Normal-temperature curing high-temperature-resistant epoxy resin adhesive and preparation method thereof

By reacting the modified amine with the epoxy resin to form a modified curing agent, combined with vacuum stirring and filtration technology, the problem of insufficient bonding strength and thermal stability of the epoxy resin adhesive when curing at room temperature is solved, and high temperature stability is achieved The improvement of properties and bonding properties has expanded the scope of application and reduced production costs.

CN118978886APending Publication Date: 2024-11-19HUIZHOU SHENGSHIDA TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411012719.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

At this stage, epoxy resin adhesives have problems such as low bond strength, large internal stress and poor heat resistance when curing at room temperature, which limits their application scope. Moreover, the thermal stability of polythiol-type curing agents is poor, and amine-based curing The high cross-linking density of the agent at high temperature leads to cracking, making it difficult to take into account the advantages of room temperature curing and thermal stability.

Method used

By mixing component A and component B in a ratio of 100:100-100:60, component A includes epoxy resin, modified epoxy resin, diluent, leveling agent, defoaming agent and dispersing agent, group Part B includes a modified curing agent, accelerator and coupling agent, which is prepared by vacuum stirring and filtration processes. The modified amine reacts with an epoxy resin to form a modified curing agent, which improves the structure and thermal stability of the curing agent.

Benefits of technology

The high temperature stability and bonding performance of epoxy resin adhesives have been improved, and cracking problems caused by low bonding strength and large internal stress have been avoided. The scope of application of adhesives has been expanded, while reducing production costs. Large-scale production conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004964852990000121
    Figure BDA0004964852990000121
Patent Text Reader

Abstract

The invention discloses a high-temperature-resistant epoxy resin adhesive and a preparation method thereof.The high-temperature-resistant epoxy resin adhesive comprises a component A and a component B. The main component of the component A is epoxy resin, the main component of the component B is a modified curing agent, and the high-temperature-resistant epoxy resin adhesive is prepared by diluting a modified amine compound and the epoxy resin, so that the product has the normal-temperature curing characteristic and the heat-resistant advantage; the modified curing agent is added, so that the viscosity of the product is increased, the adhesive property is stronger, the thermal stability of the product is improved, the cracking phenomenon of the product at high temperature is avoided, and the epoxy resin adhesive has a relatively good application value for improving the performance of the epoxy resin adhesive.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of adhesives, in particular to a room temperature curing high temperature resistant epoxy resin adhesive and a preparation method thereof. Background Art

[0002] Epoxy resin is a high molecular polymer containing two or more epoxy groups. It can cross-link with curing agent to form a three-dimensional network structure, stably wrapping the skeletal structure of the composite material in the network structure. The epoxy resin and curing agent are combined in proportion to form an adhesive. The resulting epoxy resin adhesive has stable chemical properties, acid and alkali resistance, corrosion resistance, high bonding strength and electrical insulation. It is widely used in construction, machinery, electronics and electrical, and aerospace fields.

[0003] The curing system of epoxy resin usually uses bisphenol A epoxy resin or bisphenol F epoxy resin to react with amines, anhydride curing agents, synthetic resin curing agents or latent curing agents. The curing conditions of different curing agents are different. For example, anhydride curing agents need to be baked at high temperature to completely cure, and the production cost is relatively high. Amines and polythiol curing agents can complete curing at room temperature, which reduces production costs and improves production efficiency. Therefore, they are widely used and are commercially called "universal glue."

[0004] The structure of the curing agent plays a decisive role in the thermal stability of the adhesive product. Polythiol curing agents have poor thermal stability and are not suitable for high-temperature environments. The epoxy resin obtained by curing the common amine curing agents on the market at room temperature has a high cross-linking density and large internal stress, which will cause cracking due to excessive brittleness, low bonding strength, and poor heat resistance. This limits the scope of application of room-temperature curing epoxy resins. How to retain the advantages of room-temperature curing while improving the product's bonding performance and thermal stability is a technical problem in the development of epoxy resin adhesives at this stage. Summary of the invention

