Process method for preparing superconducting quantum bits
Through ion beam cleaning and heating annealing treatment, a multi-layer metal oxide layer structure is formed, which solves the quantum noise problem caused by amorphous oxide layers, improves the life and performance of superconducting qubits, simplifies the process flow and reduces the noise source .
Patent Information
- Application Number
- CN202411058520.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-11-15
AI Technical Summary
In the existing superconducting qubit preparation process, the amorphous oxide layer causes quantum noise and mechanical damage, affecting the chip life and performance.
The substrate is treated with ion beam cleaning and heating annealing to form a multi-layer metal oxide layer structure. Through pattern processing and slow oxidation treatment, the substrate surface morphology and oxygen atom distribution are improved, and the amorphous oxide layer is reduced.
Effectively reduce quantum noise, improve the lifetime and performance of qubits, simplify the process flow, avoid additional lithography and deposition steps, and reduce noise sources.
Smart Images

Figure CN118973370A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of quantum bit preparation technology, and in particular to a process method for preparing superconducting quantum bits. Background Art
[0002] The Manhattan junction, or cross junction and its supporting micromachining are currently one of the mainstream technical routes for the preparation of superconducting quantum bits. This process can provide high-quality quantum bit chips with good scalability.
[0003] The underlying circuit and Josephson junction of the quantum bit chip can be made of micro-processed aluminum metal. The deposition of all aluminum materials faces the problem of amorphous oxide layer: the presence of amorphous oxide layer will cause quantum noise and reduce the life of the quantum bit; At present, in the preparation process of the underlying circuit and Josephson junction of superconducting quantum bits, ion cleaning is performed after the substrate is loaded to remove the amorphous layer on the surface. This amorphous layer is one of the most important reasons for the noise and loss of the final chip. However, the use of ion cleaning will cause certain mechanical damage and microscopic unevenness, which is not conducive to the deposition of subsequent materials. In addition, the use of inappropriate ion cleaning will destroy the crystal bonding of the original substrate material to a certain extent, resulting in the destruction of the substrate lattice, which will cause certain noise problems in the final quantum chip. Summary of the invention
[0004] The purpose of the present invention is to solve the shortcomings of the prior art and to propose a process for preparing superconducting quantum bits.
[0005] In order to achieve the above object, the present invention adopts the following technical solution: a process for preparing a superconducting quantum bit, comprising the steps of: S1: Perform ion beam cleaning on the end surface of the substrate, and after the cleaning is completed, perform heating annealing on the end surface; S2: forming a first metal layer on several regions of the end surface of the substrate by deposition on the annealed substrate; S3: placing the first metal layer in an oxygen environment to form a first oxide layer on the outer side of the first metal layer, and performing a patterning process; S4: performing ion beam cleaning again on the substrate between adjacent first oxide layers to prepare a second metal layer and an outer second oxide layer, and performing heating annealing treatment on the second oxide layer; S5: depositing a third metal layer on the outer side of the second oxide layer so that the third metal layer at least partially overlaps with the second metal layer in a vertical direction, and performing oxidation again to form a third oxide layer on the outer side of the third metal layer.
[0006] As a further description of the above technical solution: in the step S1, it includes: S11: In a vacuum oxygen-free state, the substrate is heated from a first temperature to a second temperature, and a first time interval is set for heat preservation; S12: After the first time interval is reached, the substrate is annealed and cooled to the first temperature.
[0007] As a further description of the above technical solution: in the step S2, it includes: S21: depositing a first metal layer on the substrate, with a deposition thickness of 110-220 nm; S22: Etching several regions of the first metal layer to form a circuit loop of the quantum bit.
[0008] As a further description of the above technical solution: in the step S4, it includes: S41: performing deposition on the substrate to form a second metal layer, and performing oxidation treatment on the outer side of the second metal layer to form a second oxide layer; S42: the second oxide layer is heated from the first temperature to a third temperature, and a second time interval is set for heat preservation. After reaching the second time interval, the second oxide layer is annealed and cooled to the first temperature.
[0009] As a further description of the above technical solution: the material of the first metal layer is selected from a mixture of one or more of aluminum, tantalum, niobium, and titanium nitride.
[0010] As a further description of the above technical solution: the material of the second metal layer and the third metal layer is aluminum, the deposition thickness of the second metal layer is 35-55nm, and the deposition thickness of the third metal layer is 80-100nm.
[0011] As a further description of the above technical solution: the substrate is heated and annealed at a first oxygen partial pressure, and the second oxide layer is heated and annealed at a second oxygen partial pressure, the first oxygen partial pressure is 0-1Pa, and the second oxygen partial pressure is greater than the first oxygen partial pressure.
