Copper-zinc-tin-sulfur precursor film prepared by low-temperature heat treatment method and copper-zinc-tin-sulfur-selenium solar cell comprising copper-zinc-tin-sulfur precursor film
The surface morphology of Cu-Zn-Sn-S precursor film is improved through low-temperature heat treatment process, promotes the diffusion of Se element and grain growth, solves the problem of low quality and efficiency of the absorption layer in the high-temperature sulfur selenization step, and achieves high efficiency CZTSSe thin-film solar cells have improved performance.
Patent Information
- Application Number
- CN202411145499.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-08-20
AI Technical Summary
During the preparation process of copper, zinc, tin, sulfur and selenium solar cells, the surface morphology and element distribution of the precursor film of the high-temperature sulfur and selenization step affect the crystal quality of the absorbing layer, resulting in low device efficiency and holes, and the double-layer grain structure is not conducive to High-efficiency photoelectric conversion.
The Cu-Zn-Sn-S precursor film was treated at 50°C by low temperature heat treatment to change its surface morphology, promote the diffusion of Se elements and grain growth, and form a single-layer large-grain CZTSSe absorber layer film.
The crystal quality and device efficiency of the CZTSSe absorber layer film are improved, from 54% filling factor and 9.03% efficiency to 63.67% and 11.8%, and holes are reduced, achieving more efficient photoelectric conversion.
Smart Images

Figure CN119038888A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of new energy of optoelectronic materials, and specifically relates to a method for preparing a copper-zinc-tin-sulfur precursor film and a copper-zinc-tin-sulfur-selenium solar cell by a low-temperature heat treatment process. Background Art
[0002] CZTSSe thin film solar cells have the advantages of rich content of constituent elements, no toxic components, environmental friendliness and low price, and have a good development prospect. The absorption layer film with a single-layer grain structure is one of the important components of high-efficiency solar cells. Among the preparation methods of CZTSSe thin films, the chemical solution method leads the development of device efficiency, which includes three important steps: 1. Preparation of precursor solution; 2. Spin coating and baking to prepare precursor film; 3. High-temperature sulfur selenization to obtain CZTSSe absorption layer film. Researchers have conducted extensive research on steps 1 and 3. As a link between the previous and the next, step 2 deserves in-depth research and optimization.
[0003] In the process of preparing copper-zinc-tin-sulfur-selenide absorption layer film by high-temperature sulfur-selenization of precursor film, the morphology and element distribution of the precursor film have an important influence on the crystal quality and film structure of the copper-zinc-tin-sulfur-selenide absorption layer. Baking the precursor wet film can volatilize the organic solvent in the film on the one hand, and make the compounds in the solution undergo decomposition and resynthesis steps to form the precursor film on the other hand. Almost all films must wait for the film prepared in the previous cycle to cool before the next cycle of spin coating. Generally speaking, after heat treatment at 300℃, it takes 4 minutes for the film to cool to room temperature, and then the absorption layer film is prepared. There are usually many holes on the surface of the film, showing a double-layer grain structure and low device efficiency. Summary of the invention
[0004] In view of this, the present invention discloses a low-temperature heat treatment method for preparing a copper-zinc-tin-sulfur precursor film and a copper-zinc-tin-sulfur-selenium solar cell containing the same. The Cu-Zn-Sn-S precursor film is prepared by a low-temperature heat treatment process, which changes the surface morphology of the precursor film, resulting in the diffusion of Se elements in the subsequent high-temperature sulfur-selenization process, thereby preparing a CZTSSe absorption layer film with a smooth surface and fewer holes. The film is used as the absorption layer of the solar cell, and finally a CZTSSe thin film solar cell with a device efficiency of 11.8% is prepared.
[0005] It should be noted that the present invention explores the use of 50°C low-temperature heat treatment of the precursor film during the cooling process of the Cu-Zn-Sn-S precursor film to change the surface morphology of the precursor film, thereby improving the crystal quality of the CZTSSe absorption layer film. After low-temperature heat treatment, the crystallization of the Cu-Zn-Sn-S precursor film is significantly improved, the grain size is significantly increased, and the surface is loose and porous, which is conducive to the downward diffusion of Se elements during the sulfur-selenization process. The grain growth mode from top to bottom dominates the grain growth, and finally a single-layer large-grain CZTSSe absorption layer film is obtained.
[0006] To achieve the above object, the present invention adopts the following technical solution:
[0007] The first technical purpose of the present invention is to provide a method for preparing a copper-zinc-tin-sulfur precursor film by a low-temperature heat treatment process, the operating steps being:
[0008] (1) Preparation of copper-zinc-tin-sulfur (Cu-Zn-Sn—S) precursor solution:
[0009] Zinc acetate dihydrate (Zn(CH3COOH)2·2H2O), cuprous chloride (CuCl), thiourea (CH4N2S, Tu), tin tetrachloride pentahydrate (SnCl4·5H2O) were mixed, and then ethylene glycol methyl ether (MOE) and dimethyl sulfoxide (DMSO) were added, and the reaction was carried out in a water bath to obtain a Cu-Zn-Sn—S precursor solution;
[0010] (2) Preparation of Cu-Zn-Sn-S precursor film by spin coating-baking-low temperature heat treatment:
[0011] The Cu-Zn-Sn-S precursor solution is dropped on the four corners and the middle of the molybdenum glass, and spin coating is performed after the solution completely covers the surface; after the spin coating is completed, the wet film is baked and low-temperature heat treated, and the spin coating-baking-low-temperature heat treatment steps are repeated 10 times to obtain a Cu-Zn-Sn-S precursor film.
