MoO3 / Fe2 (MoO4) 3 composite material as well as preparation method and application thereof

By preparing MoO3/Fe2(MoO4)3 composite material and building a heterojunction, the problems of poor catalytic performance and poor conductivity of photoelectric catalysts were solved, and the efficiency and stability of photoelectric catalytic synthesis were significantly improved.

CN118978186AActive Publication Date: 2024-11-19CHANGAN UNIV

Patent Information

Application Number
CN202411051146.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-11-19
Estimated Expiration
2044-08-01

AI Technical Summary

Technical Problem

The poor catalytic performance, poor conductivity and low synthesis efficiency of existing photoelectric catalysts limit the effectiveness of photoelectric catalytic synthesis.

Method used

Prepare MoO3/Fe2(MoO4)3 composite material, by dissolving (NH4)6Mo7O24·4H2O and Fe(NO3)9H2O in solvent, mixing and stirring and calcining, Fe2(MoO4)3 is formed, and mixed with NaBH4 and PVP, further Combined with MoO3, a heterojunction is constructed to improve photoelectrocatalytic performance.

Benefits of technology

The efficiency and selectivity of photoelectric catalytic synthesis of ammonia was significantly improved, with a yield of 2.04 mmol·h-1·gcat-1, a Faraday efficiency of 40%, and good chemical stability was maintained during cycle tests.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978186A_ABST
    Figure CN118978186A_ABST
Patent Text Reader

Abstract

The invention discloses a MoO3 / Fe2 (MoO4) 3 composite material as well as a preparation method and application thereof, and belongs to the technical field of chemical catalytic materials. The preparation method comprises the following steps: respectively dissolving (NH4) 6Mo7O24. 4H2O and Fe (NO3). 9H2O in a solvent to obtain a solution A and a solution B, and then mixing and stirring the solutions for reaction; and finally, separating solids in reactants, drying, grinding and calcining to obtain Fe2 (MoO4) 3. The preparation method comprises the following steps: uniformly mixing Fe2 (MoO4) 3, PVP and water, adding a NaBH4 solution, stirring, and separating to obtain a solid product; and mixing the solid product and (NH4) 6Mo7O24. 4H2O in a solvent, continuously stirring, evaporating and drying to obtain a solid, and calcining the solid to obtain the catalyst. The composite material prepared by the invention has high photoelectrocatalysis performance, and has high synthetic ammonia yield, Faraday efficiency and chemical stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of chemical catalytic materials, and in particular to a MoO 3 / Fe 2 (MoO 4 ) 3 Composite materials and their preparation methods and applications. Background Art

[0002] Ammonia (NH 3 ), as an indispensable chemical raw material for human society, plays an important role in industry and agriculture. However, commercial NH 3 The synthesis is mainly achieved by the Haber-Bosch (HB) process under harsh reaction conditions (650-750K, 150-350bar). 2 and N 2 The preparation and compression of NH 2 consumes about 2% of the world's fossil fuels, which leads to a large amount of greenhouse gas emissions. Therefore, it is necessary to develop an efficient and sustainable NH 3 Synthesis pathway is one of the key topics of concern in today's society. So far, various advanced methods have been proposed to promote N 2 Converted to NH 3 , such as biochemical, electrochemical, photocatalytic and photoelectrochemical (PEC); these technologies do not produce large amounts of CO 2 , especially photoelectrocatalytic N 2 reduction reaction (PEC NRR), due to photocatalysis and electrochemical 3 Synergistic effects in synthesis often manifest themselves in significant catalytic performance.

[0003] Due to N 2 It is an extremely stable molecule, so it is designed with excellent N 2 Photoelectric materials with good adsorption / activation ability are crucial. In recent years, the emergence of abundant reactive sites in photocathode materials has provided new opportunities and challenges for the field of PEC NRR. 2 O 3 As N 2 The reduction of ammonia synthesis catalyst has a certain effect. In the tandem PEC cell under AM 1.5G solar irradiation, the ideal efficiency of solar energy conversion is about 15.5%. However, α-Fe 2 O 3The photoelectrocatalytic performance is limited by certain factors, such as the high recombination rate of electrons and holes, the low diffusion length of holes (2-4nm) and poor conductivity, which leads to a large overpotential of light-assisted nitrogen reduction and low efficiency of ammonia synthesis. How to prepare a composite material with multiple composite sites, high photocatalytic performance and conductivity, high selectivity and photoelectrocatalytic efficiency is one of the key issues to be solved in the field of photoelectrocatalytic ammonia synthesis technology. Summary of the invention

[0004] In order to solve the above technical problems, the purpose of the present invention is to provide a MoO 3 / Fe 2 (MoO 4 ) 3 The composite material and its preparation method and application are used to solve the problems of poor catalytic performance, poor conductivity and low efficiency of synthetic ammonia of existing photoelectric catalysts.

