Cosmetic sponge raw material and preparation process thereof
By introducing halogen elements and chain extenders into the makeup sponge, a dense network structure is formed, which solves the problems of strong water absorption and poor makeup effects of traditional makeup sponges, and achieves a lighter and more natural makeup and a more durable sponge.
Patent Information
- Application Number
- CN202411045619.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-19
AI Technical Summary
Traditional polyurethane cosmetic sponges have problems such as strong water absorption, easy to damage, inconvenient cleaning, large friction on the skin and poor makeup effects. They are prone to adsorbing too much cosmetics, resulting in excessive thick and uneven makeup.
Using a cosmetic sponge raw material, by introducing the benzene ring of the halogen element into monoethyl malonic acid, combining a chain extender to react with the polyurethane molecular chain to form a dense and uniform network structure, reducing porosity, and through chain extension The agent enhances the interaction force between molecular chains and improves mechanical properties.
It significantly reduces the adsorption of cosmetics inside the sponge, improves the makeup effect, makes the makeup lighter and more natural, the sponge is more durable and not easy to deform, and extends the service life.
Smart Images

Figure BDA0004973409300000021 
Figure BDA0004973409300000031 
Figure BDA0004973409300000041
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polyurethane materials, and in particular to a cosmetic sponge raw material and a preparation process thereof. Background Art
[0002] As an important makeup tool, makeup sponges are traditionally made of natural or synthetic materials. As consumers' requirements for makeup effects, ease of use and personal hygiene continue to increase, the materials and technology of makeup sponges also need to continue to improve. Early makeup sponges were mostly made of natural materials, such as latex sponges. Latex sponges are extracted from rubber trees and made through a series of processing. They are favored for their good elasticity and skin-friendliness. Latex sponges not only have good water absorption, but also can simulate the effect of finger makeup to a certain extent, making the makeup more natural and docile. Due to the existence of allergens and other problems in latex materials, the wide application of its market is limited. In order to overcome the limitations of natural materials, synthetic materials based on foaming materials such as styrene butadiene copolymer (SBR), polyurethane (PU) and butadiene acrylonitrile copolymer (NBR) have gradually become a new choice for makeup sponges. Among them, polyurethane materials not only have good skin-friendliness, but also have a low chance of allergies, which can meet consumers' needs for health and safety.
[0003] However, traditional polyurethane makeup sponges have problems such as strong water absorption, easy damage, inconvenient cleaning and high friction with the skin during use. Due to its porous texture, polyurethane makeup sponges easily absorb a certain amount of foundation or other cosmetics, resulting in makeup effects that are not as good as expected, and also causing waste of cosmetics. In addition, the excess absorbed cosmetics will contaminate the makeup sponge to a certain extent, making it difficult to clean and affecting its service life. In addition, for consumers who pursue a light makeup look, the makeup sponge will make the makeup look too thick after absorbing too much cosmetics. Summary of the invention
[0004] In order to solve the problems mentioned in the above background technology, the present invention provides a cosmetic sponge raw material and a preparation process thereof.
[0005] In order to achieve the above object, the present invention adopts the following technical solutions:
[0006] A cosmetic sponge raw material, comprising component A and component B, wherein component A comprises the following raw materials in parts by weight: 40-50 parts of polyether polyol, 0.1-1 parts of slow rebound release agent, 0.002-0.01 parts of catalyst, 0.5-0.8 parts of chain extender, 4-6 parts of silicone oil and 0.1-3 parts of color paste; component B comprises the following raw materials in parts by weight: 30-40 parts of diphenylmethane diisocyanate, 0.001-0.005 parts of additives and 2-3 parts of talc;
[0007] The structural formula of the chain extender is formula (I):
[0008]
[0009] Furthermore, the polyether polyol is one or more of polyethylene glycol, polypropylene glycol and polytetramethylene glycol.
[0010] Furthermore, the additive includes 60% antioxidant and 40% antibacterial agent, wherein the antioxidant includes one of antioxidant 1010 and antioxidant 1076, and the antibacterial agent includes one of chitosan, phenolic acid and anthocyanin; and the catalyst includes one of bis(dimethylaminoethyl)ether, N,N-dimethylcyclohexylamine and bis(2-dimethylaminoethyl)ether.
[0011] Furthermore, the slow-rebound release agent includes one or more of palm wax, rice bran wax, sugarcane wax, beeswax, insect wax and polyethylene wax.