[0005] In order to solve the above problems, the present invention provides a room temperature curing high temperature resistant epoxy resin adhesive and a preparation method thereof, which is achieved by the following technical solutions:

[0006] A high temperature resistant epoxy resin adhesive, which is composed of component A and component B mixed in a weight ratio of 100:100-100:60, and can be cured at room temperature, wherein:

[0007] The raw materials for preparing component A include, by weight, 30-60 parts of epoxy resin, 20-50 parts of modified epoxy resin, 5-10 parts of diluent, 0.5-4 parts of leveling agent, 0.5-4 parts of defoaming agent, and 0.5-4 parts of dispersant;

[0008] Preferably, the epoxy resin includes one or more of bisphenol A epoxy resin (NPEL-128, NPEL-127, NPEL-134, GY-250), bisphenol F epoxy resin (NPEF-170, GY-281), and bisphenol S epoxy resin;

[0009] Preferably, the modified epoxy resin includes one or more of phenolic epoxy resin (NPPN-631, NPPN-638, EPALLOY8240, NPPN-701, NPPN-702), silicone-modified epoxy resin, multifunctional epoxy resin (MY-720, MY-721, TACTIX742), polyimide resin, bismaleic anhydride epoxy resin, and 4.4-diaminodiphenylmethane tetraglycidylamine;

[0010] Preferably, the diluent includes one or more of benzyl glycidyl ether, phenyl glycidyl ether, allyl glycidyl ether (AGE), polypropylene glycol diglycidyl ether (207), neodecanoic acid glycidyl ether (810), and benzyl glycidyl ether (692);

[0011] Preferably, the leveling agent is an acrylate leveling agent;

[0012] Preferably, the defoaming agent includes one or more of BYK-052, BYK-057, and BYK-066;

[0013] Preferably, the dispersant includes one or more of BYK-W903, BYK-109, and BYK-110;

[0014] The raw materials for preparing component B include 85-95 parts of modified curing agent, 1-12 parts of accelerator, and 0.5-3 parts of coupling agent in parts by weight;

[0015] Preferably, the modified curing agent includes one or more of the amine compounds 4,4-diaminodiphenylmethane (DDM), 4,4-diaminodiphenyl sulfone (DDS), 1,6-hexanediamine (HMDA), 1,4-cyclohexanedicarboxylic acid (CHDA), isophoronediamine (IPDA), triethanolamine, and diethylenetriamine;

[0016] Preferably, the modified curing agent comprises epoxy resin: one or more of bisphenol A epoxy resin (NPEL-128, NPEL-127, NPEL-134, GY-250), bisphenol F epoxy resin (NPEF-170, GY-281), and bisphenol S epoxy resin;

[0017] Preferably, the diluent includes one or more of benzyl glycidyl ether, phenyl glycidyl ether, allyl glycidyl ether (AGE), polypropylene glycol diglycidyl ether (207), neodecanoic acid glycidyl ether (810), and benzyl glycidyl ether (692);

[0018] Preferably, the accelerator includes one or more of DMP-30, BC-120, and triphenylphosphonium bromide;

[0019] Preferably, the coupling agent includes one or more of KH-550, KH-560, and KH-570;

[0020] Further, a method for preparing a high temperature resistant epoxy resin adhesive is as follows:

[0021] Add the raw materials of component A into the vacuum mixer according to the weight ratio;

[0022] Preferably, the stirring parameters are revolution speed 2000-2500 rpm, dispersion disk speed 2500-3000 rpm, and stirring time 15-20 minutes;

[0023] The stirring revolution speed was adjusted to 1000-1500 rpm, and vacuum was applied for 1 hour while stirring. The obtained product was filtered through a 325-mesh sieve and packaged to obtain component A.

[0024] Add the raw materials of component B into the vacuum mixer according to the weight ratio;

[0025] Preferably, the stirring parameters are revolution speed 2000-2500 rpm, dispersion disk speed 2500-3000 rpm, and stirring time 15-20 minutes;

[0026] The stirring revolution speed was adjusted to 1000-1500 rpm, and vacuum was applied for 1 hour while stirring. The obtained product was filtered and packaged using a 325-mesh screen of a filter press to obtain component B.