[0005] The technical solution of the present invention to solve the above technical problems is as follows:

[0006] A MoO 3 / Fe 2 (MoO 4 ) 3 The method for preparing the composite material comprises the following steps:

[0007] (1) First, (NH 4 ) 6 Mo 7 O 24 ·4H 2 O and Fe(NO 3 )·9H 2 O is dissolved in solvents to obtain solution A and solution B, and then solution A and solution B are mixed and stirred continuously to react; finally, the solid in the reactant is separated, dried, ground, and calcined to obtain Fe 2 (MoO 4 ) 3 ;

[0008] (2) The Fe obtained in step (1) 2 (MoO 4 ) 3 , PVP and water are mixed evenly, and NaBH 4 solution, stirring and separating to obtain a solid product;

[0009] (3) The solid product obtained in step (2) and (NH 4 ) 6 Mo 7 O 24 ·4H 2 O is mixed in a solvent, and the mixture is evaporated to dryness after continuous stirring to obtain a solid, and the solid is calcined to obtain the product.

[0010] The beneficial effects of the present invention are: the present invention converts MoO 3 with Fe 2 (MoO 4 ) 3 Successfully compounded, according to the atomic molar ratio of Mo, MoO with high photoelectrocatalytic nitrogen reduction to ammonia synthesis performance was prepared 3 / Fe 2 (MoO 4 ) 3 -x composite catalyst. Studies have shown that the structure of defects reduces the Fe 2 (MoO 4 ) 3 -x valence band position, reducing the electron from MoO 3 Transition to Fe 2 (MoO 4 ) 3 -x free energy, which is conducive to accelerating the transfer of electrons, thereby further promoting N 2 Reduction reaction. 2 (MoO 4 ) 3 -x has a strong N due to the structural oxygen vacancy 2 The adsorption effect provides a good foundation for the subsequent breaking of the N≡N triple bond and the hydrogenation reduction steps; at the same time, the construction of the heterojunction reduces the recombination of photogenerated electrons and holes, accelerates the charge transfer, and significantly improves the photoelectrocatalytic ammonia synthesis effect.

[0011] Furthermore, in step (1), the volume ratio of solution A to solution B is 0.8-1.2:0.8-1.2.

[0012] Preferably, in step (1), the volume ratio of solution A to solution B is 1:1.

[0013] Furthermore, in solution A (NH 4 ) 6 Mo 7 O 24 ·4H 2 The mass volume ratio of O and solvent is 1g:4-8mL, and the solvent is ethylene glycol; the Fe(NO 3 )·9H 2 The mass volume ratio of O and solvent is 1g:5-10mL, and the solvent is ethylene glycol.

[0014] Furthermore, in step (1), the continuous stirring time is 5 to 10 hours; the reaction temperature is 150 to 200° C., and the time is 10 to 15 hours; the drying temperature is 50 to 70° C., and the time is 5 to 10 hours; and the calcination temperature is 500 to 600° C., and the time is 8 to 12 hours.

[0015] Preferably, the continuous stirring time in step (1) is 8 hours; the reaction temperature is 170° C. and the time is 12 hours; the drying temperature is 60° C. and the time is 8 hours; and the calcination temperature is 550° C. and the time is 10 hours.

[0016] Furthermore, in step (2), Fe 2 (MoO 4 ) 3 The mass ratio of NaBH to PVP is 1:1.5~2; 4 Solution and Fe 2 (MoO 4 ) 3 The volume ratio of the mixed solution of PVP and water is 1:4-6, NaBH 4 The concentration of the solution is 5 to 100 μmol·L -1 .

[0017] Preferably, in step (2), Fe 2 (MoO 4 ) 3 The mass ratio of NaBH to PVP is 1:1.7; 4 Solution and Fe 2 (MoO 4 ) 3 The volume ratio of the mixed solution of PVP and water is 1:5.

[0018] Further, in step (2), NaBH 4 The solution is added dropwise and the stirring time is 30-90 minutes.

[0019] Furthermore, in step (3), the solid product (NH 4 ) 6 Mo 7 O 24 ·4H 2 The mass volume ratio of O and solvent is 8-9 g:1 g:100-200 mL, and the solvent is ethanol.

[0020] Furthermore, the continuous stirring time in step (3) is 20-30 hours; the calcination conditions are: heating to 500-600° C. at a heating rate of 4-6° C. and calcining for 8-12 hours.

[0021] Preferably, the continuous stirring time in step (3) is 24 hours; the calcination conditions are: heating to 550° C. at a heating rate of 5° C. and calcining for 10 hours.

[0022] A MoO 3 / Fe 2 (MoO 4 ) 3The composite material is prepared by adopting the preparation method.

[0023] The above MoO 3 / Fe 2 (MoO 4 ) 3 Application of composite materials in photoelectrocatalytic ammonia synthesis.

[0024] The present invention has the following beneficial effects:

[0025] (1) MoO prepared by the present invention 3 / Fe 2 (MoO 4 ) 3 The presence of oxygen vacancies in the composite material makes Fe 2 (MoO 4 ) 3 There are defective energy levels in the band gap, which reduces the valence band energy, reduces the band gap width, and improves the light absorption performance; MoO 3 / Fe 2 (MoO 4 ) 3 The construction of heterojunction reduces the recombination of photogenerated electrons and holes, accelerates electron transfer, and promotes the participation of electrons with high reduction potential in N 2 Reduction reaction.