[0012] Furthermore, the chain extender is prepared by the following steps:
[0013] S1. Under nitrogen protection, add 2-chloro-4-fluorophenol, hydroxystyrene and tri(2-methoxyphenyl)phosphine to N-methylpyrrolidone (NMP) in an ice-water bath, cool to 0°C, then dropwise add diisopropyl azodicarboxylate, stir and react at room temperature after the addition is complete, pour into a saturated sodium bicarbonate solution and let stand for 1-2h, and distill under reduced pressure to obtain an intermediate product;
[0014] S2. Add the intermediate product and monoethyl malonate to a mixture of ethanol and alkali, heat and stir. After the reaction is completed, extract with ethyl acetate, collect the organic layer, wash the organic layer with saturated brine, dry the organic layer with anhydrous sodium sulfate or potassium carbonate, distill under reduced pressure until a precipitate is precipitated, and recrystallize to obtain a chain extender.
[0015] Wherein, the reaction equation in step S1 is formula (II):
[0016]
[0017] In formula (II), (o-Meoph)3p is tri(2-methoxyphenyl)phosphine, and DIAD is diisopropyl azodicarboxylate;
[0018] The reaction equation of step S2 is formula (III):
[0019]
[0020] In formula (III), EtOH is ethanol, and the purity of ethanol is 98%.
[0021] Furthermore, in step S1, the molar ratio of 2-chloro-4-fluorophenol, hydroxystyrene, tri(2-methoxyphenyl)phosphine and diisopropyl azodicarboxylate is 1:(1.2-1.5):(0.02-0.04):(0.015-0.02).
[0022] Furthermore, in step S1, the stirring speed is 200-600 rpm, and the reaction time is 1-5 h.
[0023] Furthermore, in step S2, the molar ratio of the intermediate product to monoethyl malonate is 1:(1.1-1.5), and in the mixed solution of ethanol and alkali, the mass percentage of alkali is 5-20%, and the alkali is sodium hydroxide or potassium hydroxide.
[0024] Furthermore, in step S2, the reaction temperature is 25-50° C., the stirring speed is 200-600 rpm, and the reaction time is 2-3 h.
[0025] According to another aspect of the present invention, a process for preparing the above-mentioned cosmetic sponge is provided, comprising the following steps:
[0026] Component A: 40-50 parts of polyether polyol, 0.1-1 part of slow rebound release agent, 0.002-0.01 part of catalyst, 0.5-0.8 part of chain extender, 4-6 parts of silicone oil and 0.1-3 parts of color paste are weighed by weight and added into a mixer, and reacted at a stirring speed of 500-1000 rpm for 1-2 hours to obtain a mixture of component A;
[0027] Component B: 30-40 parts of diphenylmethane diisocyanate, 0.001-0.005 parts of additives and 2-3 parts of talc are weighed by weight and added into a mixer, and stirred at a speed of 2000-3000 rpm for 10-20 minutes to obtain a component B mixture.
[0028] Compared with the prior art, the present invention has the following beneficial effects:
[0029] 1. In the technical solution of the present invention, by introducing a benzene ring containing a halogen element into the monoethyl malonate molecule, it is more difficult for cosmetics such as foundation to penetrate into the pores of the sponge, thereby greatly reducing the adsorption of cosmetics inside the sponge. The hydroxyl group in the chain extender forms a covalent bond with the reactive group (isocyanate group) on the polyurethane molecular chain, thereby enhancing the interaction force between the polyurethane molecular chains, making the molecular chains more tightly arranged and orderly, thereby forming a more compact and uniform network structure. At the same time, the introduction of the halogen element brings additional polarity or hydrophobicity to the polyurethane molecular chain, which reduces the porosity of the cosmetic sponge.
[0030] 2. Since more cosmetics stay on the surface of the sponge, the powder absorption phenomenon is reduced and the makeup effect is improved. Foundation and other cosmetics are more evenly distributed on the surface of the makeup sponge and are not easily absorbed by the sponge pores, so they can be more evenly covered on the skin, making the makeup lighter and more natural, avoiding the problem of too thick or uneven makeup due to the sponge absorbing powder.
