Preparation method of nuclear fuel element and nuclear fuel element
Through the combination of cold sintering and pressure-free sintering, the problems of large energy consumption and coarse grains caused by high-temperature sintering in the manufacturing of nuclear fuel components are solved, and the formation of highly dense nuclear fuel components at lower temperatures and short time is achieved, thereby avoiding cracks and other factors. The emergence of defects.
Patent Information
- Application Number
- CN202411071825.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-11-19
AI Technical Summary
In the existing nuclear fuel component manufacturing methods, high-temperature sintering leads to large energy consumption and large grains generated, prone to defects such as cracks, and lacks effective solutions.
By combining cold sintering and pressure-free sintering, the raw material and solvent are mixed, cold sintering and pressure-free sintering are carried out to form a highly dense nuclear fuel element, with the cold sintering temperature of 120-170℃ and the pressure-free sintering temperature of 200. ~1600℃, the total time is shortened to 1.5 to 11 hours.
It effectively shortens the sintering time, reduces the temperature, inhibits the excessive growth of material grains, reduces thermal stress, solves defect problems such as cracks, and forms highly dense nuclear fuel elements.
Smart Images

Figure CN118983117A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing a nuclear fuel element and the nuclear fuel element. Background Art
[0002] As a clean and efficient form of energy, nuclear energy has been increasingly widely used in recent years. Among them, nuclear fuel is one of the key components in a nuclear reactor, and its quality and performance directly affect the safe and reliable operation of the nuclear reactor. Therefore, the research and improvement of nuclear fuel preparation technology has always attracted much attention.
[0003] Generally, the preparation process of nuclear fuel includes uranium prospecting, uranium mining, uranium smelting, uranium conversion, uranium enrichment and nuclear fuel element manufacturing. Among them, the nuclear fuel element manufacturing method is to convert the uranium hexafluoride gas with a uranium-235 content of 3% to 5% produced by uranium enrichment into uranium dioxide solid powder, which is then pressed into pellets and sintered at high temperature to obtain a pellet ceramic body, and then the ceramic pellets are polished and loaded into a cladding to make a fuel rod. The high-temperature sintering temperature is not less than 1750°C and the time is not less than 20 hours. The energy consumption is large, and the fuel rods generated by this manufacturing method have defects such as coarse grains and easy cracks. However, there is no solution yet. Summary of the invention
[0004] The present invention aims to solve the problem of high energy consumption of fuel rods in the prior art that a pellet ceramic body is obtained by high temperature sintering, and the pellet ceramic body is polished and then loaded into a cladding to form a fuel rod. The present invention forms a highly dense nuclear fuel element by combining cold sintering and pressureless sintering.
[0005] The technical method of the present invention is as follows:
[0006] A method for preparing a nuclear fuel element, the method comprising:
[0007] S1, mixing raw materials with solvent to obtain slurry;
[0008] S2, cold sintering the slurry;
[0009] S3. The cold sintered product is subjected to pressureless sintering to obtain a nuclear fuel element.
[0010] The raw material is a uranium-containing raw material or a combination of a uranium-containing raw material and an inorganic material.
[0011] Preferably, the uranium-containing raw material includes any one of UO2, UN, U3Si2, UC, and UCN. The inorganic material includes any one of silicon carbide, carbon nanotubes, graphene, diamond, and aluminum.
[0012] The volume ratio of the uranium-containing raw material to the inorganic material is (1-10):(9-0).
[0013] The particle size of the uranium-containing raw material is 50nm-170μm.
[0014] The silicon carbide is in granular or whisker form, the particle size of the granular silicon carbide is 20nm-5μm; the diameter of the silicon carbide whisker is 20nm-200nm and the length is 5-20μm; the diameter of the carbon nanotube is 5nm-100nm and the length is 1-20μm; the plane diameter of the graphene is 100nm-200μm; the particle size of the diamond is 20nm-10μm; and the particle size of the aluminum is 20nm-10μm.
[0015] The solvent includes any one of water, formic acid and acetic acid.
[0016] The mass ratio of the raw material to the solvent is (70-75):(30-25).
[0017] In the step S2, the cold sintering pressure is 200-500 MPa, the cold sintering temperature is 120-170° C., and the cold sintering time is 30-300 min.
[0018] In the step S3, the pressureless sintering temperature is 200 to 1600° C., and the pressureless sintering time is 1 to 6 hours.