[0026] (2) MoO provided by the present invention 3 / Fe 2 (MoO 4 ) 3 The composite material is used in synthetic ammonia, which can make the synthetic ammonia yield reach 2.04mmol·h -1 ·g cat -1 and 40% Faradaic efficiency, and almost no decrease in ammonia production efficiency after 6 cycle tests, indicating good chemical stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 is the XRD pattern in Experimental Example 1;

[0028] Figure 2 The UV-visible diffuse reflectance spectra and band gap diagrams in Experimental Example 2, wherein (a) and (c) are spectra, and (b) and (d) are band gap diagrams;

[0029] Figure 3 The nitrogen adsorption-desorption isotherm and pore size distribution diagram in Experimental Example 3, wherein (a) is the nitrogen adsorption-desorption isotherm, and (b) is the pore size distribution diagram;

[0030] Figure 4 It is the linear sweep voltammetry curve in Experimental Example 4;

[0031] Figure 5 is the transient photocurrent diagram in Experimental Example 5;

[0032] Figure 6 The electrochemical impedance diagram in Experimental Example 6;

[0033] Figure 7 The electrochemical ammonia synthesis efficiency and Faraday efficiency diagram in Experimental Example 7;

[0034] Figure 8 This is a graph showing the cycle stability test results at -0.6V vs. RHE bias voltage in Experimental Example 8. DETAILED DESCRIPTION

[0035] The principles and features of the present invention are described below in conjunction with the accompanying drawings. The examples are only used to explain the present invention and are not used to limit the scope of the present invention. If specific conditions are not specified in the embodiments, they are carried out according to normal conditions or conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0036] Embodiment 1:

[0037] A MoO 3 / Fe 2 (MoO 4 ) 3 The method for preparing the composite material comprises the following steps:

[0038] (1)Fe 2 (MoO 4 ) 3 Preparation

[0039] First, 2.47g (NH 4 ) 6 Mo 7 O 24 ·4H 2 O was added to 20 mL of ethylene glycol and ultrasonicated for 30 min until it was completely dissolved to obtain solution A. 3.77 g Fe(NO 3 )·9H 2 O was added into 20 mL of ethylene glycol and ultrasonicated for 30 min to completely dissolve to obtain solution B;

[0040] Then, after solution A and solution B are mixed, the solution turns orange-red, and after continuous stirring for 8 hours, an orange-red precipitate appears in the solution. The stirred mixed solution is transferred to a 100 mL polytetrafluoroethylene liner, the liner is placed in a stainless steel reactor and sealed, and the reactor is placed in a 170°C forced air drying oven for reaction for 12 hours;

[0041] Finally, after cooling to room temperature, the reactants were taken out and centrifuged with pure water and ethanol respectively. The obtained solid was dried in an oven at 60°C for 8 hours and then fully ground with a mortar. The ground powder was placed in a magnetic boat and calcined at 550°C for 10 hours and cooled to room temperature to obtain brick red Fe 2 (MoO 4 ) 3 powder.

[0042] (2)Fe 2 (MoO 4 ) 3 -X Preparation

[0043] The Fe obtained in step (1) 2 (MoO 4 ) 3 0.592 g of powder and 1 g of PVP were added to 100 mL of pure water and ultrasonicated for 30 min to make them dispersed evenly. 20 mL of 10 μmol·L -1 NaBH 4 The solution was stirred for 1 h and then the solid was separated to obtain Fe 2 (MoO 4 ) 3 -10.

[0044] (3)MoO 3 / Fe 2 (MoO 4 ) 3 Preparation of composite materials

[0045] Add 1.478 g of Fe prepared in step (2) to 20 mL of ethanol. 2 (MoO 4 ) 3 -10, stir evenly and add 0.17g (NH 4 ) 6 Mo 7 O 24 ·4H 2 O, and then evaporated at 80 °C after continuous stirring for 24 h to obtain a dry solid. The solid was calcined in a muffle furnace for 6 h at a heating rate of 5 °C / min to obtain a composite material MoO 3 / Fe 2 (MoO 4 ) 3 -10.

[0046] Embodiment 2:

[0047] A MoO 3 / Fe 2 (MoO 4 ) 3The method for preparing the composite material comprises the following steps:

[0048] (1)Fe 2 (MoO 4 ) 3 Preparation

[0049] First, 2.47g (NH 4 ) 6 Mo 7 O 24 ·4H 2 O was added to 20 mL of ethylene glycol and ultrasonicated for 30 min until it was completely dissolved to obtain solution A. 3.77 g Fe(NO 3 )·9H 2 O was added into 20 mL of ethylene glycol and ultrasonicated for 30 min to completely dissolve to obtain solution B;

[0050] Then, after solution A and solution B are mixed, the solution turns orange-red, and after continuous stirring for 8 hours, an orange-red precipitate appears in the solution. The stirred mixed solution is transferred to a 100 mL polytetrafluoroethylene liner, the liner is placed in a stainless steel reactor and sealed, and the reactor is placed in a 170°C forced air drying oven for reaction for 12 hours;

[0051] Finally, after cooling to room temperature, the reactants were taken out and centrifuged with pure water and ethanol respectively. The obtained solid was dried in an oven at 60°C for 8 hours and then fully ground with a mortar. The ground powder was placed in a magnetic boat and calcined at 550°C for 10 hours and cooled to room temperature to obtain brick red Fe 2 (MoO 4 ) 3 powder.