[0031] 3. The chain extender also extends the length of the polyurethane chain and increases the molecular weight by reacting with polyether polyols and diphenylmethane diisocyanate (MDI). The molecular structure of the sponge is more complex and stable, which directly improves the mechanical properties of the sponge, making the cosmetic sponge more durable and not easy to deform, and able to maintain a stable shape and performance during use. DETAILED DESCRIPTION
[0032] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0033] Unless otherwise specified, the raw materials used in the present invention are all from conventional products purchased on the market. Among them, the CAS number of 2-chloro-4-fluorophenol is 1996-41-4, the CAS number of hydroxystyrene is 2628-17-3, the CAS number of tri(2-methoxyphenyl)phosphine is 4731-65-1, the CAS number of diisopropyl azodicarboxylate is 2446-83-5, the CAS number of monoethyl malonate is 1071-46-1, the silicone oil is dimethyl silicone oil (DC-200), and the color paste is yellow color paste, and the trade name is BASF Paliotol Yellow L0960 HD.
[0034] Preparation Example 1
[0035] The chain extender is prepared by the following steps:
[0036] S1. Under nitrogen protection, add 1 mol of 2-chloro-4-fluorophenol, 1.2 mol of hydroxystyrene and 0.02 mol of tri(2-methoxyphenyl)phosphine to 100 mL of N-methylpyrrolidone in an ice-water bath, cool to 0°C, then dropwise add 0.015 mol of diisopropyl azodicarboxylate. After the dropwise addition, react at room temperature at a stirring speed of 200 rpm for 1 hour. After the reaction is completed, pour into a saturated sodium bicarbonate solution and let stand for 1 hour, and distill under reduced pressure to obtain an intermediate product.
[0037] S2. Add 1 mol of the intermediate product and 1.1 mol of monoethyl malonate to a mixture of 200 mL of 80% ethanol and 20% sodium hydroxide, heat to 25°C, and react at a stirring speed of 200 rpm for 2 hours. After the reaction is completed, extract with ethyl acetate, collect the organic layer, wash the organic layer with saturated brine, dry the organic layer with anhydrous sodium sulfate, distill under reduced pressure until a precipitate is precipitated, and recrystallize to obtain a chain extender.
[0038] Preparation Example 2
[0039] The chain extender is prepared by the following steps:
[0040] S1. Under nitrogen protection, add 1 mol of 2-chloro-4-fluorophenol, 1.35 mol of hydroxystyrene and 0.03 mol of tri(2-methoxyphenyl)phosphine to 150 mL of N-methylpyrrolidone in an ice-water bath, cool to 0°C, then dropwise add 0.018 mol of diisopropyl azodicarboxylate. After the dropwise addition is completed, react at room temperature at a stirring speed of 400 rpm for 3 h. After the reaction is completed, pour into a saturated sodium bicarbonate solution and let stand for 1.5 h, and distill under reduced pressure to obtain an intermediate product.
[0041] S2. Add 1 mol of the intermediate product and 1.3 mol of monoethyl malonate to a mixture of 250 mL of 90% ethanol and 10% sodium hydroxide, raise the temperature to 35°C, and react at a stirring speed of 400 rpm for 2.5 hours. After the reaction is completed, extract with ethyl acetate, collect the organic layer, wash the organic layer with saturated brine, dry the organic layer with anhydrous sodium sulfate, distill under reduced pressure until a precipitate is precipitated, and recrystallize to obtain a chain extender.
[0042] Preparation Example 3
[0043] The chain extender is prepared by the following steps:
[0044] S1. Under nitrogen protection, add 1 mol 2-chloro-4-fluorophenol, 1.5 mol hydroxystyrene and 0.04 mol tri(2-methoxyphenyl)phosphine to 100 mL N-methylpyrrolidone in an ice water bath, cool to 0°C, then dropwise add 0.02 mol diisopropyl azodicarboxylate. After the dropwise addition, react at room temperature at a stirring speed of 600 rpm for 5 h. After the reaction is completed, pour into a saturated sodium bicarbonate solution and let stand for 2 h, and distill under reduced pressure to obtain an intermediate product.
[0045] S2. Add 1 mol of the intermediate product and 1.5 mol of monoethyl malonate to a mixture of 200 mL of 95% ethanol and 5% sodium hydroxide, raise the temperature to 50°C, and react at a stirring speed of 600 rpm for 3 hours. After the reaction is completed, extract with ethyl acetate, collect the organic layer, wash the organic layer with saturated brine, dry the organic layer with anhydrous sodium sulfate, distill under reduced pressure until a precipitate is precipitated, and recrystallize to obtain a chain extender.