[0012] Preferably, the element design ratio of the precursor solution follows the principle of copper-poor and zinc-rich, and the molar ratio design ratios of the constituent elements Cu / (Zn+Sn) and Znn / Sn are 0.72 and 1.14; the water bath reaction temperature is 66°C, and the reaction time is 3 hours to obtain a fully dissolved precursor solution.
[0013] Preferably, the size of the molybdenum glass is 2×2 cm, including a 2 mm thick soda-lime glass and a 1 μm thick molybdenum layer; the parameters of the spin coating setting are: a rotation speed of 3600 r / min and a time of 36 s; baking parameters: a time of 2 min and a temperature of 300°C; low-temperature heat treatment parameters after baking: a time of 5 min and a temperature of 50°C. After the low-temperature treatment, the next cycle of spin coating is carried out directly without waiting for the film to cool to room temperature.
[0014] The second technical purpose of the present invention is to provide a copper-zinc-tin-sulfur-selenium absorption layer film, wherein the absorption layer film is prepared by high-temperature sulfur-selenization of a copper-zinc-tin-sulfur (Cu-Zn-Sn—S) precursor film prepared by the above method; the method is as follows:
[0015] The copper-zinc-tin-sulfur (Cu-Zn-Sn-S) precursor film, tin sulfide (SnS) and selenium pellets (Se) are subjected to high-temperature sulfur-selenization to obtain the copper-zinc-tin-sulfur-selenium absorption layer film (CZTSSe film).
[0016] Optionally, there is a specific quantitative relationship between the mass ratio of the copper-zinc-tin-sulfur (Cu-Zn-Sn-S) precursor film and stannous sulfide (SnS) and selenium pills (Se), and the ratio is 4 pieces: 10 mg: 350 mg.
[0017] Optionally, the sulfur-selenization operation is: heating from room temperature to 280° C. and maintaining for 10 minutes for soft sulfur-selenization, with a heating rate of 28.3° C. / min; continuing to heat to 510° C. to start high-temperature sulfur-selenization and timing, with a heating rate of 25.5° C. / min during this process;
[0018] Among them, high-temperature sulfur-selenization was repeated twice between 510℃-570℃, and the heating and cooling rates were both 17.1℃ / min. The specific operations were: heating from 510℃ to 570℃ for 3.5min, cooling from 570℃ to 510℃ for 3.5min, heating from 510℃ to 570℃ for 3.5min, cooling from 570℃ to 510℃ for 3.5min, and then heating from 510℃ to 570℃ for 3.5min, and then cooling from 570℃ to 510℃ for 3.5min. The heating and cooling rates were both 17.1℃ / min, thus completing the entire sulfur-selenization process.
[0019] The third technical purpose of the present invention is to provide a copper-zinc-tin-sulfur-selenium solar cell, wherein the solar cell comprises the copper-zinc-tin-sulfur-selenium absorption layer film as described above.
[0020] Preferably, the preparation operation of the copper-zinc-tin-sulfur-selenium solar cell is as follows:
[0021] A 50 nm thick CdS buffer layer is first deposited on the copper zinc tin sulfur selenium absorption layer thin film (CZTSSe thin film) to form a pn junction with CZTSSe and reduce the lattice mismatch and band gap mismatch between the absorption layer and the window layer, and then a 50 nm thick intrinsic zinc oxide (i-ZnO) and a 230 nm thick tin-doped indium oxide (ITO) window layer are magnetron sputtered as the upper surface structure of the solar cell, and finally a 100 nm thick Ag electrode is thermally evaporated to collect photogenerated current. In summary, the preparation of the copper zinc tin sulfur selenium solar cell (CZTSSe thin film solar cell) is completed.
[0022] Furthermore, the CdS film was deposited by a chemical water bath method, the water bath temperature was 70°C, the rotation speed was 600 r / min; the background vacuum of magnetron sputtering was 5×10 -4 Pa, the working gas pressure for sputtering i-ZnO is 0.5Pa, and the sputtering power is 35W-20min, 60W-5min; the working gas pressure for sputtering ITO is 0.3Pa, and the sputtering power is 80W-90min.
[0023] Preferably, the copper-zinc-tin-sulfur-selenium solar cell has a structure of SLG / Mo / CZTSSe / CdS / i-ZnO / ITO / Ag.
[0024] The technology of the present invention can be used to prepare a complete copper-zinc-tin-sulfur-selenium thin film solar cell with an efficiency of 11.8%, an open circuit voltage of 523.49 mV, and a short circuit current density of 35.53 mA / cm 2 , the filling factor is 63.67%.