[0052] (2)Fe 2 (MoO 4 ) 3 -X Preparation

[0053] The Fe obtained in step (1) 2 (MoO 4 ) 3 0.592 g of powder and 1 g of PVP were added to 100 mL of pure water and ultrasonicated for 30 min to make them dispersed evenly. 20 mL of 30 μmol·L -1 NaBH 4 The solution was stirred for 1 h and then the solid was separated to obtain Fe 2 (MoO 4 ) 3 -30.

[0054] (3)MoO 3 / Fe 2 (MoO4 ) 3 Preparation of composite materials

[0055] Add 1.478 g of Fe prepared in step (2) to 20 mL of ethanol. 2 (MoO 4 ) 3 -30, stir evenly and add 0.17g (NH 4 ) 6 Mo 7 O 24 ·4H 2 O, and then evaporated at 80 °C after continuous stirring for 24 h to obtain a dry solid. The solid was calcined in a muffle furnace for 6 h at a heating rate of 5 °C / min to obtain a composite material MoO 3 / Fe 2 (MoO 4 ) 3 -30.

[0056] Embodiment 3:

[0057] A MoO 3 / Fe 2 (MoO 4 ) 3 The method for preparing the composite material comprises the following steps:

[0058] (1)Fe 2 (MoO 4 ) 3 Preparation

[0059] First, 2.47g (NH 4 ) 6 Mo 7 O 24 ·4H 2 O was added to 20 mL of ethylene glycol and ultrasonicated for 30 min until it was completely dissolved to obtain solution A. 3.77 g Fe(NO 3 )·9H 2 O was added into 20 mL of ethylene glycol and ultrasonicated for 30 min to completely dissolve to obtain solution B;

[0060] Then, after solution A and solution B are mixed, the solution turns orange-red, and after continuous stirring for 8 hours, an orange-red precipitate appears in the solution. The stirred mixed solution is transferred to a 100 mL polytetrafluoroethylene liner, the liner is placed in a stainless steel reactor and sealed, and the reactor is placed in a 170°C forced air drying oven for reaction for 12 hours;

[0061] Finally, after cooling to room temperature, the reactants were taken out and centrifuged with pure water and ethanol respectively. The obtained solid was dried in an oven at 60°C for 8 hours and then fully ground with a mortar. The ground powder was placed in a magnetic boat and calcined at 550°C for 10 hours and cooled to room temperature to obtain brick red Fe 2 (MoO 4 ) 3 powder.

[0062] (2)Fe 2 (MoO 4 ) 3 -X Preparation

[0063] The Fe obtained in step (1) 2 (MoO 4 ) 3 0.592 g of powder and 1 g of PVP were added to 100 mL of pure water and ultrasonicated for 30 min to make them dispersed evenly. 20 mL of 50 μmol·L -1 NaBH 4 The solution was stirred for 1 h and then the solid was separated to obtain Fe 2 (MoO 4 ) 3 -50.

[0064] (3)MoO 3 / Fe 2 (MoO 4 ) 3 Preparation of composite materials

[0065] Add 1.478 g of Fe prepared in step (2) to 20 mL of ethanol. 2 (MoO 4 ) 3 -50, stir evenly and add 0.17g (NH 4 ) 6 Mo 7 O 24 ·4H 2 O, and then evaporated at 80 °C after continuous stirring for 24 h to obtain a dry solid. The solid was calcined in a muffle furnace for 6 h at a heating rate of 5 °C / min to obtain a composite material MoO 3 / Fe 2 (MoO 4 ) 3 -50.

[0066] Embodiment 4:

[0067] A MoO 3 / Fe 2 (MoO 4 ) 3The method for preparing the composite material comprises the following steps:

[0068] (1)Fe 2 (MoO 4 ) 3 Preparation

[0069] First, 2.47g (NH 4 ) 6 Mo 7 O 24 ·4H 2 O was added to 20 mL of ethylene glycol and ultrasonicated for 30 min until it was completely dissolved to obtain solution A. 3.77 g Fe(NO 3 )·9H 2 O was added into 20 mL of ethylene glycol and ultrasonicated for 30 min to completely dissolve to obtain solution B;

[0070] Then, after solution A and solution B are mixed, the solution turns orange-red, and after continuous stirring for 8 hours, an orange-red precipitate appears in the solution. The stirred mixed solution is transferred to a 100 mL polytetrafluoroethylene liner, the liner is placed in a stainless steel reactor and sealed, and the reactor is placed in a 170°C forced air drying oven for reaction for 12 hours;

[0071] Finally, after cooling to room temperature, the reactants were taken out and centrifuged with pure water and ethanol respectively. The obtained solid was dried in an oven at 60°C for 8 hours and then fully ground with a mortar. The ground powder was placed in a magnetic boat and calcined at 550°C for 10 hours and cooled to room temperature to obtain brick red Fe 2 (MoO 4 ) 3 powder.