[0027] Among them, the preparation method of the modified curing agent of component B is to stir the amine compound and the epoxy resin in proportion at 90-120°C for 3 hours and then cool to room temperature, add the diluent to the resulting product in a mass ratio of modified amine: epoxy resin: diluent = 100:10-30:5-20, stir for 1 hour, and cool to room temperature to obtain the modified curing agent.

[0028] Preferably, the weight ratio of the amine compound to the epoxy resin is 100:10-100:30, and the preferred ratio is 100:15-100:25.

[0029] Compared with the prior art, the beneficial effect of this solution is that the modified amine used is a condensation of aliphatic amines, aromatic amines and alicyclic amines. The modified curing agent is synthesized by the modified amine and epoxy resin. The active groups of the epoxy resin and the modified amine react to improve the structure of the curing agent, so that the curing agent has both the room temperature curing characteristics of aliphatic amines and the high temperature resistance advantages of aromatic amines and alicyclic amines. The thermal stability of epoxy resin adhesives is improved. The modified curing agent provided by this solution can avoid the problems of low bonding strength, cracking caused by large internal stress, poor heat resistance, etc. in the adhesive. At the same time, it can also increase the proportion of epoxy resin in the adhesive, and the molecular structure of the cured adhesive is more stable. The scope of application of epoxy resin adhesives has been expanded. At the same time, the production process of this product is simple, the commercialization of raw materials is mature, the production cost is low, the practicability is strong, and the conditions for large-scale production are met. DETAILED DESCRIPTION

[0030] The following examples are used to illustrate the present invention, but are not intended to limit the scope of the present invention. Without departing from the spirit and essence of the present invention, modifications or substitutions made to the methods, steps or conditions of the present invention all belong to the scope of protection of the present invention. Unless otherwise specified, the experimental materials, reagents, instruments, etc. used in the examples of the present invention are all commercially available; unless otherwise specified, all technical means in the examples of the present invention are conventional means well known to those skilled in the art.

[0031] In order to enable those skilled in the art to better understand the technical solution of the present invention, the product of the present invention is further described in detail below in conjunction with embodiments.

[0032] The raw materials for preparing component A include, by weight, 30-60 parts of epoxy resin, 20-50 parts of modified epoxy resin, 5-10 parts of diluent, 0.5-4 parts of leveling agent, 0.5-4 parts of defoaming agent, and 0.5-4 parts of dispersant;

[0033] The raw materials for preparing component B include 85-95 parts of modified curing agent, 1-12 parts of accelerator, and 0.5-3 parts of coupling agent by weight. The raw materials of the modified curing agent are modified amine and epoxy resin.

[0034] The more epoxy groups an epoxy resin has, the higher the epoxy value of the epoxy resin, the longer the curing time, the higher the degree of crosslinking after curing, the greater the strength, resulting in greater brittleness and poor high temperature resistance. Therefore, a curing agent is usually used to improve the structure of the epoxy resin. Although a single fatty amine can also be used as a curing agent for epoxy resins, it can be cured at room temperature and the curing speed is relatively fast, but the epoxy resin cured by fatty amines has poor heat resistance and will crack under high temperature conditions, which is not conducive to the application of epoxy resins. By modifying fatty amines and introducing aromatic amines, alicyclic amines, etc. to improve the thermal stability of the modified amines, epoxy resins with high epoxy values ​​can still maintain a stable crosslinked structure under high temperature conditions and also maintain the characteristics of curing at room temperature.

[0035] The raw materials of component A and component B are added into a vacuum mixer respectively, and the stirring parameters are revolution speed 2000-2500 rpm, dispersion disk speed 2500-3000 rpm, and stirring time 15-20 minutes; the stirring revolution speed is adjusted to 1000-1500 rpm, and vacuum is drawn for 1 hour while stirring. The obtained product is filtered through a 325 mesh sieve to obtain component A and component B respectively.