[0019] Furthermore, before step S1, the raw materials, ball milling beads and anhydrous ethanol are ball milled at a rotation speed of 60 to 70 rpm for 22 to 25 hours.
[0020] Specifically, the ball milling beads include zirconia ball milling beads with a diameter of 4 to 6 mm and zirconia ball milling beads with a diameter of 1 to 3 mm.
[0021] The present invention also provides a nuclear fuel element, which is obtained by the preparation method of the nuclear fuel element.
[0022] The beneficial effects of the present invention are:
[0023] (1) The present invention uses cold sintering to dissolve and precipitate raw materials under the action of pressure, temperature and liquid phase, which can fill the gaps between the raw materials. Then, through pressureless sintering, a product with a high degree of densification can be obtained at a lower sintering temperature, ensuring the formation of highly dense nuclear fuel elements.
[0024] (2) In the prior art, nuclear fuel elements are obtained by high-temperature sintering, but the temperature of high-temperature sintering is not less than 1750°C and the time is not less than 20 hours. The present invention effectively shortens the time to within 11 hours and reduces the temperature to below 1600°C by cold sintering and pressureless sintering;
[0025] (3) Since the reaction temperature of cold sintering is low and the reaction time is short, the excessive growth of material grains can be effectively inhibited, resulting in smaller grains. At the same time, low-temperature sintering reduces the thermal stress inside the material, which can effectively solve the problem of defects such as cracks that are prone to occur in pressureless sintering. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 This is a diagram of the U3Si2-Al nuclear fuel element of Example 1 of the present invention. DETAILED DESCRIPTION
[0027] The technical solution of the present invention is described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0028] The present invention provides a method for preparing a nuclear fuel element, the method comprising:
[0029] S1. Mixing raw materials with solvent to obtain slurry.
[0030] The raw material is a uranium-containing raw material or a combination of a uranium-containing raw material and an inorganic material.
[0031] Here, the uranium-containing raw material includes any one of UO2, UN, U3Si2, UC, and UCN. Specifically, the uranium fuel of the present invention has a wide range, and can be not only a high-concentration fuel, but also a low core uranium density and low enrichment uranium fuel. Specifically, it can be a highly enriched uranium fuel UO2, and can also be a core uranium density, low enrichment uranium fuel UN, U3Si2, UC, and UCN.
[0032] Here, the inorganic material includes any one of silicon carbide, carbon nanotube, graphene, diamond, and aluminum. The inorganic material includes one of silicon carbide, carbon nanotube, graphene, diamond, and aluminum.
[0033] Specifically, the present invention improves the thermal conductivity of nuclear fuel elements by introducing inorganic materials.
[0034] In one embodiment, the volume ratio of the uranium-containing raw material to the inorganic material is (1-10):(9-0). For example, the volume ratio of the uranium-containing raw material to the inorganic material is 2:8, the volume ratio of the uranium-containing raw material to the inorganic material is 3:7, and the volume ratio of the uranium-containing raw material to the inorganic material is 8:2.
[0035] In one embodiment, the particle size of the uranium-containing raw material is 50 nm to 170 μm. For example, the particle size of the uranium-containing raw material is 60 nm, 100 μm, or 150 μm.
[0036] In one embodiment, the silicon carbide has a granular or whisker shape. The particle size of the granular silicon carbide is 20nm to 5μm. For example, the particle size of the granular silicon carbide is 50nm, 1μm, and 4μm. The diameter of the silicon carbide whisker is 20nm to 200nm and the length is 5 to 20μm. For example, the diameter of the silicon carbide whisker is 50nm, 100nm, and 150nm, and the length is 6μm, 8μm, and 15μm.
[0037] In one embodiment, the diameter of the carbon nanotube is 5 nm to 100 nm, and the length is 1 to 20 μm. For example, the diameter of the carbon nanotube is 10 nm, 50 nm, or 90 nm, and the length of the carbon nanotube is 5 μm, 10 μm, or 15 μm.
[0038] In one embodiment, the planar diameter of the graphene is 100 nm to 200 μm. For example, the planar diameter of the graphene is 120 nm, 150 nm, or 190 nm.
[0039] In one embodiment, the particle size of the diamond is 20 nm to 10 μm, for example, the particle size of the diamond is 50 nm, 1 μm, or 9 μm.
[0040] In one embodiment, the particle size of aluminum is 20 nm to 10 μm, for example, the particle size of aluminum is 50 nm, 1 μm, or 9 μm.