[0072] (2)Fe 2 (MoO 4 ) 3 -X Preparation

[0073] The Fe obtained in step (1) 2 (MoO 4 ) 3 0.592 g of powder and 1 g of PVP were added to 100 mL of pure water and ultrasonicated for 30 min to make them dispersed evenly. 20 mL of 70 μmol·L -1 NaBH 4 The solution was stirred for 1 h and then the solid was separated to obtain Fe 2 (MoO 4 ) 3 -70.

[0074] (3)MoO 3 / Fe 2 (MoO4 ) 3 Preparation of composite materials

[0075] Add 1.478 g of Fe prepared in step (2) to 20 mL of ethanol. 2 (MoO 4 ) 3 -70, and then add 0.17g (NH 4 ) 6 Mo 7 O 24 ·4H 2 O, and then evaporated at 80 °C after continuous stirring for 24 h to obtain a dry solid. The solid was calcined in a muffle furnace for 6 h at a heating rate of 5 °C / min to obtain a composite material MoO 3 / Fe 2 (MoO 4 ) 3 -70.

[0076] Comparative Example 1:

[0077] A MoO 3 / Fe 2 (MoO 4 ) 3 The method for preparing the composite material comprises the following steps:

[0078] (1)Fe 2 (MoO 4 ) 3 Preparation

[0079] First, 2.47g (NH 4 ) 6 Mo 7 O 24 ·4H 2 O was added to 20 mL of ethylene glycol and ultrasonicated for 30 min until it was completely dissolved to obtain solution A. 3.77 g Fe(NO 3 )·9H 2 O was added into 20 mL of ethylene glycol and ultrasonicated for 30 min to completely dissolve to obtain solution B;

[0080] Then, after solution A and solution B are mixed, the solution turns orange-red, and after continuous stirring for 8 hours, an orange-red precipitate appears in the solution. The stirred mixed solution is transferred to a 100 mL polytetrafluoroethylene liner, the liner is placed in a stainless steel reactor and sealed, and the reactor is placed in a 170°C forced air drying oven for reaction for 12 hours;

[0081] Finally, after cooling to room temperature, the reactants were taken out and centrifuged with pure water and ethanol respectively. The obtained solid was dried in an oven at 60°C for 8 hours and then fully ground with a mortar. The ground powder was placed in a magnetic boat and calcined at 550°C for 10 hours and cooled to room temperature to obtain brick red Fe 2 (MoO 4 ) 3 powder.

[0082] (2) MoO 3 / Fe 2 (MoO 4 ) 3 Preparation of composite materials

[0083] Add 1.478 g of Fe prepared in step (1) to 20 mL of ethanol. 2 (MoO 4 ) 3 , stir evenly and add 0.17g (NH 4 ) 6 Mo 7 O 24 ·4H 2 O, and then evaporated at 80 °C after continuous stirring for 24 h to obtain a dry solid. The solid was calcined in a muffle furnace for 6 h at a heating rate of 5 °C / min to obtain a composite material MoO 3 / Fe 2 (MoO 4 ) 3 .

[0084] Test Example 1: XRD Analysis

[0085] The Fe prepared in Example 2 2 (MoO 4 ) 3 、MoO 3 / Fe 2 (MoO 4 ) 3 -30 and pure MoO 3 X-ray diffraction analysis was performed on the samples using a PANalytical X'Pert PRO X-ray diffraction instrument at a scanning speed of 10° / min and a scanning angle of 10-80°.

[0086] The experimental results are as follows Figure 1 As shown. Figure 1 It can be seen that Fe 2 (MoO 4 ) 3The peaks at 13.79°, 15.32°, 20.43°, 21.76°, 22.66°, 22.99°, 24.90°, 25.71°, and 27.50° completely correspond to the (200), (012), (120), (214), (022), (202), (212), (122), and (224) crystal planes of the standard card PDF#83-1701, indicating the successful preparation of the material. MoO 3 The diffraction peaks at 23.33°, 25.698°, 25.88°, 27.32°, 33.76°, and 38.9° completely correspond to the (110), (040), (120), (021), (111), and (060) crystal planes of the standard card PDF#76-1003. 2 (MoO4) 3 / MoO 3 The -30 composite material has all the peaks corresponding to the two substances, indicating the successful preparation of the material.

[0087] Test Example 2: UV-Vis Diffuse Reflectance Analysis

[0088] For pure MoO 3 , Fe prepared in Example 1 2 (MoO 4 ) 3 , Fe prepared in Example 1-4 2 (MoO 4 ) 3 -10, Fe 2 (MoO 4 ) 3 -30, Fe 2 (MoO 4 ) 3 -50, Fe 2 (MoO 4 ) 3 -70, MoO prepared in Example 2 3 / Fe 2 (MoO 4 ) 3 -30 and MoO prepared in Comparative Example 1 3 / Fe 2 (MoO 4 ) 3 For characterization, the above samples were measured in the spectral range of 200-800nm ​​with barium sulfate as the reference condition using an Agilent Cary 100 UV spectrophotometer to obtain the UV-visible diffuse reflectance spectrum of each sample.