[0025] Through the above technical solution, compared with the prior art, it can be seen that the present invention uses a low-temperature heat treatment method to prepare a copper-zinc-tin-sulfur precursor film and a copper-zinc-tin-sulfur-selenium solar cell containing the same. It has the following technical effects:
[0026] Compared with the Cu-Zn-Sn-S precursor film that has not undergone low-temperature heat treatment, the surface of the precursor film is looser, the grain aggregation is significantly expanded, the gap between the grains is more obvious, and the loose porous surface structure is more obvious, which is conducive to the downward diffusion of Se elements. The porous structure of the Cu-Zn-Sn-S precursor film accelerates the growth of grains, and finally obtains a single-layer large-grain CZTSSe absorption layer. Using this film as a solar cell absorption layer film, the filling factor and efficiency of the prepared CZTSSe thin film solar cell are increased from 54% and 9.03% to 63.67% and 11.8% respectively.
[0027] That is, the present invention prepares a Cu-Zn-Sn-S precursor film by low-temperature heat treatment, optimizes the surface morphology of the precursor film, obtains a CZTSSe absorption layer with a single-layer grain structure and a CZTSSe thin-film solar cell with an efficiency of 11.8%. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0029] Figure 1Surface SEM image of the Cu-Zn-Sn-S precursor film prepared in Example 1;
[0030] Figure 2 Surface SEM image of the Cu-Zn-Sn-S precursor film prepared in Comparative Example 1;
[0031] Figure 3 Surface SEM image of the Cu-Zn-Sn-S precursor film prepared in Comparative Example 2;
[0032] Figure 4 Surface SEM image of the Cu-Zn-Sn-S precursor film prepared in Comparative Example 3;
[0033] Figure 5 This is a surface SEM image of the copper-zinc-tin-sulfur-selenium absorption layer film prepared in Example 1;
[0034] Figure 6 This is a surface SEM image of the copper-zinc-tin-sulfur-selenium absorption layer film prepared in Comparative Example 1;
[0035] Figure 7 This is a surface SEM image of the copper-zinc-tin-sulfur-selenium absorption layer film prepared in Comparative Example 2;
[0036] Figure 8 This is a surface SEM image of the copper-zinc-tin-sulfur-selenium absorption layer film prepared in Comparative Example 3;
[0037] Fig. 9 This is a cross-sectional SEM image of the copper-zinc-tin-sulfur-selenium absorption layer film prepared in Example 1;
[0038] Fig.10 This is a cross-sectional SEM image of the copper-zinc-tin-sulfur-selenium absorption layer film prepared in Comparative Example 1;
[0039] Fig.11 This is a cross-sectional SEM image of the copper-zinc-tin-sulfur-selenium absorption layer film prepared in Comparative Example 2;
[0040] Fig.12 This is a cross-sectional SEM image of the copper-zinc-tin-sulfur-selenium absorption layer film prepared in Comparative Example 3;
[0041] Fig.13 The JV curve of the copper-zinc-tin-sulfur-selenium thin film solar cell prepared in Example 2;
[0042] Fig.14 The JV curve of the copper-zinc-tin-sulfur-selenium thin film solar cell prepared in Comparative Example 4;
[0043] Fig.15 EQE curve of the copper-zinc-tin-sulfur-selenium thin film solar cell prepared in Example 2;
[0044] Fig.16 This is the EQE curve of the copper-zinc-tin-sulfur-selenium thin film solar cell prepared in Comparative Example 4. DETAILED DESCRIPTION
[0045] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0046] The word "embodiment" used here as an "exemplary" does not necessarily mean that any embodiment described is superior to or better than other embodiments. Unless otherwise specified, the performance index tests in the embodiments of this application are performed using conventional test methods in the art. It should be understood that the terms described in this application are only used to describe specific implementation methods and are not used to limit the content disclosed in this application.
[0047] Unless otherwise specified, the technical and scientific terms used in this document have the same meanings as commonly understood by ordinary technicians in the technical field to which this application belongs; other experimental methods and technical means not specifically specified in this application refer to experimental methods and technical means commonly used by ordinary technicians in this field.
[0048] In order to better illustrate the content of the present application, numerous specific details are provided in the specific examples below. It should be understood by those skilled in the art that the present application can also be implemented without certain specific details. In the embodiments, some methods, means, instruments, equipment, etc. well known to those skilled in the art are not described in detail in order to highlight the main purpose of the present application.
[0049] Under the premise of no conflict, the technical features disclosed in the embodiments of the present application can be combined arbitrarily, and the resulting technical solutions belong to the contents disclosed in the embodiments of the present application.
[0050] The present invention discloses a method for preparing a Cu-Zn-Sn-S precursor film by a low temperature heat treatment process, and the specific preparation steps are:
[0051] (1) Preparation of Cu-Zn-Sn-S precursor solution:
[0052] 0.8166g zinc acetate dihydrate (Zn(CH3COOH)2·2H2O), 0.0.4989g cuprous chloride (CuCl), 1.6991g thiourea (CH4N2S), and 1.1412g tin tetrachloride pentahydrate (SnCl4·5H2O) were weighed in sequence and added into a clean transparent glass bottle (volume 10mL), and then 3mL ethylene glycol methyl ether (MOE) and 3mL dimethyl sulfoxide (DMSO) were added thereto and sealed with a bottle cap. Finally, the solution was placed in a constant temperature water bath (temperature: 66°C, rotation speed: 666r / min) and stirred for 3 hours to obtain a Cu-Zn-Sn—S precursor solution.