[0041] The solvent includes any one of water, formic acid and acetic acid. The solvent is added to the raw materials to assist / activate the dissolution, precipitation and nucleation of the raw materials by applying pressure and heat.
[0042] Among them, the mass ratio of raw materials to solvent is (70-75): (30-25).
[0043] Before step S1, the process further includes: milling the raw materials, ball milling beads and anhydrous ethanol at a rotation speed of 60 to 70 rpm for 22 to 25 hours. For example, the rotation speed is 61 rpm, 65 rpm, 69 rpm, and the ball milling time is 23 hours or 24 hours.
[0044] Specifically, when the raw materials are uranium-containing raw materials and inorganic materials, ball milling can mix the uranium-containing raw materials and the inorganic materials evenly.
[0045] Here, the ball milling beads include zirconia ball milling beads with a diameter of 4 to 6 mm and zirconia ball milling beads with a diameter of 1 to 3 mm, and the volume ratio of the zirconia ball milling beads with a diameter of 4 to 6 mm to the zirconia ball milling beads with a diameter of 1 to 3 mm is (3 to 7): (7 to 3). The present invention can better mix the uranium-containing raw material and the inorganic material by using two different specifications of zirconia ball milling beads.
[0046] Here, the ball milling is followed by drying. The drying method may be vacuum drying. The vacuum drying time is 10 to 12 hours. The vacuum drying temperature is 50 to 60°C.
[0047] S2. cold sintering the slurry.
[0048] Specifically, the S2 step is a cold sintering step. The S2 step consists of two stages. The first stage is mainly stress and particle rearrangement, and the second stage is mainly a pressure and temperature assisted solid particle (e.g., raw material) dissolution and precipitation process. In the first stage, densification is driven by uniaxial mechanical force, and the liquid medium (i.e., solvent) can facilitate lubrication between solid particles. In the second stage, the solid particles and the liquid medium are in a high temperature and high pressure environment, which increases the solubility of the solid particles and is conducive to the formation of a supersaturated solution. As the liquid phase gradually evaporates at high temperature, the supersaturation of the solution also increases, and the dissolved solid particles precipitate into nuclei.
[0049] Among them, the cold sintering pressure is 200-500MPa, the cold sintering temperature is 120-170°C, and the cold sintering time is 30-300min. For example, the cold sintering pressure is 200MPa, 300MPa, 400MPa. The cold sintering temperature is 130°C, 140°C, 150°C. The cold sintering time is 40min, 100min, 200min.
[0050] Specifically, the pressure may be applied in the form of uniaxial pressure.
[0051] In one embodiment, step S2 may specifically include: applying a preset pressure to the slurry, heating it to the cold sintering temperature at a preset heating rate, maintaining the cold sintering time, then cooling it to the cold sintering end temperature at a preset cooling rate, and finally cooling it to room temperature.
[0052] Here, after the cold sintering end temperature is reached, the cold sintering ends, so natural cooling is subsequently adopted.
[0053] Among them, the cold sintering end temperature is 50-70°C, the heating rate is 5-8°C / min, and the cooling rate is 3-5°C / min. For example, the cold sintering end temperature is 55°C, 59°C, 65°C. The heating rate is 6°C / min, 7°C / min. The cooling rate is 3.5°C / min, 4°C / min.
[0054] Here, after cooling to room temperature, drying treatment can be performed. The drying treatment can be performed by vacuum drying. The vacuum drying time is 10 to 12 hours. The vacuum drying temperature is 50 to 60°C.
[0055] S3. The cold sintered product is subjected to pressureless sintering to obtain a nuclear fuel element.
[0056] The pressureless sintering temperature is 200-1600°C, and the pressureless sintering time is 1-6 hours. For example, the pressureless sintering temperature is 400°C, 600°C, and 1200°C. The pressureless sintering time is 3 hours, 4 hours, and 5 hours.
[0057] Specifically, cold sintering is to obtain a preliminary formed sample, but the temperature of cold sintering is relatively low, and the density of the sample may not meet the requirements. Therefore, this step of pressureless sintering is required to effectively improve the densification of the nuclear fuel elements.
[0058] Specifically, in step S3, the product can be kept at a pressureless sintering temperature for a pressureless sintering time under an atmosphere protection condition. The atmosphere protection condition requires the introduction of a protective gas, which is one of vacuum, hydrogen, argon, nitrogen, a hydrogen-argon mixture, and a hydrogen-nitrogen mixture.