[0012] As a further description of the above technical solution: when oxidation is carried out, the oxidation time is 5-20 minutes.
[0013] As a further description of the above technical solution: the first temperature is 25°C, the second temperature is 900-1100°C, the third temperature is lower than the secondary flow temperature of the photoresist during etching, the first time interval is 30-60min, and the second time interval is greater than 45min.
[0014] As a further description of the above technical solution: when annealing is performed, the annealing speed is less than 10°C / min.
[0015] The above technical solution has the following advantages or beneficial effects: 1. Annealing after ion beam cleaning can improve the surface morphology of the substrate at the atomic level and repair local damage and atomic bonding problems caused by ion beam cleaning, thereby improving the performance of subsequent deposited metals and corresponding devices.
[0016] 2. Annealing the second oxide layer changes the distribution of oxygen atoms in the amorphous oxide layer, changes the dipole moment distribution state of the internal electric dipole, and then changes the interaction frequency band and distribution of the electric dipole and the electric field. This reduces the interaction between the dipole and the electric field, suppresses the intensity of the interaction of the Josephson junction or improves the spectrum, and ultimately increases the life of the quantum bit.
[0017] 3. Through slow heating and slow annealing, the distribution of oxygen atoms inside the material is made more uniform, reducing the amorphous oxide layer, avoiding excessive noise generated by the quantum bit, and reducing the life of the quantum bit. At the same time, there is no need to add additional lithography, development, deposition, and degumming process steps. The process flow is simple and does not introduce additional noise sources. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 The process of the process proposed by the present invention Figure 1 ; Figure 2 The process of the process proposed by the present invention Figure 2 ; Figure 3 The process of the process proposed by the present invention Figure 3 ; Figure 4 The process of the process proposed by the present invention Figure 4 ; Figure 5 It is a schematic diagram of the structure of ion beam cleaning of the substrate in the present invention; Figure 6 It is a schematic diagram of the structure of depositing the first metal layer of the present invention; Figure 7 A top view of depositing a first metal layer according to the present invention; Figure 8 A schematic diagram of the structure of forming a first oxide layer according to the present invention; Fig. 9 A top view of forming a first oxide layer according to the present invention; Fig.10 It is a schematic diagram of the structure of cleaning the Josephson junction area at the substrate according to the present invention; Fig.11A top view of depositing a second metal layer according to the present invention; Fig.12 It is a schematic diagram of the structure of depositing the second metal layer of the present invention; Fig.13 A top view of forming a second oxide layer according to the present invention; Fig.14 A schematic diagram of the structure of forming a second oxide layer according to the present invention; Fig.15 A top view of depositing a third metal layer according to the present invention; Fig.16 It is a schematic diagram of the structure of depositing the third metal layer of the present invention; Fig.17 A top view showing the formation of a third oxide layer according to the present invention; Fig.18 is a distribution curve diagram of oxygen atoms under heating annealing treatment in the present invention; Legend: 1. Substrate; 2. First metal layer; 3. First oxide layer; 4. Second metal layer; 5. Second oxide layer; 6. Third metal layer; 7. Third oxide layer. DETAILED DESCRIPTION
[0019] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0020] Reference Figure 1 , Figure 5-Figure 17 , an embodiment provided by the present invention: a process for preparing a superconducting quantum bit, comprising the steps of: S1: Perform ion beam cleaning on the end surface of the substrate, and after the cleaning is completed, perform heating annealing on the end surface; S2: forming a first metal layer on several regions of the end surface of the substrate by deposition on the annealed substrate; S3: placing the first metal layer in an oxygen environment to form a first oxide layer on the outer side of the first metal layer, and performing a patterning process; S4: performing ion beam cleaning again on the substrate between adjacent first oxide layers, preparing a second metal layer and an outer second oxide layer, and performing heating annealing treatment on the second oxide layer; S5: depositing a third metal layer on the outer side of the second oxide layer so that the third metal layer at least partially overlaps with the second metal layer in a vertical direction, and performing oxidation again to form a third oxide layer on the outer side of the third metal layer.