[0089] The experimental results are as follows Figure 2 As shown, from Figure 2 It can be seen that MoO3 There is light absorption in the wavelength range of 300-450nm, Fe 2 (MoO 4 ) 3 The light absorption range of MoO is 300-630nm. 3 / Fe 2 (MoO 4 ) 3 and MoO 3 / Fe 2 (MoO 4 ) 3 -30 has light absorption in the range of 300-800nm, and the absorption intensity in the range of 300-800nm ​​is higher than that of MoO 3 and Fe 2 (MoO 4 ) 3 There are significant improvements. It is worth noting that in 480-800nm ​​MoO 3 / Fe 2 (MoO 4 ) 3 -30 has a higher light absorption than MoO 3 / Fe 2 (MoO 4 ) 3 . Fe with different oxygen vacancies 2 (MoO 4 ) 3 -x responds differently to light. In the range of 300-800nm, Fe 2 (MoO 4 ) 3 -30 has the largest light absorption range and the highest light absorption intensity.

[0090] like Figure 2 As shown in Figures (b) and (d), MoO 3 and Fe 2 (MoO 4 ) 3 The band gaps of Fe and Fe are 2.80eV and 2.87eV respectively. When different amounts of oxygen vacancies are introduced, the band gaps are narrowed to varying degrees. 2 (MoO 4 ) 3 -30 band gap changes the most, to 2.30eV. Therefore, Fe 2 (MoO 4 ) 3 -30 exhibits strong light absorption performance and a wide light absorption range. It is possible to generate more photogenerated carriers under irradiation, which is conducive to the photoexcitation of valence band electrons to the conduction band, thereby participating in the subsequent nitrogen reduction reaction.

[0091] Test Example 3: Adsorption isotherm and specific surface area and pore size distribution analysis

[0092] The Fe prepared in Example 2 was measured using a Micromeritics ASAP 2460 instrument. 2 (MoO 4 ) 3 , Fe 2 (MoO 4 ) 3 -30 and MoO 3 / Fe 2 (MoO 4 ) 3 -30 for analysis of adsorption isotherm, specific surface area and pore size distribution.

[0093] The experimental results are as follows Figure 3 As shown. Figure 3 It can be seen that all samples showed H3 type hysteresis curves, proving that these three electrode materials have mesoporous structures. 2 (MoO 4 ) 3 , Fe 2 (MoO 4 ) 3 -30, MoO 3 / Fe 2 (MoO 4 ) 3 The average pore sizes of -30 are 17.63, 12.2, and 16.04 nm, respectively. The Fe 2 (MoO 4 ) 3 , Fe 2 (MoO 4 ) 3 -30 and MoO 3 / Fe 2 (MoO 4 ) 3 -30 The specific surface areas of the electrode materials are 7.29, 13.35, and 35.12 m 2 g -1 The creation of oxygen vacancies and the composite of materials increase the Fe 2 (MoO 4 ) 3 The larger specific surface area increases the reactive sites, which is beneficial to N 2 The pore size distribution diagram ( Figure 3 Figure (b) shows that Fe2 (MoO 4 ) 3 , Fe 2 (MoO 4 ) 3 -30 and MoO 3 / Fe 2 (MoO 4 ) 3 The pores of -30 electrode materials are mainly mesopores.

[0094] Test Example 4: Photoresponse performance measurement

[0095] The Fe prepared in Example 2 2 (MoO 4 ) 3 , Fe 2 (MoO 4 ) 3 -30, MoO 3 / Fe 2 (MoO 4 ) 3 -30, MoO prepared in Comparative Example 1 3 / Fe 2 (MoO 4 ) 3 and pure MoO 3 The LSV curve, i.e., the linear sweep voltammetry curve of the composite electrode, was tested by an electrochemical workstation model CHI6503, using a three-electrode system, with the Ag / AgCl electrode as the reference electrode, the platinum electrode as the counter electrode, and the test sample as the working electrode.

[0096] The experimental results are as follows Figure 4 As shown. Figure 4 It can be seen that Fe 2 (MoO 4 ) 3 、MoO 3 、MoO 3 / Fe 2 (MoO 4 ) 3 , Fe 2 (MoO 4 ) 3 -30, MoO 3 / Fe 2 (MoO 4 ) 3 The voltages of -30 at -1.2 V vs. RHE are -0.15, -1.04, -3.02, -4.98, and -6.22 mA·cm -2 .MoO 3 / Fe 2 (MoO4 ) 3 The photocurrent of -30 is pure Fe 2 (MoO 4 ) 3 and pure MoO 3 41.5 and 5.98 times.