[0036] The preparation method of the modified curing agent is as follows: the modified amine and epoxy resin are stirred at 90-120°C for 3 hours in proportion, and then cooled to room temperature; 5-20 parts of diluent are added to the obtained product, stirred for 1 hour, and cooled to room temperature to obtain the modified curing agent.

[0037] Component A and component B are uniformly mixed in a mass ratio of 100:100-100:60 to obtain an adhesive.

[0038] The modified curing agent is composed of modified amine and epoxy resin. A small amount of epoxy resin reacts more fully with the active groups of the modified amine. The mixture of AB components can better integrate the epoxy resin and the modified curing agent. At the same time, it increases the proportion of epoxy resin in the adhesive, so that the cross-linking strength of the cured adhesive is higher but the brittleness is not too large and it is not easy to crack.

[0039] Example 1

[0040] The raw materials of component A include bisphenol A epoxy resin 128: 45 parts, novolac epoxy resin NPES-638: 44.9 parts, epoxy diluent AGE: 8 parts, leveling agent 495: 0.5 parts, defoamer BYK-066: 0.6 parts, dispersant 110: 1 parts;

[0041] The raw materials of component B include 88 parts of modified curing agent 1, 10 parts of accelerator DMP-30, and 2 parts of coupling agent KH-550;

[0042] The raw materials of the modified curing agent 1 include: 1,4-cyclohexanedicarboxylic acid, bisphenol A epoxy resin 128, and diluent 810;

[0043] The raw materials of component A are added into a vacuum mixer according to the weight ratio. The stirring parameters are revolution speed of 2000-2500 rpm, dispersion disk speed of 2500-3000 rpm, and stirring time of 15-20 minutes. The stirring revolution speed is adjusted to 1000-1500 rpm, and vacuum is drawn for 1 hour while stirring. The obtained product is filtered through a 325 mesh sieve to obtain component A.

[0044] 1,4-cyclohexanedicarboxylic acid and epoxy resin were added into a mixer in a weight ratio of 100:20, stirred at 90-120° C. for 3 hours, and then cooled to room temperature. 15 parts of diluent were added to the obtained product, stirred for 1 hour, and cooled to room temperature to obtain modified curing agent 1.

[0045] The raw materials for component B are added into a vacuum mixer according to the weight ratio. The stirring parameters are revolution speed of 2000-2500 rpm, dispersion disk speed of 2500-3000 rpm, and stirring time of 15-20 minutes. The stirring revolution speed is adjusted to 1000-1500 rpm, and vacuum is drawn for 1 hour while stirring. The obtained product is filtered through a 325-mesh sieve to obtain component B.

[0046] Component A and component B were mixed in a mass ratio of 100:100 to form an adhesive, which was cured at room temperature for 24 hours.

[0047] Example 2

[0048] The raw materials of component A include 170: 55 parts of bisphenol F epoxy resin, 34.9 parts of organosilicon modified epoxy resin ES-3201, 8 parts of epoxy diluent AGE, 0.5 parts of leveling agent 495, 0.6 parts of defoaming agent BYK-066, and 110: 1 part of dispersant;

[0049] The raw materials of component B include modified curing agent 1: 92 parts, accelerator DMP-30: 6 parts, coupling agent KH-550: 2 parts;

[0050] The raw materials of the modified curing agent 1 include: 1,4-cyclohexanedicarboxylic acid, bisphenol A epoxy resin 128, and diluent 810;

[0051] The raw materials of component A are added into a vacuum mixer according to the weight ratio. The stirring parameters are revolution speed of 2000-2500 rpm, dispersion disk speed of 2500-3000 rpm, and stirring time of 15-20 minutes. The stirring revolution speed is adjusted to 1000-1500 rpm, and vacuum is drawn for 1 hour while stirring. The obtained product is filtered through a 325 mesh sieve to obtain component A.

[0052] 1,4-cyclohexanedicarboxylic acid and epoxy resin were added into a mixer in a weight ratio of 100:20, stirred at 90-120° C. for 3 hours, and then cooled to room temperature. 15 parts of diluent were added to the obtained product, stirred for 1 hour, and cooled to room temperature to obtain modified curing agent 1.

