it in the above reaction solution to react at room temperature and pressure for 1 hour. After the reaction is completed;

[0118] (4) The obtained product was washed with ethanol and water three times in sequence, and dried in a vacuum oven at a temperature of 80 degrees Celsius for 12 hours to obtain a copper-tetracyanobenzoquinone dimethane nanorod catalyst.

[0119] Based on the above scheme, 0.05 mol·L -1 of sodium nitrate and 0.5 mol·L -1The sodium sulfate mixed solution was used as the electrolyte, the copper-tetracyano-p-benzoquinone dimethane catalyst was used as the working electrode, the carbon rod was used as the counter electrode, and the Ag / AgCl electrode was used as the reference electrode to form a three-electrode test system. The voltage required for the reaction was provided by the electrochemical workstation. The voltage parameter was set on the computer control system, and the voltage parameter was set to -1.1V. The constant potential test was performed for 1 hour. After the test, the electrolyte was collected to detect the remaining amount of nitrate reactants and the content of ammonia products. Then, the conversion rate of nitrate ions was calculated to be 84.23%, and the ammonia yield was 263.7mmol·mg cat. -1 ·h -1 , the ammonia Faraday efficiency is 82.07%.

[0120] Example 9

[0121] A method for preparing a copper-tetracyano-p-benzoquinodimethane catalyst, exemplarily comprising the following steps:

[0122] (1) acetonitrile, ethanol and water are mixed in a certain proportion as a solvent, wherein the volumes of acetonitrile, ethanol and water are 8 mL, 0.5 mL and 1.5 mL respectively, and the order is that ethanol is first added to the acetonitrile solvent, and then water is added to the above mixed solvent;

[0123] (2) Dissolve 2 mg of tetracyano-p-benzoquinodimethane in the above solvent to prepare a reaction solution. The concentration of tetracyano-p-benzoquinodimethane is 0.2 g·L -1 ;

[0124] (3) soaking the porous copper foam in acetone, dilute hydrochloric acid and ethanol solutions in turn to remove impurities on the surface, rinsing with water, and then placing it in the above reaction solution to react at room temperature and pressure for 2 hours. After the reaction is completed;

[0125] (4) The obtained product was washed with ethanol and water three times in sequence, and dried in a vacuum oven at a temperature of 70 degrees Celsius for 12 hours to obtain a copper-tetracyanobenzoquinone dimethane nanorod catalyst.

[0126] Based on the above scheme, 0.01 mol·L -1 of sodium nitrate and 0.1 mol·L -1The sodium sulfate mixed solution was used as the electrolyte, copper-tetracyano-p-benzoquinone dimethane catalyst was used as the working electrode, carbon rod was used as the counter electrode, and Ag / AgCl electrode was used as the reference electrode to form a three-electrode test system. The voltage required for the reaction was provided by the electrochemical workstation. The voltage parameter was set on the computer control system, and the voltage parameter was set to -0.8V. The constant potential test was performed for 1 hour. After the test, the electrolyte was collected to detect the remaining amount of nitrate reactants and the content of ammonia products. Then, the conversion rate of nitrate ions was calculated to be 67.24%, and the ammonia yield was 184.9mmol·mg cat. -1 ·h -1 , the ammonia Faraday efficiency is 87.46%.

[0127] Comparative Example 1

[0128] A method for preparing a copper-tetracyano-p-benzoquinodimethane catalyst comprises the following steps:

[0129] (1) Using acetonitrile as the solvent, the volume of acetonitrile is 10 mL;

[0130] (2) Dissolve 5 mg of tetracyano-p-benzoquinodimethane in the above solvent to prepare a reaction solution. The concentration of tetracyano-p-benzoquinodimethane is 0.5 g·L -1 ;

[0131] (3) soaking the porous copper foam in acetone, dilute hydrochloric acid and ethanol solutions in turn to remove surface impurities, then rinsing with water, and then placing it in the above reaction solution to react at room temperature and pressure for 1 hour. After the reaction is completed;

[0132] (4) The obtained product was washed with ethanol and water three times in sequence, and dried in a vacuum oven at a temperature of 60 degrees Celsius for 24 hours to obtain a copper-tetracyanobenzoquinone dimethane nanorod catalyst.

[0133] Based on the above scheme, 0.01 mol·L -1 of sodium nitrate and 0.1 mol·L -1 The sodium sulfate mixed solution was used as the electrolyte, the copper-tetracyano-p-benzoquinone dimethane catalyst was used as the working electrode, the carbon rod was used as the counter electrode, and the Ag / AgCl electrode was used as the reference electrode to form a three-electrode test system. The voltage required for the reaction was provided by the electrochemical workstation. The voltage parameter was set on the computer control system, and the voltage parameter was set to -1.2V. The constant potential test was performed for 1 hour. After the test, the electrolyte was collected to detect the remaining amount of nitrate reactants and the content of ammonia products. Then, the conversion rate of nitrate ions was calculated to be 38.08%, and the ammonia yield was 97.47mmol·mg cat. -1 ·h -1, the ammonia Faraday efficiency is 36.52%.