[0097] Test Example 5: Photosensitivity measurement

[0098] The Fe prepared in Example 2 2 (MoO 4 ) 3 , Fe 2 (MoO 4 ) 3 -30, MoO 3 / Fe 2 (MoO 4 ) 3 -30, MoO prepared in Comparative Example 1 3 / Fe 2 (MoO 4 ) 3 and pure MoO 3 The photosensitivity was measured by using a CHI6503 electrochemical workstation to determine the It curve.

[0099] The experimental results are as follows Figure 5 As shown. Figure 5 You can see MoO 3 / Fe 2 (MoO 4 ) 3 -30 The instantaneous current density of the photocatalytic material when the light is turned on and off is 5μA·cm -2 The TPR value of Fe 2 (MoO 4 ) 3 The TPR value of -30 is smaller: 4.03μA·cm -2 , Fe 2 (MoO 4 ) 3 、MoO 3 、MoO 3 / Fe 2 (MoO 4 ) 3 The TPR values ​​are very low, respectively: 2.32μA·cm -2 , 1.05μA·cm -2 , 0.98μA·cm -2 .

[0100] Test Example 6: Electrochemical Impedance Spectroscopy Measurement

[0101] The Fe prepared in Example 2 2 (MoO 4 ) 3 , Fe 2 (MoO 4 ) 3 -30, MoO 3 / Fe 2 (MoO 4 ) 3 -30, MoO prepared in Comparative Example 1 3 / Fe 2 (MoO 4 ) 3 and pure MoO 3 Electrochemical impedance spectroscopy is performed to test the carrier migration and separation dynamics of the electrode. Generally, the smaller the radius of the electrochemical impedance spectroscopy, the greater the photogenerated electron-hole transfer rate.

[0102] The experimental results are as follows Figure 6 As shown. Figure 6 It can be seen that Fe 2 (MoO 4 ) 3 The radius is the largest, composite MoO 3 After MoO 3 / Fe 2 (MoO 4 ) 3 The smaller the radius of the electrochemical impedance spectrum, the smaller the MoO 3 The construction of heterojunction increases the reaction kinetics and improves the carrier transfer efficiency. 2 (MoO 4 ) 3 -30 radius is Fe 2 (MoO 4 ) 3 Small, even smaller than MoO 3 / Fe 2 (MoO 4 ) 3 The radius of the oxygen vacancy increases the Fe 2 (MoO 4 ) 3 The electron capture ability of MoO reduces the recombination of electrons and holes to a certain extent, which is beneficial for holes to participate in subsequent reactions. 3 / Fe 2 (MoO 4 ) 3 The radius of -30 is the smallest, indicating that the synergistic effect of the heterojunction and defect oxygen vacancies improves the reaction kinetics.

[0103] Test Example 7: Photocatalytic activity measurement

[0104] The photoelectrocatalytic ammonia synthesis performance of the samples was studied using nitrogen as the nitrogen source, a xenon lamp to simulate sunlight, and 1 mol / L KOH as the electrolyte. The test sample was the Fe prepared in Example 2. 2 (MoO 4 ) 3 , Fe 2 (MoO 4 ) 3 -30, MoO 3 / Fe 2 (MoO 4 ) 3 -30, MoO prepared in Comparative Example 1 3 / Fe 2 (MoO 4 ) 3 and pure MoO 3 Before the reaction, nitrogen was pre-flowed into the cathode cell for 0.5 h to 1 h to form a nitrogen-saturated KOH solution, and then constant potential electrolysis was performed (nitrogen reduction reaction and hydrogen evolution reaction occurred at the cathode, and oxygen evolution reaction occurred at the anode) for 2 h. The stirring speed was set to 400 rpm. After 2 h of reaction, samples were taken for testing to obtain the yield.

[0105] The experimental results are as follows Figure 7 As shown. When the bias voltage is -0.6V vs.RHE, Fe 2 (MoO 4 ) 3 、MoO 3 、MoO 3 / Fe 2 (MoO 4 ) 3 , Fe 2 (MoO 4 ) 3 -30, MoO 3 / Fe 2 (MoO 4 ) 3 -30 ammonia synthesis efficiencies are 0.30, 0.85, 1.08, 1.36, and 2.04 mmol·h -1 ·g cat -1 , the Faradaic efficiency is: 19.02%, 3.40%, 1.28%, 8.86%, 43.00%. MoO 3 / Fe 2 (MoO 4 ) 3 -30 is Fe 2 (MoO 4 )3 6.8 times and 2.26 times. MoO 3 / Fe 2 (MoO 4 ) 3 -30 is MoO 3 2.4 times and 12.65 times. MoO 3 and Fe 2 (MoO 4 ) 3 The heterojunction formed by -30 regulates the carrier transmission channel, is beneficial to the separation of electrons and holes, and improves the efficiency of ammonia synthesis.

[0106] Test Example 8: Stability Determination

[0107] Take the MoO prepared in Example 2 3 / Fe 2 (MoO 4 ) 3 -30 composite material was subjected to stability test, and 6 cycles of ammonia synthesis experiment were carried out under the same conditions as in Test Example 7.