[0053] (2) Spin coating-baking-low temperature heat treatment to prepare precursor film:
[0054] First, use a disposable syringe (capacity: 2.5mL) to absorb the filtered solution for later use, then place the cleaned molybdenum glass on the suction cup of the spin coater and fix it, and drop the solution on the four corners and the middle of the molybdenum glass. After the solution completely covers the surface, spin coating is performed; after the spin coating is completed, the wet film is placed on a 300°C heating table and baked for 2 minutes, and then the sample is moved to a 50°C heating table for low-temperature heat treatment for 5 minutes; repeat the spin coating-baking-low-temperature heat treatment steps 10 times to obtain a Cu-Zn-Sn—S precursor film.
[0055] (3) Preparation of CZTSSe absorption layer film by high temperature sulfur selenization:
[0056] Place 10 mg of tin sulfide (SnS), 350 mg of selenium pills (Se) and the Cu-Zn-Sn-S precursor film obtained in step (2) in a graphite box in sequence, then place the graphite box in the middle position of the quartz tube of a single-temperature zone tubular furnace, clean the quartz tube three times with high-purity argon (Ar) and seal the quartz tube. After high-temperature sulfur-selenization, wait for the sample to cool to room temperature and then take it out.
[0057] (4) A 50 nm thick CdS buffer layer is deposited on the CZTSSe thin film obtained in step (3), followed by sputtering a 50 nm thick intrinsic zinc oxide (i-ZnO) and a 230 nm thick tin-doped indium oxide (ITO) window layer, and finally a 100 nm thick Ag electrode is deposited by thermal evaporation to complete the preparation of the CZTSSe thin film solar cell.
[0058] Preferably, the Zn(CH3COOH)2·2H2O in step (1) is purchased with a purity of 99.99%; the purity of CuCl is 99.9%; the purity of SnCl4·5H2O is purchased with a purity of 99.995%; the purity of DMSO is purchased with a purity of 99.9%; the purity of MOE is 99.8%, and all of the above drugs are purchased from Shanghai Aladdin Biochemical Technology Co., Ltd. CH4N2S is purchased from Beijing Inokai Technology Co., Ltd. with a purity of 99%. The element design ratio of the precursor solution follows the principle of poor copper and rich zinc, and the design ratio of the molar ratio of Cu / (Zn+Sn) and Zn / Sn is 0.72 and 1.14. All experimental operations for the preparation of the Cu-Zn-Sn-S precursor solution are completed in an air environment.
[0059] Preferably, the size of the molybdenum glass in step (2) is 2×2 cm, including a 2 mm thick soda-lime glass and a 1 μm thick molybdenum layer; the parameters set for the spin coater are 3600 r / min and the time is 36; the thickness of the Cu-Zn-Sn-S precursor film obtained by spin coating-baking-low-temperature heat treatment 10 times is 1.2 μm, and the precursor film is prepared in an air environment.
[0060] Preferably, the specific operation of the high-temperature sulfur-selenide in step (3) is: first, the temperature is raised from room temperature to 280°C for 9 minutes and maintained for 10 minutes for soft sulfur-selenide, and the heating rate of this process is 28.3°C / min; then the temperature is raised for 9 minutes to 510°C to start high-temperature sulfur-selenide and timing, and the heating rate of this process is 25.5°C / min; the temperature is raised from 510°C to 570°C for 3.5 minutes, and the temperature is lowered from 570°C to 510°C for 3.5 minutes, and the temperature is raised from 510°C to 570°C for 3.5 minutes, and the temperature is lowered from 570°C to 510°C for 3.5 minutes, and the temperature is raised from 510°C to 570°C for 3.5 minutes, and the temperature is lowered from 570°C to 510°C for 3.5 minutes, and the heating and cooling rates are both 17.1°C / min, thereby completing the entire sulfur-selenide process.
[0061] Preferably, the specific steps of the method for preparing the copper-zinc-tin-sulfur-selenium thin film solar cell are:
[0062] 1) The copper-zinc-tin-sulfur-selenium absorption layer thin film is deposited by chemical water bath deposition to prepare a 50 nm thick n-type CdS buffer layer. The specific operation is as follows:
[0063] Use processed tweezers to pick up the absorption layer film and soak it in ultrapure water for 15 minutes to remove the oxide on the surface of the CZTSSe film; measure 22mL of ultrapure water and put it into the small beakers with numbers, weigh 1.256gTu and 0847gCdSO4·8 / 3H20 in turn and add them to the above beakers and put them through ultrasound to promote dissolution; set the temperature of the constant temperature water bath to 70℃ and the speed to 600r / min, and move the soaked sample to a sedimentation beaker with 150mL ultrapure water and a rotor. First pour in the cadmium sulfate aqueous solution, then pour in the ammonia water after 40s, then pour in the thiourea aqueous solution after 1 minute and 40s, take out the sample after 8 minutes and 30s and rinse it with ultrapure water 3 times, and finally dry it on a heating plate.
