Multi-metal sulfide electrocatalyst, preparation method and application
Through the preparation of polymetal sulfide electrocatalysts, using nitrogen-doped carbon loading and foam nickel structure, the problem of slow kinetics and high overpotentials of electrocatalysts in HER, OER and UOR is solved, and efficient and stable catalytic performance is achieved. and low-cost electrocatalysts suitable for a variety of application areas.
Patent Information
- Application Number
- CN202410941518.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-07-15
AI Technical Summary
The existing electrocatalysts are slow and overpotential in hydrogen evolution reaction (HER), oxygen evolution reaction (OER) and urea oxidation reaction (UOR), which hinders the realization of high energy efficiency and output power, and precious metal-based catalysts are expensive. , Laminated hydroxides have insufficient conductivity, carbon-based materials are easily oxidized during high current reactions, and the transition metal-based materials have unstable structure.
Using the preparation method of polymetal sulfide electrocatalyst, through the preparation, doping/replacement reaction and sulfurization doping of bimetal MOF, nitrogen-doped carbon-supported polymetal sulfide electrocatalyst, using the porous structure and sulfide of nickel foam Nanoclusters achieve the stability and efficiency of the catalyst.
A multifunctional electrocatalyst with excellent catalytic performance, low overpotential and high stability is obtained. It is suitable for HER, OER and UOR, meets the needs of industrial applications, and has a wide range of application potential due to the low cost of using transition metals.
Smart Images

Figure CN118988366A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of electrocatalysts, and in particular relates to multimetallic sulfide electrocatalysts, preparation methods and applications. Background Art
[0002] Urea is a basic metabolite that is ubiquitous in nature and abundant in agricultural environments and industrial wastewater. The use of advanced electrocatalytic technologies to convert biomass resources and industrial wastewater into valuable substances is crucial for environmental protection and the promotion of sustainable energy pathways. However, the slow kinetics and high overpotential problems of electrochemical processes in hydrogen evolution reaction (HER), oxygen evolution reaction (OER), and urea oxidation reaction (UOR) have largely hindered these reactions from achieving high energy efficiency and output power in various related applications. Therefore, ideal electrocatalysts with high activity, high stability, and low economic cost are extremely important for accelerating the redox kinetics of electrochemical processes.
[0003] The existing HER, OER, and UOR trifunctional catalysts include precious metal-based catalysts, layered hydroxide catalysts, carbon-based material catalysts, and transition metal-based catalysts. Precious metal-based catalysts have excellent performance but are expensive, which hinders their application; layered hydroxide catalysts have insufficient conductivity, which is not conducive to the transmission of electrons in the product; carbon-based materials are easily oxidized during high-current reactions, reducing current efficiency; transition metal-based materials have been widely studied and have certain application prospects, but their unstable structure leads to a significant decline in performance after a period of use, making it difficult to meet practical applications. Summary of the invention
[0004] In view of this, on the one hand, some embodiments disclose a method for preparing a multimetallic sulfide electrocatalyst, comprising the steps of:
[0005] S1. Preparation of bimetallic MOF;
[0006] A solution containing a first transition metal salt and a second transition metal salt is mixed with an organic ligand solution to obtain a first mixed solution; wherein the first transition metal salt and the second transition metal salt are XY with the same acid radical ion but different cations, X is Co, Fe, Ni, Mn, Zn or Cu, and Y is NO3 2- , Cl - or SO4 2- ;
[0007] The nickel foam is immersed in the first mixed solution to react, thereby obtaining a bimetallic MOF grown on the nickel foam;
[0008] S2. The bimetallic MOF grown on the nickel foam is immersed in a second mixed solution to perform a doping / substitution reaction of bimetallic metal ions, and a multimetal hydroxide nanostructure is grown on the bimetallic MOF; wherein the second mixed solution contains a third transition metal salt and a fourth transition metal salt that are different from the first transition metal salt and the second transition metal salt, and the third transition metal salt and the fourth transition metal salt are XY with the same acid radical ion but different cations, where X is Co, Fe, Ni, Mn, Zn or Cu, and Y is NO3 2- , Cl - or SO4 2- ;
[0009] S3. Sulfurization doping is performed on the polymetallic hydroxide nanostructure to obtain a nitrogen-doped carbon-supported polymetallic sulfide electrocatalyst.