[0134] Figures 2 to 11 The scanning electron microscope images of the copper-tetracyano-p-benzoquinone dimethane catalysts provided in Examples 1 to 10 and Comparative Example 1 of the present application are shown respectively; it can be seen from the figure that the copper-tetracyano-p-benzoquinone dimethane catalysts of Examples 1 to 10 are in the shape of nanorods, with a nanorod diameter of 50nm to 500nm, wherein the nanorods of Example 5 are evenly distributed, with a nanorod diameter of 100nm to 200nm. The diameter of the nanorods of Comparative Example 1 is about 1μm to 2μm. Therefore, the copper-tetracyano-p-benzoquinone dimethane nanorod catalyst prepared by the present application by forming a mixed solution of acetonitrile, ethanol and water in a certain proportion has an increased length and a reduced particle size, which can significantly expose more active sites.

[0135] In addition, one or more technical solutions in the embodiments of the present invention have at least the following technical effects or advantages:

[0136] In the embodiment of the present invention, the copper-tetracyanoquinodimethane nanorod catalyst is applied to the electrocatalytic nitrate reduction to produce ammonia for the first time, and obtains good catalytic performance. The conversion rate of nitrate can reach up to 99.87%, and the ammonia production rate can reach up to 309.6mmol·mg cat. -1 ·h -1 , the ammonia Faraday efficiency can reach up to 98.57%.

[0137] In an embodiment of the present invention, in the process of preparing a copper-tetracyanoquinodimethane nanorod catalyst, a mixed solution is formed by acetonitrile, ethanol and water in a certain proportion, and the length of the prepared copper-tetracyanoquinodimethane nanorod catalyst is increased and the particle size is reduced, which can significantly expose more active sites and effectively promote the catalytic effect of the catalyst.

[0138] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.

Claims

1. A method for preparing a copper-tetracyano-p-benzoquinodimethane catalyst, characterized in that: The method comprises: Mixing acetonitrile, ethanol and water according to a set volume ratio to obtain a mixed solvent; dissolving tetracyano-p-benzoquinodimethane in the mixed solution to obtain a reaction solution; and The porous copper foam is added into the reaction solution to react and obtain copper-tetracyano-p-benzoquinodimethane grown on at least a portion of the surface of the porous copper foam.

2. The method according to claim 1, characterized in that In the mixed solvent, the volume proportion of the acetonitrile is ≥70% and <100%, and the sum of the volume proportions of the ethanol and the water is >0 and ≤30%.

3. The method according to claim 1, characterized in that In the reaction solution, the concentration of tetracyanobenzoquinodimethane is 0.25 g·L -1 ~1.0g·L -1 .

4. The method according to claim 1, characterized in that: The reaction temperature is room temperature, the reaction pressure is normal pressure, and the reaction time is 0.5h to 2h.

5. The method according to claim 1, characterized in that Before adding the porous copper foam to the reaction solution, the method comprises: The porous copper foam is sequentially immersed in acetone, dilute hydrochloric acid and ethanol solution to remove surface impurities of the porous copper foam.

6. A copper-tetracyano-p-benzoquinodimethane catalyst prepared by the method according to any one of claims 1 to 5, characterized in that: The copper-tetracyano-p-benzoquinodimethane catalyst is in the shape of a nanorod, and the diameter of the nanorod of the copper-tetracyano-p-benzoquinodimethane catalyst is 50nm-500nm.

7. Use of the copper-tetracyano-p-benzoquinodimethane catalyst as claimed in claim 6 in nitrate reduction to produce ammonia, characterized in that: The applications include: The copper-tetracyano-p-benzoquinodimethane catalyst is used as a working electrode to electrocatalytically reduce nitrate to obtain an ammonia product.

8. The use according to claim 7, characterized in that: The electrolyte used in the electrocatalytic reduction is a mixed solution of sodium nitrate and sodium sulfate, and the concentration of the sodium nitrate is 0.01 mol·L -1 ~0.5mol·L -1 The concentration of sodium sulfate is 0.1 mol·L -1 ~0.5mol·L -1 .

9. The use according to claim 7, characterized in that: The electrocatalytic reduction includes the following parameters: voltage is -0.6V to -1.3V, and time is 1h to 2h.

10. The use according to claim 7, characterized in that: The electrocatalytic reduction of nitrates satisfies at least one of the following properties: nitrate conversion rate ≥ 55%, ammonia yield ≥ 100 mmol·mg cat. -1 ·h -1 , ammonia Faraday efficiency ≥ 65%.