[0021] In this embodiment, by performing ion beam cleaning on the substrate, removing impurities and oxide layers on the surface of the substrate, and performing annealing on the end face of the substrate, the surface morphology of the substrate can be improved at the atomic level, and local damage and atomic bonding problems caused by ion cleaning can be repaired, thereby improving the performance of subsequent deposited metals and corresponding devices. A first metal layer is deposited on the substrate to prepare the underlying circuit of the quantum bit, and a first oxide layer is formed on the outside of the first metal layer, and a graphic process is performed. The graphic process is a photolithography or etching process to form the underlying circuit of the quantum bit. In the process of preparing the Josephson junction, the substrate on the area between the underlying circuits is ion beam cleaned, and a second metal layer is deposited to form the second metal layer, and the second metal layer is oxidized on the outside to form the second oxide layer, and the second oxide layer is heated and annealed to change the distribution relationship of oxygen atoms inside the oxide layer inside the amorphous oxide layer, change the dipole moment distribution state of the internal electric dipole, and then change the interaction frequency band and distribution of the electric dipole and the electric field (refer to Fig.18 ), the solid line part is the distribution relationship of oxygen atom content from the oxidized surface to the inside of the material without post-annealing treatment; the dotted line part is annealed under high temperature and low oxygen partial pressure environment, so that some oxygen atoms overflow and the distribution of oxygen atoms in the oxide layer is more uniform; the final state is as shown in the thick solid line part. (The mathematical formula refers to Fick's diffusion law under non-steady-state conditions, which is a known algorithm and will not be described in detail). Deposition is performed again on the outside of the second oxide layer to form a third metal layer. At this time, the third metal layer is a semi-encapsulated structure, so that part of the surface of the second oxide layer is in contact with the outside world. At the same time, the second metal layer and the third metal layer have an overlapping area in the vertical direction. The second metal layer, the second oxide layer and the third metal layer form a hierarchical structure of a Josephson junction. Oxidation is performed again on the outside of the third metal layer to form a third oxide layer to protect the Josephson junction.
[0022] Reference Figure 2 and Figure 5 , in step S1, comprising: S11: In a vacuum oxygen-free state, the substrate is heated from a first temperature to a second temperature, and a first time interval is set for heat preservation; S12: After reaching the first time interval, annealing the substrate to cool it down to a first temperature.
[0023] In this embodiment, the substrate is ion beam cleaned, and the material of the substrate includes but is not limited to a sapphire substrate and a high-resistance silicon substrate. The surface of the substrate is bombarded by an argon ion beam. After ion beam cleaning, the substrate is annealed, and the first temperature is room temperature (25°C). In the heating stage, the temperature is raised from room temperature to a second temperature, and the second temperature is 900-1100°C, preferably 1000°C, and then maintained at the second temperature for a first time interval, and then slowly annealed, the first time interval is 30-60min, preferably 45min, and the annealing rate is less than 10°C / min. In this process, the oxygen partial pressure is maintained at the first oxygen partial pressure, the first oxygen partial pressure is 0-1Pa, and the vacuum oxygen-free environment is as close to 0 as possible, and there is no artificial introduction of oxygen to adjust the first oxygen partial pressure. The annealing process can repair the substrate surface bombarded by argon ions and repair the damaged bonding, thereby reducing the generation of amorphous.
[0024] Reference Figure 3 , Figure 6-Figure 7 , in step S2, including: S21: depositing a first metal layer on the substrate, with a deposition thickness of 110-220 nm; S22: Etching several areas of the first metal layer to form a circuit loop of the quantum bit.
[0025] In this embodiment, deposition is performed on the surface of the substrate to form a first metal layer in several areas on the surface. The material of the first metal layer is selected from a mixture of one or more of aluminum, tantalum, niobium, and titanium nitride. The deposition thickness is 110-220nm, and the preferred thickness of aluminum metal is 120nm, and the preferred thickness of tantalum metal is 200nm.
[0026] Reference Figure 8-Figure 9 According to the design requirements of the quantum circuit, the first metal layer is covered with a mask plate and then etched. After part of the first metal layer is removed, the underlying circuit of the quantum bit is formed.
[0027] Reference Figure 4 , Figure 10-Figure 14 , in step S4, including: S41: performing deposition on the substrate to form a second metal layer, and performing oxidation treatment on the outer side of the second metal layer to form a second oxide layer; S42: the second oxide layer is heated from the first temperature to a third temperature, and a second time interval is set for heat preservation. After reaching the second time interval, annealing is performed to cool the second oxide layer to the first temperature.
[0028] In this embodiment, the substrate between the two bottom circuits is ion beam cleaned again, and a second metal layer is deposited, and oxidation is performed on the outside to form a second oxide layer, and the second oxide layer is heated and annealed. After the temperature is raised from the first temperature to the third temperature under the second oxygen partial pressure, a second time interval is set for insulation, the second oxygen partial pressure is an oxygen-deficient state, and the second time interval is greater than 45 minutes. The third temperature is lower than the secondary flow temperature of the mask plate during the etching process, and needs to be determined according to the secondary flow temperature of the material of the mask plate used. The mask plate material is PMMA or MMA copolymer or a special type of photoresist, etc. In order to prevent the pattern of the mask plate from changing, the secondary flow temperature of the mask plate material is actually lowered by 20-30°C to the third temperature. Taking PMMA as an example, the flow temperature is about 160°C and the third temperature is 130°C.