[0064] 2) On the basis of the buffer layer, a 50nm thick i-ZnO film and a 230nm thick ITO film are sputtered by magnetron sputtering and radio frequency sputtering as a window layer. The specific operation is as follows:
[0065] The sample deposited with the buffer layer was placed in the window layer chamber of the magnetron sputtering, and the pressure was pumped from atmospheric pressure to 10 Pa using a mechanical pump, and then pumped to 5×10 -4 When sputtering i-ZnO, the working gas pressure is 0.5Pa, the high-purity argon flow rate is 13sccm, and the sputtering power is 35W-20min, 60W-5min; when sputtering ITO, the working gas pressure is 0.3Pa, the high-purity argon flow rate is 7sccm, and the sputtering power is 80W-90min.
[0066] 3) Finally, a Ag electrode is evaporated on the window layer to obtain a copper-zinc-tin-sulfur-selenium thin film solar cell.
[0067] Preferably, the copper-zinc-tin-sulfur-selenium thin-film solar cell has a complete structure of SLG / Mo / CZTSSe / CdS / i-ZnO / ITO / Ag.
[0068] In order to better understand the present invention, the present invention is further specifically described below through the following examples, but it should not be understood as a limitation of the present invention. Some non-essential improvements and adjustments made by technicians in this field based on the above invention content are also considered to fall within the protection scope of the present invention.
[0069] Example 1
[0070] (1) Preparation of Cu-Zn-Sn-S precursor solution: 0.8166 g zinc acetate dihydrate (Zn(CH3COOH)2·2H2O), 0.0.4989 g cuprous chloride (CuCl), 1.6991 g thiourea (CH4N2S, Tu), and 1.1412 g tin tetrachloride pentahydrate (SnCl4·5H2O) were weighed in sequence and added into a clean transparent glass bottle (volume: 10 mL), and then 3 mL ethylene glycol methyl ether (MOE) and 3 mL dimethyl sulfoxide (DMSO) were added thereto and the solution was tightly sealed with a bottle cap. Finally, the solution was placed in a constant temperature water bath (temperature: 66°C, rotation speed: 666 r / min) and stirred for 3 hours to obtain a Cu-Zn-Sn-S precursor solution.
[0071] (2) Preparation of Cu-Zn-Sn-S precursor film by spin coating-baking-low temperature heat treatment: First, use a disposable syringe (capacity: 2.5 mL) to absorb the filtered solution for use, then place the cleaned molybdenum glass on the spin coater suction cup and fix it, and drop the solution on the four corners and the middle of the molybdenum glass. After the solution completely covers the surface, spin coating is performed; after the spin coating is completed, the wet film is placed on a 300°C heating table for baking for 2 minutes, and then the sample is moved to a 50°C heating table for low temperature heat treatment for 5 minutes. Repeat the spin coating-baking-low temperature heat treatment steps 10 times to obtain a Cu-Zn-Sn-S precursor film.
[0072] (3) Preparation of copper-zinc-tin-sulfur-selenide absorption layer film by high-temperature sulfur-selenide treatment: 10 mg of stannous sulfide (SnS), 350 mg of selenium pellets (Se) and the precursor film obtained in step (2) were placed in a graphite box in sequence, and then the graphite box was placed in the middle position of the quartz tube of a single-temperature zone tubular furnace. The quartz tube was cleaned three times with high-purity argon (Ar) and sealed, and then high-temperature sulfur-selenide treatment was started. Finally, the sample was cooled to room temperature and then taken out.
[0073] from Figure 1 From the SEM image of the precursor Cu-Zn-Sn-S film surface, it can be seen that the grain size of the film surface obtained in Example 1 is significantly increased, the gaps between the grains are more prominent, and there are more holes on the surface, which is conducive to the diffusion of Se elements during the sulfur-selenization process. Figure 5 and Fig. 9 It can be seen that the CZTSSe absorption layer film prepared by the Cu-Zn-Sn-S precursor after low-temperature heat treatment at 50°C has fewer holes on the surface and the cross-section is an absorption layer film with a single-layer grain structure.
[0074] Example 2
[0075] The specific steps of preparing a copper-zinc-tin-sulfur-selenide thin film solar cell according to the copper-zinc-tin-sulfur-selenide absorption layer film described in Example 1 are as follows: a 50nm thick cadmium sulfide (CdS) buffer layer is prepared on the CZTSSe thin film obtained by temperature-dependent sulfur-selenization by chemical water bath deposition, followed by magnetron sputtering of a 50nm thick intrinsic zinc oxide (i-ZnO) and a 230nm thick tin-doped indium oxide (ITO) window layer, and finally a 100nm thick Ag electrode is evaporated by thermal evaporation (current of 60A, time of 15min) to complete the preparation of the CZTSSe solar cell.