[0108] like Figure 8 As shown, at a bias voltage of -0.6 V vs. RHE, MoO 3 / Fe 2 (MoO 4 ) 3 After 6 cycles of 2h nitrogen reduction to synthesize ammonia reaction with -30 as the photoelectrocatalyst, the ammonia yield of the catalyst remained stable at ~98%.

[0109] In summary, the present invention comprises MoO 3 with Fe 2 (MoO 4 ) 3 Successfully compounded, according to the atomic molar ratio of Mo, MoO with high photoelectrocatalytic nitrogen reduction to ammonia synthesis performance was prepared 3 / Fe 2 (MoO 4 ) 3 -x composite catalyst. Studies have shown that the structure of defects reduces the Fe 2 (MoO 4 ) 3 -x valence band position, reducing the electron from MoO 3 Transition to Fe 2 (MoO 4 ) 3 -x free energy, which is conducive to accelerating the transfer of electrons, thereby further promoting N 2 Reduction reaction. 2 (MoO 4 )3 -x has a strong N due to the structural oxygen vacancy 2 The adsorption effect provides a good foundation for the subsequent N≡N triple bond breaking and hydrogenation reduction steps; at the same time, the construction of the heterojunction reduces the recombination of photogenerated electrons and holes and accelerates the charge transfer, so MoO 3 / Fe 2 (MoO 4 ) 3 -x's photoelectrocatalytic ammonia synthesis effect has been significantly improved.

[0110] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a MoO3 / Fe2(MoO4)3 composite material, characterized in that: The following steps are involved: (1) First, (NH4)6Mo7O 24 ·4H2O and Fe(NO3)·9H2O are dissolved in solvents to obtain solution A and solution B respectively, and then solution A and solution B are mixed and stirred continuously to react; finally, the solid in the reactant is separated, dried, ground, and calcined to obtain Fe2(MoO4)3; (2) uniformly mixing the Fe2(MoO4)3, PVP and water obtained in step (1), adding NaBH4 solution, stirring and separating to obtain a solid product; (3) The solid product obtained in step (2) and (NH4)6Mo7O 24 ·4H2O is mixed in a solvent, and the mixture is evaporated to dryness after continuous stirring to obtain a solid, and the solid is calcined to obtain the product.

2. The method for preparing the MoO3 / Fe2(MoO4)3 composite material according to claim 1, characterized in that: In the step (1), the volume ratio of solution A to solution B is 0.8-1.2:0.8-1.

2.

3. The method for preparing the MoO3 / Fe2(MoO4)3 composite material according to claim 1 or 2, characterized in that: In solution A, (NH4)6Mo7O 24 The mass volume ratio of Fe(NO3)·9H2O to the solvent is 1g:4-8mL, and the solvent is ethylene glycol; the mass volume ratio of Fe(NO3)·9H2O to the solvent in solution B is 1g:5-10mL, and the solvent is ethylene glycol.

4. The method for preparing the MoO3 / Fe2(MoO4)3 composite material according to claim 1, characterized in that: In the step (1), the continuous stirring time is 5 to 10 hours; the reaction temperature is 150 to 200° C. and the time is 10 to 15 hours; the drying temperature is 50 to 70° C. and the time is 5 to 10 hours; the calcination temperature is 500 to 600° C. and the time is 8 to 12 hours.

5. The method for preparing the MoO3 / Fe2(MoO4)3 composite material according to claim 1, characterized in that: In the step (2), the mass ratio of Fe2(MoO4)3 to PVP is 1:1.5-2; the volume ratio of NaBH4 solution to the mixed solution of Fe2(MoO4)3, PVP and water is 1:4-6, and the concentration of NaBH4 solution is 5-100 μmol·L -1 .

6. The method for preparing the MoO3 / Fe2(MoO4)3 composite material according to claim 1, characterized in that: In the step (2), the NaBH4 solution is added dropwise, and the stirring time is 30-90 minutes.

7. The method for preparing the MoO3 / Fe2(MoO4)3 composite material according to claim 1, characterized in that: The solid product in step (3), (NH4)6Mo7O 24 The mass volume ratio of 4H2O and solvent is 8-9g:1g:100-200mL, and the solvent is ethanol.

8. The method for preparing the MoO3 / Fe2(MoO4)3 composite material according to claim 1, characterized in that: The continuous stirring time in step (3) is 20-30 hours; the calcination conditions are: heating to 500-600° C. at a heating rate of 4-6° C. and calcining for 8-12 hours.

9. A MoO3 / Fe2(MoO4)3 composite material, characterized in that: The method is prepared according to any one of claims 1 to 7.

10. Use of the MoO3 / Fe2(MoO4)3 composite material according to claim 9 in photoelectrocatalytic synthesis of ammonia.

Citation Information

Patent Citations

  • Beaded iron molybdate nanofiber photocatalyst as well as preparation method and application

    CN111945249A

  • Synthesis method of oxygen-vacancy-rich ruthenium / nickel molybdate material and application of oxygen-vacancy-rich ruthenium / nickel molybdate material in hydrogen evolution reaction in seawater

    CN116855996A

Cited By

  • Catalyst for preparing formaldehyde through methanol oxidation and preparation method thereof

    CN121534727A