[0046] Example 1
[0047] A preparation process for a raw material of a cosmetic sponge comprises the following steps: weighing 40 parts of polyethylene glycol, 0.002 parts of bis(dimethylaminoethyl)ether (BDMAEE), 0.5 parts of a chain extender obtained in Preparation Example 1, 4 parts of silicone oil, 0.1 parts of palm wax and 0.1 parts of a color paste, adding the mixture into a mixer, and reacting the mixture at a stirring speed of 500 rpm for 1 hour to obtain a component A mixture; adding 30 parts of diphenylmethane diisocyanate, 0.001 parts of an antioxidant 1010 and chitosan in total, and 2 parts of talc into the mixer, and stirring the mixture at a speed of 2000 rpm for 10 minutes to obtain a component B mixture.
[0048] When used, a cosmetic sponge comprising the above raw materials is prepared by the following steps:
[0049] Add the mixed materials of component A and component B into a mixer, stir at a speed of 1000 rpm for 10 minutes, heat to 80° C. and solidify for 10 minutes to obtain a finished cosmetic sponge.
[0050] Example 2
[0051] A raw material for a cosmetic sponge: 45 parts of polypropylene glycol, 0.006 parts of bis(dimethylaminoethyl)ether (BDMAEE), 0.6 parts of a chain extender obtained in Preparation Example 2, 5 parts of silicone oil, 0.5 parts of sugarcane wax and 1.5 parts of a color paste are added into a mixer, and reacted at a stirring speed of 500 rpm for 1 hour to obtain a component A mixture; 35 parts of diphenylmethane diisocyanate, 0.003 parts of an antioxidant 1076 and chitosan in total, and 2 parts of talc are added into a mixer, and stirred at a speed of 2000 rpm for 10 minutes to obtain a component B mixture.
[0052] When used, a cosmetic sponge comprising the above raw materials is prepared by the following steps:
[0053] Add the mixed materials of component A and component B into a mixer, stir at a speed of 1000 rpm for 10 minutes, heat to 80° C. and solidify for 10 minutes to obtain a finished cosmetic sponge.
[0054] Example 3
[0055] A raw material for a cosmetic sponge is provided. 47 parts of polypropylene glycol, 0.008 parts of bis(dimethylaminoethyl)ether (BDMAEE), 0.6 parts of a chain extender obtained in Preparation Example 2, 4.5 parts of silicone oil, 0.45 parts of beeswax and 2 parts of a color paste are added into a mixer, and the mixture is reacted at a stirring speed of 500 rpm for 1 hour to obtain a component A mixture. 37 parts of diphenylmethane diisocyanate, 0.0025 parts of an antioxidant 1076 and phenolic acid in total, and 2.5 parts of talc are added into the mixer, and the mixture is stirred at a speed of 2500 rpm for 15 minutes to obtain a component B mixture.
[0056] When used, a cosmetic sponge comprising the above raw materials is prepared by the following steps:
[0057] Add the mixed materials of component A and component B into a mixer, stir at a speed of 1000 rpm for 10 minutes, heat to 80° C. and solidify for 10 minutes to obtain a finished cosmetic sponge.
[0058] Example 4
[0059] A raw material for a cosmetic sponge: 48 parts of polypropylene glycol, 0.009 parts of bis(2-dimethylaminoethyl) ether, 0.8 parts of a chain extender obtained in Preparation Example 3, 5 parts of silicone oil, 0.8 parts of rice bran wax and 2.5 parts of a color paste are added into a mixer, and reacted at a stirring speed of 600 rpm for 1 hour to obtain a component A mixture; 35 parts of diphenylmethane diisocyanate, 0.004 parts of an antioxidant 1076 and anthocyanin in total, and 3 parts of talc are added into the mixer, and stirred at a speed of 2500 rpm for 15 minutes to obtain a component B mixture.
[0060] When used, a cosmetic sponge comprising the above raw materials is prepared by the following steps:
[0061] Add the mixed materials of component A and component B into a mixer, stir at a speed of 1000 rpm for 10 minutes, heat to 80° C. and solidify for 10 minutes to obtain a finished cosmetic sponge.
[0062] Example 5
[0063] A raw material for a cosmetic sponge comprises, by weight: 50 parts of polytetramethylene glycol, 0.01 parts of N,N-dimethylcyclohexylamine, 0.8 parts of a chain extender obtained in Preparation Example 3, 6 parts of silicone oil, 1 part of insect wax and 3 parts of color paste are added into a mixer, and reacted at a stirring speed of 1000 rpm for 2 hours to obtain a component A mixture; 40 parts of diphenylmethane diisocyanate, 0.005 parts of an antioxidant 1010 and anthocyanin in total, and 3 parts of talcum powder are added into the mixer, and stirred at a speed of 3000 rpm for 20 minutes to obtain a component B mixture.