[0076] The JV curve of the copper-zinc-tin-sulfur-selenium thin film solar cell prepared according to Example 2 is as follows: Fig.13 As shown, the efficiency is 11.8%, the open circuit voltage is 523.49mV, and the short circuit current density is 35.53mA / cm 2 , the filling factor is 63.67%. Fig.15 As shown, the maximum EQE is greater than 90%, and the EQE is greatly improved in the long-wave range, indicating that the crystal quality of the absorption layer thin film is good.
[0077] In order to further demonstrate the beneficial effects of the present invention and to better understand the present invention, the following comparative examples are used to further illustrate the technical features disclosed in the present invention, but they should not be construed as limiting the present invention. Other improvements made by those skilled in the art based on the above invention content without inventive work are also considered to fall within the scope of protection of the present invention.
[0078] Comparative Example 1
[0079] (1) Preparation of Cu-Zn-Sn-S precursor solution: 0.8166 g zinc acetate dihydrate (Zn(CH3COOH)2·2H2O), 0.0.4989 g cuprous chloride (CuCl), 1.6991 g thiourea (CH4N2S, Tu), and 1.1412 g tin tetrachloride pentahydrate (SnCl4·5H2O) were weighed in sequence and added into a clean transparent glass bottle (volume: 10 mL), and then 3 mL ethylene glycol methyl ether (MOE) and 3 mL dimethyl sulfoxide (DMSO) were added thereto and the solution was tightly sealed with a bottle cap. Finally, the solution was placed in a constant temperature water bath (temperature: 66°C, rotation speed: 666 r / min) and stirred for 3 hours to obtain a Cu-Zn-Sn-S precursor solution.
[0080] (2) Spin coating-baking treatment to prepare the precursor film: First, use a disposable syringe (capacity: 2.5 mL) to absorb the filtered solution for later use, then place the cleaned molybdenum glass on the spin coater suction cup and fix it, and then drop the solution on the four corners and the middle of the molybdenum glass until the solution completely covers the surface before spin coating; after the spin coating is completed, place the wet film on a 300°C heating table and bake it for 2 minutes, then wait for the sample to cool before the next cycle of spin coating. Repeat the spin coating-baking steps 10 times to obtain the precursor film.
[0081] (3) Preparation of absorption layer film by high-temperature sulfur-selenization: 10 mg of tin sulfide (SnS), 350 mg of selenium pellets (Se) and the precursor film obtained in step (2) were placed in a graphite box in sequence, and then the graphite box was placed in the middle position of the quartz tube of a single-temperature zone tubular furnace. The quartz tube was cleaned with high-purity argon (Ar) for 3 times and sealed, and then high-temperature sulfur-selenization was started. Finally, the sample was cooled to room temperature and taken out.
[0082] from Figure 2 It can be seen from the surface SEM image of the precursor film that the precursor film obtained in Comparative Example 1 has obvious agglomeration phenomenon, the grain outline is relatively fuzzy, and the grain gap is small, which is not conducive to the diffusion of Se element in the subsequent high-temperature sulfur-selenization process. Figure 6 and Fig.10 It can be seen that there are many holes on the surface of the copper-zinc-tin-sulfur-selenium absorption layer film prepared from the precursor that has not undergone low-temperature heat treatment, and the cross-section is a double-layer grain structure with obvious boundaries.
[0083] Comparative Example 2
[0084] (1) Preparation of Cu-Zn-Sn-S precursor solution: 0.8166 g zinc acetate dihydrate (Zn(CH3COOH)2·2H2O), 0.0.4989 g cuprous chloride (CuCl), 1.6991 g thiourea (CH4N2S, Tu), and 1.1412 g tin tetrachloride pentahydrate (SnCl4·5H2O) were weighed in sequence and added into a clean transparent glass bottle (volume: 10 mL), and then 3 mL ethylene glycol methyl ether (MOE) and 3 mL dimethyl sulfoxide (DMSO) were added thereto and the solution was tightly sealed with a bottle cap. Finally, the solution was placed in a constant temperature water bath (temperature: 66°C, rotation speed: 666 r / min) and stirred for 3 hours to obtain a Cu-Zn-Sn-S precursor solution.
[0085] (2) Preparation of Cu-Zn-Sn-S precursor film by spin coating-baking-low temperature heat treatment: First, use a disposable syringe (capacity: 2.5 mL) to absorb the filtered solution for use, then place the cleaned molybdenum glass on the spin coater suction cup and fix it, and drop the solution on the four corners and the middle of the molybdenum glass. After the solution completely covers the surface, spin coating is performed; after the spin coating is completed, the wet film is placed on a 300°C heating table for baking for 2 minutes, and then the sample is moved to a 40°C heating table for low temperature heat treatment for 5 minutes. Repeat the spin coating-baking-low temperature heat treatment steps 10 times to obtain a Cu-Zn-Sn-S precursor film.
[0086] (3) Preparation of copper-zinc-tin-sulfur-selenide absorption layer film by high-temperature sulfur-selenide treatment: 10 mg of stannous sulfide (SnS), 350 mg of selenium pellets (Se) and the precursor film obtained in step (2) were placed in a graphite box in sequence, and then the graphite box was placed in the middle position of the quartz tube of a single-temperature zone tubular furnace. The quartz tube was cleaned three times with high-purity argon (Ar) and sealed, and then high-temperature sulfur-selenide treatment was started. Finally, the sample was cooled to room temperature and then taken out.