[0059] The cold sintering time of the present invention is 30-300 minutes, and the pressureless sintering time is 1-6 hours, so the total time is 1.5-11 hours. The cold sintering temperature of the present invention is 120-170°C, and the pressureless sintering temperature is 200-1600°C, so the temperature does not exceed 1600°C.
[0060] In the prior art, nuclear fuel elements are obtained by high temperature sintering, but the temperature of high temperature sintering is not less than 1750°C and the time is not less than 20 hours. The present invention effectively shortens the time to 1.5-11 hours and reduces the temperature to below 1600°C through cold sintering and pressureless sintering.
[0061] The present invention also provides a nuclear fuel element, which is obtained by the above-mentioned method for preparing the nuclear fuel element.
[0062] In order to better understand the present invention, the content of the present invention is further explained below with reference to the accompanying drawings and examples, but the content of the present invention is not limited to the following embodiments.
[0063] Example 1
[0064] Step 1: In the glove box, measure U3Si2 powder and aluminum powder in a volume ratio of 1:9 and add them to a mixing bottle; then add 20% of the volume of the mixing bottle of zirconium oxide ball milling beads: 30% of the ball milling beads with a diameter of 2 mm and 70% of the ball milling beads with a diameter of 5 mm; finally, add 30% of the mass fraction of the mixed powder in anhydrous ethanol and seal the mixing bottle.
[0065] Step 2: Place the mixing bottle on the roller of the rod mill, set the speed to 65 rpm, and the mixing time to 24 hours.
[0066] Step 3: Take the mixed powder in an agate mortar in the glove box, add 30% mass fraction of formic acid, mix and grind thoroughly. Load the slurry into a cylindrical mold with a diameter of 6mm and a sample molding height of 100mm. After vibrating the screen, apply a uniaxial pressure of 350MPa at room temperature. Turn on the digital temperature controller, set the parameters so that the heating jacket is heated to 170℃ at 5℃ / min and kept warm for 30min. After the insulation is completed, cool down to 60℃ at 5℃ / min, and demold the sample after the sample cools naturally to room temperature. Apply a pressure of 350MPa throughout the cold burning process. Then dry the sample in a vacuum drying oven at 60℃ for 12h.
[0067] Step 4: Place the dried cold-sintered sample into a tubular furnace and sinter it at 380°C for 6 hours under argon protection to obtain a U3Si2-Al nuclear fuel rod with a density of 92%. Figure 1 This is a diagram of the U3Si2-Al nuclear fuel rod of this embodiment.
[0068] Example 2
[0069] Step 1: In the glove box, measure UO2 powder and graphene powder in a volume ratio of 9:1 and add them to a mixing bottle. Then add 20% of the volume of the mixing bottle of zirconium oxide ball milling beads: 30% of the ball milling beads with a diameter of 2 mm and 70% of the ball milling beads with a diameter of 5 mm, and seal the mixing bottle.
[0070] Step 2: Place the mixing bottle on the roller of the rod mill, set the speed to 65 rpm, and the mixing time to 24 hours.
[0071] Step 3: Take the mixed powder in an agate mortar in the glove box, add 30% mass fraction of deionized water, mix and grind thoroughly. Load the slurry into a cylindrical mold with a diameter of 6mm and a sample molding height of 100mm. After vibrating the screen, apply a uniaxial pressure of 350MPa at room temperature. Turn on the digital temperature controller, set the parameters so that the heating jacket is heated to 120℃ at 5℃ / min and kept warm for 300min. After the insulation is completed, cool it to 60℃ at 5℃ / min, and demold the sample after the sample cools naturally to room temperature. Apply a pressure of 350MPa throughout the cold burning process. Then dry the sample in a vacuum drying oven at 60℃ for 12h.
[0072] Step 4: Place the dried cold-sintered sample into a tubular furnace and sinter it at 1200°C for 3 hours under hydrogen protection to obtain UO2-graphene nuclear fuel pellets with a density of 94%.
[0073] Example 3
[0074] Step 1: In the glove box, measure UO2 powder and SiC powder in a volume ratio of 9:1 and add them to a mixing bottle. Then add 20% of the volume of the mixing bottle of zirconium oxide ball milling beads: 30% of the ball milling beads with a diameter of 2 mm and 70% of the ball milling beads with a diameter of 5 mm, and seal the mixing bottle.
[0075] Step 2: Place the mixing bottle on the roller of the rod mill, set the speed to 65 rpm, and the mixing time to 24 hours.