[0064] When used, a cosmetic sponge comprising the above raw materials is prepared by the following steps:
[0065] Add the mixed materials of component A and component B into a mixer, stir at a speed of 1000 rpm for 10 minutes, heat to 80° C. and solidify for 10 minutes to obtain a finished cosmetic sponge.
[0066] Comparative Example 1
[0067] The difference between this comparative example and Example 1 is that no chain extender is added, and the remaining steps are the same as those of Example 1.
[0068] Comparative Example 2
[0069] The difference between this comparative example and Example 2 is that the intermediate product prepared in Preparation Example 2 is used instead of the chain extender, and the remaining steps are the same as those in Example 2.
[0070] Comparative Example 3
[0071] The difference between this comparative example and Example 3 is that 2-chloro-4-fluorophenol is used instead of the chain extender, and the remaining steps are the same as those in Example 3.
[0072] Comparative Example 4
[0073] The difference between this comparative example and Example 4 is that hydroxystyrene is used instead of the chain extender, and the remaining steps are the same as those of Example 4.
[0074] Comparative Example 5
[0075] The difference between this comparative example and Example 5 is that monoethyl malonate is used instead of the chain extender, and the remaining steps are the same as those in Example 5.
[0076] The sponge samples prepared in Examples 1-5 and Comparative Examples 1-5 were cut into cubes with a side length of 1 cm, with 3 replicates in each group. 0.1 ml of foundation liquid (mainly composed of vaseline, liquid paraffin, silicone oil, ethanol, glycerin and water, etc.) was dripped onto each sponge cube using a micropipette. The penetration of the foundation on the sponge surface was observed under a microscope, and the time required for the foundation to fully penetrate was recorded. All sponge cubes were washed 5 times with deionized water and dried to constant weight, and then weighed to calculate the residual amount of foundation liquid, which was equal to the initial sponge cube mass minus the sponge cube mass after drying. The average value was taken, and the results are shown in Table 1:
[0077] Table 1. Permeability test results of each sample
[0078] serial number Complete penetration time (s) Residue(mg) Example 1 8.2 0.003 Example 2 8.6 0.002 Example 3 8.2 0.003 Example 4 8.4 0.003 Example 5 8.5 0.003 Comparative Example 1 3.3 0.012 Comparative Example 2 4.5 0.010 Comparative Example 3 4.6 0.009 Comparative Example 4 4.3 0.011 Comparative Example 5 4.9 0.011
[0079] With reference to GB / T 20467-2006 "Compression performance test of finished products of molded and extruded sponge rubber products of soft foam polymer materials", sponge samples obtained in Examples 1-5 and Comparative Examples 1-5 were prepared, with 3 replicates in each group, and compression tests were performed on the samples using a compression testing machine. The compression speed was set to 10% of the original height of the sample per second, the compression amount was set to 50% of the original height of the sample, and the recovery time was set to hold for 5 seconds after compression, and the compression stress and compression permanent deformation of each sample were recorded. In addition, the tensile strength of each sponge was measured using a tensile strength tester, and the maximum tensile force (N) of each sponge before breaking was recorded; the tear strength of each sponge was measured using a tear strength tester, and the maximum force (N) of each sponge when tearing was recorded. The average value was taken, and the results are shown in Table 2:
[0080] Table 2. Physical properties test results of each sample
[0081]
[0082] As shown in Table 1, the penetration time of Examples 1-5 is significantly longer than that of Comparative Examples 1-5, and the residual amount is significantly lower than that of Comparative Examples 1-5. This indicates that the addition of the chain extender effectively reduces the penetration speed and residual amount of cosmetics such as foundation in the sponge. The halogen elements and hydroxyl groups in the chain extender may work together to reduce the porosity of the cosmetic sponge, forming an internal structure that is more difficult for cosmetics to penetrate, thereby reducing the penetration and residual of cosmetics.
[0083] As shown in Table 2, the compressive stress of Examples 1-5 is significantly higher than that of Comparative Examples 1-5, and the compression permanent deformation is lower. This indicates that the addition of the chain extender enhances the compressive resistance and shape recovery ability of the sponge. The chain extender enhances the interaction between the polyurethane molecular chains to form a more dense and uniform network structure, thereby improving the mechanical properties of the sponge.
[0084] The tensile strength and tear strength of Examples 1-5 are higher than those of Comparative Examples 1-5, indicating the enhancing effect of the chain extender on the mechanical properties of the sponge. The chain extender extends the length of the polyurethane chain, increases the molecular weight, and makes the molecular structure of the sponge more complex and stable, thereby improving its tensile and tear strength.