[0087] from Figure 3 From the SEM image of the precursor Cu-Zn-Sn-S film surface, it can be seen that the grain size of the film surface obtained in Comparative Example 2 is increased, and the gaps between the grains are increased, which is conducive to the diffusion of Se elements during the sulfur-selenization process. Figure 7 and Fig.11 It can be seen that the surface holes of the CZTSSe absorption layer film prepared by the Cu-Zn-Sn-S precursor after low-temperature heat treatment at 40°C are reduced, and the cross-sectional morphology is improved to a certain extent, but it is still a double-layer grain structure.
[0088] Comparative Example 3
[0089] (1) Preparation of Cu-Zn-Sn-S precursor solution: 0.8166 g zinc acetate dihydrate (Zn(CH3COOH)2·2H2O), 0.0.4989 g cuprous chloride (CuCl), 1.6991 g thiourea (CH4N2S, Tu), and 1.1412 g tin tetrachloride pentahydrate (SnCl4·5H2O) were weighed in sequence and added into a clean transparent glass bottle (volume: 10 mL), and then 3 mL ethylene glycol methyl ether (MOE) and 3 mL dimethyl sulfoxide (DMSO) were added thereto and the solution was tightly sealed with a bottle cap. Finally, the solution was placed in a constant temperature water bath (temperature: 66°C, rotation speed: 666 r / min) and stirred for 3 hours to obtain a Cu-Zn-Sn-S precursor solution.
[0090] (2) Preparation of Cu-Zn-Sn-S precursor film by spin coating-baking-low temperature heat treatment: First, use a disposable syringe (capacity: 2.5 mL) to absorb the filtered solution for use, then place the cleaned molybdenum glass on the spin coater suction cup and fix it, and drop the solution on the four corners and the middle of the molybdenum glass. After the solution completely covers the surface, spin coating is performed; after the spin coating is completed, the wet film is placed on a 300°C heating table for baking for 2 minutes, and then the sample is moved to a 60°C heating table for low temperature heat treatment for 5 minutes. Repeat the spin coating-baking-low temperature heat treatment steps 10 times to obtain a Cu-Zn-Sn-S precursor film.
[0091] (3) Preparation of copper-zinc-tin-sulfur-selenide absorption layer film by high-temperature sulfur-selenide treatment: 10 mg of stannous sulfide (SnS), 350 mg of selenium pellets (Se) and the precursor film obtained in step (2) were placed in a graphite box in sequence, and then the graphite box was placed in the middle position of the quartz tube of a single-temperature zone tubular furnace. The quartz tube was cleaned three times with high-purity argon (Ar) and sealed, and then high-temperature sulfur-selenide treatment was started. Finally, the sample was cooled to room temperature and then taken out.
[0092] from Figure 4 From the SEM image of the precursor Cu-Zn-Sn-S film surface, it can be seen that the film surface obtained in Comparative Example 3 has more gaps and holes, which is conducive to the diffusion of Se element during the sulfur-selenization process. Figure 8 and Fig.12 It can be seen that the surface grains of the CZTSSe absorption layer film prepared by the Cu-Zn-Sn-S precursor after low-temperature heat treatment at 60°C are relatively large, but there are many small holes on the surface of the film probably due to the loss of elements, and the cross section is an absorption layer film with an obvious single-layer grain structure.
[0093] Comparative Example 4
[0094] The specific steps of preparing the copper-zinc-tin-sulfur-selenide thin film solar cell according to the copper-zinc-tin-sulfur-selenide absorption layer film described in Comparative Example 1 are as follows: a 50nm thick cadmium sulfide (CdS) buffer layer is prepared by chemical water bath deposition on the CZTSSe film obtained by constant temperature sulfur selenization, followed by magnetron sputtering of a 50nm thick intrinsic zinc oxide (i-ZnO) and a 230nm thick tin-doped indium oxide (ITO) window layer. Finally, a 100nm thick Ag electrode is deposited by thermal evaporation to complete the preparation of the CZTSSe solar cell.
[0095] The JV curve of the copper-zinc-tin-sulfur-selenium thin film solar cell prepared in Comparative Example 2 is as follows: Fig.14 As shown, the efficiency is 9.03%, the open circuit voltage is 504.99mV, and the short circuit current density is 33.13mA / cm 2 , the filling factor is 54.00%. EQE Fig.16As shown, compared with the device prepared by the low-temperature heat treatment method, the solar cell has a poor collection efficiency in the long-wave range, which may be related to the double-layer grains of the absorption layer film, which is also one of the main reasons for the low short-circuit current density.