[0053] The raw materials for component B are added into a vacuum mixer according to the weight ratio. The stirring parameters are revolution speed of 2000-2500 rpm, dispersion disk speed of 2500-3000 rpm, and stirring time of 15-20 minutes. The stirring revolution speed is adjusted to 1000-1500 rpm, and vacuum is drawn for 1 hour while stirring. The obtained product is filtered through a 325-mesh sieve to obtain component B.

[0054] Component A and component B were mixed in a mass ratio of 100:80 to form an adhesive, which was cured at room temperature for 24 hours.

[0055] Example 3

[0056] The raw materials of component A include 128:50 parts of bisphenol A epoxy resin, 39.9 parts of organosilicon modified epoxy resin ES-3201, 8 parts of epoxy diluent AGE, 0.5 parts of leveling agent 495, 0.6 parts of defoaming agent BYK-066, and 110:1 parts of dispersant;

[0057] The raw materials of component B include modified curing agent 2: 88 parts, accelerator DMP-30: 10 parts, coupling agent KH-550: 2 parts;

[0058] The raw materials of modified curing agent 2 include: isophorone diamine, bisphenol F epoxy resin 128, and diluent 207;

[0059] The raw materials of component A are added into a vacuum mixer according to the weight ratio. The stirring parameters are revolution speed of 2000-2500 rpm, dispersion disk speed of 2500-3000 rpm, and stirring time of 15-20 minutes. The stirring revolution speed is adjusted to 1000-1500 rpm, and vacuum is drawn for 1 hour while stirring. The obtained product is filtered through a 325 mesh sieve to obtain component A.

[0060] Isophorone diamine and epoxy resin were added to a mixer in a weight ratio of 100:15, stirred at 90-120° C. for 3 hours, and then cooled to room temperature. 10 parts of a diluent were added to the resulting product, stirred for 1 hour, and cooled to room temperature to obtain a modified curing agent 2.

[0061] The raw materials for component B are added into a vacuum mixer according to the weight ratio. The stirring parameters are revolution speed of 2000-2500 rpm, dispersion disk speed of 2500-3000 rpm, and stirring time of 15-20 minutes. The stirring revolution speed is adjusted to 1000-1500 rpm, and vacuum is drawn for 1 hour while stirring. The obtained product is filtered through a 325-mesh sieve to obtain component B.

[0062] Component A and component B were mixed in a mass ratio of 100:90 to form an adhesive, which was cured at room temperature for 24 hours.

[0063] Example 4

[0064] The raw materials of component A include 128:55 parts of bisphenol F epoxy resin, 34.9 parts of phenolic epoxy resin NPES-638, 8 parts of epoxy diluent AGE, 0.5 parts of leveling agent 495, 0.6 parts of defoaming agent BYK-066, and 110:1 parts of dispersant;

[0065] The raw materials of component B include modified curing agent 2: 92 parts, accelerator DMP-30: 6 parts, coupling agent KH-550: 2 parts;

[0066] The raw materials of modified curing agent 2 include: isophorone diamine, bisphenol F epoxy resin 128, and diluent 207;

[0067] The raw materials of component A are added into a vacuum mixer according to the weight ratio. The stirring parameters are revolution speed of 2000-2500 rpm, dispersion disk speed of 2500-3000 rpm, and stirring time of 15-20 minutes. The stirring revolution speed is adjusted to 1000-1500 rpm, and vacuum is drawn for 1 hour while stirring. The obtained product is filtered through a 325 mesh sieve to obtain component A.

[0068] Isophorone diamine and epoxy resin were added to a mixer in a weight ratio of 100:15, stirred at 90-120° C. for 3 hours, and then cooled to room temperature. 10 parts of a diluent were added to the resulting product, stirred for 1 hour, and cooled to room temperature to obtain a modified curing agent 2.

[0069] The raw materials for component B are added into a vacuum mixer according to the weight ratio. The stirring parameters are revolution speed of 2000-2500 rpm, dispersion disk speed of 2500-3000 rpm, and stirring time of 15-20 minutes. The stirring revolution speed is adjusted to 1000-1500 rpm, and vacuum is drawn for 1 hour while stirring. The obtained product is filtered through a 325-mesh sieve to obtain component B.