[0029] Annealing the second oxide layer changes the distribution of oxygen atoms in the amorphous oxide layer. By changing the distribution of oxygen atoms in the second oxide layer, the dipole moment distribution state of the internal electric dipole is changed, and the interaction frequency band and distribution of the electric dipole and the electric field are changed in a targeted manner. This reduces the interaction between the dipole and the electric field, suppresses the intensity of the interaction of the Josephson junction or improves the spectrum, and ultimately increases the life of the quantum bit.
[0030] Reference Figure 15-17 , a third metal layer is continuously deposited on the outside of the second oxide layer after annealing, so that the second metal layer, the second oxide layer and the third metal layer form a Josephson junction, the material of the second metal layer and the third metal layer is aluminum, the deposition thickness of the second metal layer is 35-55nm, preferably 45nm, the deposition thickness of the third metal layer is 80-100nm, preferably 90nm, and during oxidation, the oxidation time in an oxygen environment is 5-20min, preferably 10min.
[0031] During the heating and annealing process, the heating methods include but are not limited to halogen lamps, electric heating wires, laser annealing, etc. During heating, the heating rate is less than 10°C / min. Through slow heating and slow annealing, the oxygen atoms inside the material are distributed more evenly, reducing the amorphous oxide layer, avoiding excessive noise generated by the quantum bit, and reducing the life of the quantum bit. At the same time, there is no need to add additional lithography, development, deposition, and degumming process steps, and no additional noise will be introduced. The process flow is simple and does not introduce additional noise sources.
[0032] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A process for preparing a superconducting quantum bit, characterized in that: Includes steps: S1: Perform ion beam cleaning on the end surface of the substrate, and after the cleaning is completed, perform heating annealing on the end surface; S2: forming a first metal layer on several regions of the end surface of the substrate by deposition on the annealed substrate; S3: placing the first metal layer in an oxygen environment to form a first oxide layer on the outer side of the first metal layer, and performing a patterning process; S4: performing ion beam cleaning again on the substrate between adjacent first oxide layers to prepare a second metal layer and an outer second oxide layer, and performing heating annealing treatment on the second oxide layer; S5: depositing a third metal layer on the outer side of the second oxide layer so that the third metal layer at least partially overlaps with the second metal layer in a vertical direction, and performing oxidation again to form a third oxide layer on the outer side of the third metal layer.
2. The process according to claim 1, characterized in that: In the step S1, it includes: S11: In a vacuum oxygen-free state, the substrate is heated from a first temperature to a second temperature, and a first time interval is set for heat preservation; S12: After the first time interval is reached, the substrate is annealed and cooled to the first temperature.
3. The process according to claim 1, characterized in that: In the step S2, it includes: S21: depositing a first metal layer on the substrate, with a deposition thickness of 110-220 nm; S22: Etching several regions of the first metal layer to form a circuit loop of the quantum bit.
4. The process according to claim 3, characterized in that: In the step S4, it includes: S41: performing deposition on the substrate to form a second metal layer, and performing oxidation treatment on the outer side of the second metal layer to form a second oxide layer; S42: the second oxide layer is heated from the first temperature to a third temperature, and a second time interval is set for heat preservation. After reaching the second time interval, the second oxide layer is annealed and cooled to the first temperature.
5. The process according to claim 1, characterized in that: The material of the first metal layer is selected from a mixture of one or more of aluminum, tantalum, niobium and titanium nitride.
6. The process according to claim 1, characterized in that: The materials of the second metal layer and the third metal layer are aluminum, the deposition thickness of the second metal layer is 35-55 nm, and the deposition thickness of the third metal layer is 80-100 nm.
7. The process according to claim 1, characterized in that: The substrate is heated and annealed at a first oxygen partial pressure, and the second oxide layer is heated and annealed at a second oxygen partial pressure, wherein the first oxygen partial pressure is 0-1 Pa, and the second oxygen partial pressure is greater than the first oxygen partial pressure.
8. The process according to claim 1, characterized in that: When oxidation is performed, the oxidation time is 5-20 minutes.
9. The process according to claim 4, characterized in that: The first temperature is 25° C., the second temperature is 900-1100° C., the third temperature is lower than the secondary flow temperature of the photoresist during the etching process, the first time interval is 30-60 minutes, and the second time interval is greater than 45 minutes.
10. The process according to claim 1, characterized in that: When annealing is performed, the annealing rate is less than 10°C / min.