[0085] In summary, the addition of chain extenders significantly improves the physical properties and makeup effects of cosmetic sponges by changing the structure and properties of polyurethane molecular chains. By using the above-mentioned raw materials for cosmetic sponges, cosmetic sponges are made more durable, less prone to deformation, and can better carry and release cosmetics, thereby improving the quality and durability of makeup.
[0086] In the description of the specification, the description with reference to the terms "preparation example", "embodiment", "various embodiments" and the like means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or preparation example are included in at least one embodiment or preparation example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or preparation example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or preparation examples in a suitable manner.
[0087] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A cosmetic sponge raw material, characterized in that: The components include, by weight: component A and component B, component A includes, by weight: 40-50 parts of polyether polyol, 0.1-1 parts of slow rebound release agent, 0.002-0.01 parts of catalyst, 0.5-0.8 parts of chain extender, 4-6 parts of silicone oil and 0.1-3 parts of color paste; component B includes, by weight: 30-40 parts of diphenylmethane diisocyanate, 0.001-0.005 parts of additives and 2-3 parts of talc; The structural formula of the chain extender is formula (I):
2. A cosmetic sponge raw material according to claim 1, characterized in that: The polyether polyol is one or more of polyethylene glycol, polypropylene glycol and polytetramethylene glycol.
3. A cosmetic sponge raw material according to claim 1, characterized in that: The additives include antioxidants and antimicrobial agents, wherein the antioxidant includes one of antioxidant 1010 and antioxidant 1076, and the antimicrobial agent includes one of chitosan, phenolic acid and anthocyanin; the catalyst includes one of bis(dimethylaminoethyl) ether, N,N-dimethylcyclohexylamine and bis(2-dimethylaminoethyl) ether.
4. A cosmetic sponge raw material according to claim 1, characterized in that: The slow-rebound release agent includes one or more of palm wax, rice bran wax, sugarcane wax, beeswax, insect white wax and polyethylene wax.
5. A cosmetic sponge raw material according to claim 1, characterized in that: The chain extender is prepared by the following steps: S1. Under nitrogen protection, add 2-chloro-4-fluorophenol, hydroxystyrene and tri(2-methoxyphenyl)phosphine to N-methylpyrrolidone in an ice-water bath, cool to 0°C, then dropwise add diisopropyl azodicarboxylate, stir and react at room temperature after the addition is complete, pour into a saturated sodium bicarbonate solution and let stand for 1-2 hours, and distill under reduced pressure to obtain an intermediate product; S2. Add the intermediate product and monoethyl malonate to a mixture of ethanol and alkali, heat and stir, and after the reaction is completed, purify the product to obtain a chain extender.
6. A cosmetic sponge raw material according to claim 5, characterized in that: In step S1, the molar ratio of 2-chloro-4-fluorophenol, hydroxystyrene, tri(2-methoxyphenyl)phosphine and diisopropyl azodicarboxylate is 1:(1.2-1.5):(0.02-0.04):(0.015-0.02).
7. A cosmetic sponge raw material according to claim 5, characterized in that: In step S1, the stirring speed is 200-600 rpm, and the reaction time is 1-5 h.
8. The cosmetic sponge raw material according to claim 5, characterized in that: In step S2, the molar ratio of the intermediate product to monoethyl malonate is 1:(1.1-1.5), and in the mixed solution of ethanol and alkali, the mass percentage of alkali is 5-20%, and the alkali is sodium hydroxide or potassium hydroxide.
9. A cosmetic sponge raw material according to claim 5, characterized in that: In step S2, the reaction temperature is 25-50° C., the stirring speed is 200-600 rpm, and the reaction time is 2-3 h.
10. The process for preparing the cosmetic sponge raw material according to any one of claims 1 to 9, characterized in that: The following steps are involved: Component A: 40-50 parts of polyether polyol, 0.1-1 part of slow rebound release agent, 0.002-0.01 part of catalyst, 0.5-0.8 part of chain extender, 4-6 parts of silicone oil and 0.1-3 parts of color paste are weighed by weight and added into a mixer, and reacted at a stirring speed of 500-1000 rpm for 1-2 hours to obtain a mixture of component A; Component B: 30-40 parts of diphenylmethane diisocyanate, 0.001-0.005 parts of additives and 2-3 parts of talc are weighed by weight and added into a mixer, and stirred at a speed of 2000-3000 rpm for 10-20 minutes to obtain a component B mixture.