[0070] Component A and component B were mixed in a mass ratio of 100:65 to form an adhesive, which was cured at room temperature for 24 hours.

[0071] Comparative Example 1

[0072] The raw materials of component A include bisphenol A epoxy resin 128: 45 parts, novolac epoxy resin NPES-638: 44.9 parts, epoxy diluent AGE: 8 parts, leveling agent 495: 0.5 parts, defoamer BYK-066: 0.6 parts, dispersant 110: 1 parts;

[0073] The raw materials of component B include 128:88 parts of bisphenol A epoxy resin, 10 parts of accelerator DMP-30, and 2 parts of coupling agent KH-550;

[0074] The raw materials of component A are added into a vacuum mixer according to the weight ratio. The stirring parameters are revolution speed of 2000-2500 rpm, dispersion disk speed of 2500-3000 rpm, and stirring time of 15-20 minutes. The stirring revolution speed is adjusted to 1000-1500 rpm, and vacuum is drawn for 1 hour while stirring. The obtained product is filtered through a 325 mesh sieve to obtain component A.

[0075] The raw materials for component B are added into a vacuum mixer according to the weight ratio. The stirring parameters are revolution speed of 2000-2500 rpm, dispersion disk speed of 2500-3000 rpm, and stirring time of 15-20 minutes. The stirring revolution speed is adjusted to 1000-1500 rpm, and vacuum is drawn for 1 hour while stirring. The obtained product is filtered through a 325-mesh sieve to obtain component B.

[0076] Component A and component B were mixed in a mass ratio of 100:100 to form an adhesive, which was cured at room temperature for 24 hours.

[0077] Comparative Example 2

[0078] The raw materials of component A include bisphenol A epoxy resin 128: 45 parts, novolac epoxy resin NPES-638: 44.9 parts, epoxy diluent AGE: 8 parts, leveling agent 495: 0.5 parts, defoamer BYK-066: 0.6 parts, dispersant 110: 1 parts;

[0079] The raw materials of component B include 1,4-cyclohexanedicarboxylic acid: 88 parts, accelerator DMP-30: 10 parts, coupling agent KH-550: 2 parts;

[0080] The raw materials of component A are added into a vacuum mixer according to the weight ratio. The stirring parameters are revolution speed of 2000-2500 rpm, dispersion disk speed of 2500-3000 rpm, and stirring time of 15-20 minutes. The stirring revolution speed is adjusted to 1000-1500 rpm, and vacuum is drawn for 1 hour while stirring. The obtained product is filtered through a 325 mesh sieve to obtain component A.

[0081] The raw materials for component B are added into a vacuum mixer according to the weight ratio. The stirring parameters are revolution speed of 2000-2500 rpm, dispersion disk speed of 2500-3000 rpm, and stirring time of 15-20 minutes. The stirring revolution speed is adjusted to 1000-1500 rpm, and vacuum is drawn for 1 hour while stirring. The obtained product is filtered through a 325-mesh sieve to obtain component B.

[0082] Component A and component B were mixed in a mass ratio of 100:100 to form an adhesive, which was cured at room temperature for 24 hours.

[0083] Experimental example

[0084] The performance of the products of the embodiments and comparative examples was tested, including the viscosity and Shore hardness of components A and B. The test results are shown in the following table:

[0085]

[0086] By comparing the test results of Examples 1-4 and Comparative Example 1, it is shown that adding modified amines to component B can greatly increase the viscosity and better the bonding performance, and adding modified curing agents can make this product have a higher hardness at room temperature or high temperature (≤180°C) after curing. Comparing the test results of Examples 1-4 and Comparative Example 2, it is shown that improving the curing agent structure with modified amines and epoxy resins can increase the viscosity of the product and the thermal stability after curing, and reduce internal stress. Comparing the test results of Examples 1-2 and Examples 3-4, modified curing agent 1 performs better in enhancing the heat resistance of the product, while modified curing agent 2 is beneficial to enhancing the viscosity of product component B. This scheme improves the structure of the curing agent through modified amines, improves the thermal stability of the epoxy resin adhesive, and makes the product have high temperature resistance, which is a significant improvement over existing products.