[0096] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A method for preparing a copper-zinc-tin-sulfur precursor film by a low-temperature heat treatment process, characterized in that: The steps are: (1) Preparation of copper-zinc-tin-sulfur (Cu-Zn-Sn—S) precursor solution: Zinc acetate dihydrate (Zn(CH3COOH)2·2H2O), cuprous chloride (CuCl), thiourea (CH4N2S, Tu), tin tetrachloride pentahydrate (SnCl4·5H2O) were mixed, and then ethylene glycol methyl ether (MOE) and dimethyl sulfoxide (DMSO) were added, and the reaction was carried out in a water bath to obtain a Cu-Zn-Sn—S precursor solution; (2) Preparation of Cu-Zn-Sn-S precursor film by spin coating-baking-low temperature heat treatment: The Cu-Zn-Sn-S precursor solution is dropped on the four corners and the middle of the molybdenum glass, and spin coating is performed after the solution completely covers the surface; after the spin coating is completed, the wet film is baked and low-temperature heat treated, and the spin coating-baking-low-temperature heat treatment steps are repeated 10 times to obtain a Cu-Zn-Sn-S precursor film.
2. The method for preparing a copper-zinc-tin-sulfur precursor film by a low-temperature heat treatment process according to claim 1, characterized in that: The element ratio design of the precursor solution follows the principle of poor copper and rich zinc, and the molar ratios of the constituent elements Cu / (Zn+Sn) and Z11 / Sn are designed to be 0.72 and 1.14; The water bath reaction temperature was 66°C and the reaction time was 3 hours.
3. The method for preparing a copper-zinc-tin-sulfur precursor film by a low-temperature heat treatment process according to claim 2, characterized in that: The size of the molybdenum glass is 2×2 cm, including a 2 mm thick soda-lime glass and a 1 μm thick molybdenum layer; the parameters of the spin coating setting are: a rotation speed of 3600 r / min and a time of 36 s; baking parameters: a time of 2 min and a temperature of 300° C.; low-temperature heat treatment parameters: a time of 5 min and a temperature of 50° C.
4. A copper-zinc-tin-sulfur-selenium absorption layer film, characterized in that: The absorption layer film is prepared by high-temperature sulfur-selenization of a copper-zinc-tin-sulfur (Cu-Zn-Sn-S) precursor film prepared by the method described in claim 1; the method is as follows: The copper-zinc-tin-sulfur (Cu-Zn-Sn-S) precursor film, tin sulfide (SnS) and selenium pellets (Se) are subjected to high-temperature sulfur-selenization to obtain the copper-zinc-tin-sulfur-selenium absorption layer film (CZTSSe film).
5. The copper-zinc-tin-sulfur-selenium absorption layer thin film according to claim 4, characterized in that: There is a specific quantitative relationship between the copper-zinc-tin-sulfur (Cu-Zn-Sn-S) precursor film and stannous sulfide (SnS) and selenium pills (Se), and the ratio is 4 pieces: 10 mg: 350 mg.
6. The copper-zinc-tin-sulfur-selenium absorption layer thin film according to claim 4, characterized in that: The operation of the sulfur-selenization is as follows: heating from room temperature to 280°C and maintaining for 10 minutes for soft sulfur-selenization, with a heating rate of 28.3°C / min; continuing to heat to 510°C to start high-temperature sulfur-selenization and timing, with a heating rate of 25.5°C / min during this process; The high-temperature sulfur-selenization was repeated twice between 510°C and 570°C, with the heating and cooling rates both being 17.1°C / min, thus completing the entire sulfur-selenization process.
7. A copper-zinc-tin-sulfur-selenium solar cell, characterized in that: The solar cell comprises the copper-zinc-tin-sulfur-selenium absorption layer thin film as claimed in claim 4.
8. The copper-zinc-tin-sulfur-selenium solar cell according to claim 7, characterized in that: The preparation operation is as follows: A 50 nm thick CdS buffer layer is first deposited on the copper zinc tin sulfur selenium absorption layer film (CZTSSe film), and then a 50 nm thick intrinsic zinc oxide (i-ZnO) and a 230 nm thick tin-doped indium oxide (ITO) window layer are deposited by magnetron sputtering, and finally a 100 nm thick Ag electrode is thermally evaporated to complete the preparation of the copper zinc tin sulfur selenium solar cell (CZTSSe thin film solar cell).
9. The copper-zinc-tin-sulfur-selenium solar cell according to claim 8, characterized in that: The CdS film was deposited by a chemical water bath method, the water bath temperature was 70°C, the rotation speed was 600r / min; the background vacuum of magnetron sputtering was 5×10 -4 Pa, the working gas pressure of sputtering i-ZnO is 0.5Pa, the sputtering power is 35W-20min, 60W-5min; the working gas pressure of sputtering ITO is 0.3Pa, the power is 80W-90min.
10. The copper-zinc-tin-sulfur-selenium solar cell according to claim 8, characterized in that: The copper-zinc-tin-sulfur-selenium solar cell has a structure of SLG / Mo / CZTSSe / CdS / i-ZnO / ITO / Ag.
Citation Information
Patent Citations
Copper-zinc-tin-sulfur-selenium thin film, preparation method and copper-zinc-tin-sulfur-selenium thin film solar cell comprising same
CN117133660A
Copper-zinc-tin-sulfur-selenium thin film prepared by variable-temperature sulfur selenylation process, method and solar cell
CN117613143A
Porous CZTS-based thin fiom and Its manufacturing method
KR101583361B1