[0076] Step: 3: Take the mixed powder in an agate mortar in the glove box, add 30% mass fraction of deionized water to mix and grind thoroughly. Load the slurry into a cylindrical mold with a diameter of 6mm and a sample molding height of 100mm. After vibrating the screen, apply a uniaxial pressure of 350MPa at room temperature. Turn on the digital temperature controller and set the parameters so that the heating jacket is heated to 170℃ at 5℃ / min and kept warm for 60min. After the insulation is completed, cool it to 60℃ at 5℃ / min. After the sample is naturally cooled to room temperature, demold it and take a sample. Continuously apply a pressure of 350MPa during the entire cold burning process. Then dry the sample in a vacuum drying oven at 60℃ for 12h.
[0077] Step 4: Place the dried cold-sintered sample into a tubular furnace and sinter it at 1300°C for 3 hours under the protection of a hydrogen-argon mixed gas to obtain a UO2-SiC nuclear fuel pellet with a density of 95%.
[0078] Example 4
[0079] Step 1: Take UO2 powder in an agate mortar in a glove box, add 30% mass fraction of deionized water, mix and grind thoroughly. Load the slurry into a cylindrical mold with a diameter of 6mm and a sample molding height of 100mm. After vibrating the screen, apply a uniaxial pressure of 350MPa at room temperature. Turn on the digital temperature controller and set the parameters so that the heating jacket is heated to 170℃ at 5℃ / min and kept warm for 60min. After the insulation is completed, cool down to 60℃ at 4℃ / min. After the sample cools naturally to room temperature, demold and sample it. Apply a pressure of 350MPa continuously during the entire cold burning process. Then dry the sample in a vacuum drying oven at 60℃ for 12h.
[0080] Step 2: Place the dried cold-sintered sample into a tubular furnace and sinter it at 1400°C for 5 hours under the protection of a hydrogen-argon mixed gas to obtain UO2 nuclear fuel pellets with a density of 96%.
[0081] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for preparing a nuclear fuel element, It is characterized in that The preparation method comprises: S1, mixing raw materials with solvent to obtain slurry; S2, cold sintering the slurry; S3. The cold sintered product is subjected to pressureless sintering to obtain a nuclear fuel element.
2. The preparation method according to claim 1, It is characterized in that The raw material is a uranium-containing raw material or a combination of a uranium-containing raw material and an inorganic material; the uranium-containing raw material includes UO 2 、UN、U 3 Si 2 , UC, UCN; the inorganic material includes any one of silicon carbide, carbon nanotubes, graphene, diamond and aluminum.
3. The preparation method according to claim 2, It is characterized in that The volume ratio of the uranium-containing raw material to the inorganic material is (1-10):(9-0).
4. The preparation method according to claim 2, It is characterized in that The particle size of the uranium-containing raw material is 50nm to 170μm The preparation method according to claim 2 is characterized in that the silicon carbide is in a granular or whisker shape, the particle size of the granular silicon carbide is 20nm to 5μm; the diameter of the silicon carbide whisker is 20nm to 200nm and the length is 5 to 20μm; The diameter of carbon nanotubes is 5nm to 100nm and the length is 1 to 20μm; The plane diameter of graphene is 100nm~200μm; the particle size of diamond is 20nm~10μm; the particle size of aluminum is 20nm~10μm.
5. The preparation method according to claim 1, It is characterized in that The solvent includes any one of water, formic acid and acetic acid.
6. The preparation method according to claim 1, It is characterized in that The mass ratio of the raw material to the solvent is (70-75):(30-25).
7. The preparation method according to claim 1, It is characterized in that In the step S2, the cold sintering pressure is 200-500 MPa, the cold sintering temperature is 120-170° C., and the cold sintering time is 30-300 min.
8. The preparation method according to claim 1, It is characterized in that In the step S3, the pressureless sintering temperature is 200 to 1600° C., and the pressureless sintering time is 1 to 6 hours.
9. The preparation method according to claim 1, It is characterized in that Prior to step S1, the raw materials, ball milling beads and anhydrous ethanol were ball milled at a rotation speed of 60 to 70 rpm for 22 to 25 h.
10. A nuclear fuel element, It is characterized in that The nuclear fuel element is obtained by the preparation method of the nuclear fuel element according to any one of claims 1-9.
Citation Information
Cited By
High-entropy pyrochlore ceramic as well as preparation method and application thereof
CN119841641A
Ceramic slurry, ceramic prefabricated part, and preparation method and application of ceramic prefabricated part