[0087] It can be understood that the above embodiments only express the preferred implementation modes of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the patent scope of the present invention. It should be pointed out that, for ordinary technicians in this field, the above technical features can be freely combined without departing from the concept of the present invention, and several deformations and improvements can be made, which all belong to the protection scope of the present invention. Therefore, all equivalent changes and modifications made to the scope of the claims of the present invention should belong to the coverage of the claims of the present invention.

Claims

1. A high temperature resistant epoxy resin adhesive, characterized in that: The epoxy resin adhesive is made by mixing component A and component B and can be cured at room temperature. The raw materials for preparing component A include, by weight, 30-60 parts of epoxy resin, 20-50 parts of modified epoxy resin, 5-10 parts of diluent, 0.5-4 parts of leveling agent, 0.5-4 parts of defoaming agent, and 0.5-4 parts of dispersant; The raw materials for preparing component B include 85-95 parts of modified curing agent, 1-12 parts of accelerator and 0.5-3 parts of coupling agent in parts by weight, wherein the modified curing agent includes modified amine and epoxy resin.

2. A high temperature resistant epoxy resin adhesive according to claim 1, characterized in that: The raw materials of component A are as follows: The epoxy resin includes one or more of bisphenol A epoxy resin, bisphenol F epoxy resin and bisphenol S epoxy resin.

3. The high temperature resistant epoxy resin adhesive according to claim 1, characterized in that: The modified epoxy resin includes one or more of phenolic epoxy resin, silicone modified epoxy resin, multifunctional epoxy resin, polyimide resin, bismaleic anhydride epoxy resin and 4.4-diaminodiphenylmethane tetraglycidylamine.

4. The high temperature resistant epoxy resin adhesive according to claim 1, characterized in that: The diluent includes one or more of benzyl glycidyl ether, phenyl glycidyl ether, allyl glycidyl ether, polypropylene glycol diglycidyl ether, neodecanoic acid glycidyl ether and benzyl glycidyl ether.

5. The high temperature resistant epoxy resin adhesive according to claim 1, characterized in that: The raw materials of component B are as follows: The modified curing agent includes modified amines: one or more of 4,4-diaminodiphenylmethane, 4,4-diaminodiphenyl sulfone, 1,6-hexanediamine, 1,4-cyclohexanedicarboxylic acid, isophoronediamine, triethanolamine, and diethylenetriamine.

6. The high temperature resistant epoxy resin adhesive according to claim 1, characterized in that: The modified curing agent includes epoxy resin: one or more of bisphenol A epoxy resin, bisphenol F epoxy resin and bisphenol S epoxy resin.

7. The high temperature resistant epoxy resin adhesive according to claim 1, characterized in that: The diluent includes one or more of benzyl glycidyl ether, phenyl glycidyl ether, allyl glycidyl ether, polypropylene glycol diglycidyl ether, neodecanoic acid glycidyl ether and benzyl glycidyl ether.

8. A method for preparing a high temperature resistant epoxy resin adhesive according to claim 1, characterized in that: include: The preparation method of component A is to add the raw materials into a vacuum mixer according to the weight ratio, stir, vacuumize and filter to obtain component A; The preparation method of component B is to add the raw materials into a vacuum mixer according to the weight ratio, stir, vacuumize and filter to obtain component B; Component A and component B are mixed in a mass ratio of 100:100-100:60 to obtain a high temperature resistant epoxy resin adhesive.

9. The preparation method according to claim 8, characterized in that: The preparation method of the modified curing agent of component B is as follows: modified amine and epoxy resin are stirred at a mass ratio of 100:10-100:30 at 90-120° C. and then cooled to room temperature, and a diluent is added to the obtained product at a mass ratio of modified amine: epoxy resin: diluent = 100:10-30:5-20, and the mixture is stirred and then cooled to room temperature to obtain a modified curing agent.