[0010] Furthermore, in some embodiments of the preparation method of the multi-metal sulfide electrocatalyst disclosed, in step S1, the molar concentration ratio of the first transition metal salt to the second transition metal salt in the first mixed solution is 2:3-5, the molar concentration of the organic ligand solution is 0.2-0.4M, and the reaction time of the nickel foam in the first mixed solution is 2-6h.
[0011] In the method for preparing a multi-metal sulfide electrocatalyst disclosed in some embodiments, in step S2, the concentration ratio of the third transition metal salt to the fourth transition metal salt in the second mixed solution is 3:1-4.
[0012] In the method for preparing a multi-metal sulfide electrocatalyst disclosed in some embodiments, in step S2, the multi-metal hydroxide nanostructure is nanoparticles, nanosheets, nanowires, or nanoclusters.
[0013] In the preparation method of the multi-metal sulfide electrocatalyst disclosed in some embodiments, in step S2, the doping / substitution reaction is carried out at 15-40°C for 30-120 minutes, and then the obtained sample is vacuum dried at 60-90°C to grow a multi-metal hydroxide nanostructure on the bimetallic MOF.
[0014] Some embodiments disclose a method for preparing a multi-metal sulfide electrocatalyst. In step S3, the multi-metal hydroxide nanostructure is sulfided and doped with a dopant C2H5SH, S(CH3)2 or C2H5NS to obtain a nitrogen-doped carbon-supported multi-metal sulfide electrocatalyst.
[0015] In the preparation method of the multi-metal sulfide electrocatalyst disclosed in some embodiments, in step S3, the sulfidation doping includes: immersing the multi-metal hydroxide nanostructure in a dopant alcohol solution with a concentration of 0.25 to 1 mg / mL, hydrothermally heating the solution at 60 to 200° C. for 3 to 15 hours, cooling and drying.
[0016] In the method for preparing a multi-metal sulfide electrocatalyst disclosed in some embodiments, in step S3, the solvent of the alcohol solution is methanol, ethanol or propanol.
[0017] On the other hand, some embodiments disclose multi-metal sulfide electrocatalysts obtained by the preparation method of the multi-metal sulfide electrocatalyst disclosed in the embodiments of the present invention.
[0018] In yet another aspect, some embodiments disclose the use of a multi-metal sulfide catalyst as an electrocatalyst for a hydrogen evolution reaction, an oxygen evolution reaction, or a urea oxidation reaction.
[0019] The nitrogen-doped carbon-supported polymetallic sulfide electrocatalyst obtained by the preparation method of the polymetallic sulfide electrocatalyst disclosed in the embodiment of the present invention has a stable structure, and the three-dimensional structure nickel foam provides a porous structure, which is not only conducive to the contact between the catalyst and the reactant, but also conducive to the transmission of gas; the sulfide nanoclusters are stably anchored on the nickel foam, maintaining a low urea oxidation overpotential, and at the same time have excellent urea catalytic performance, high-efficiency electron transmission efficiency and ultra-long stability, with ultra-stable performance, and can meet the application needs of industrialization; it has three catalytic activities of HER / OER / UOR, and has a low overpotential for HER, OER and UOR, so it can be used in a variety of application fields, for example, it can be used as a catalyst for electrolysis of water to produce hydrogen and oxygen, and can be used for the degradation of urea in environmental governance; the multifunctionality makes the metal sulfide electrocatalyst have a wide range of potential in practical applications and can adapt to different needs. Moreover, transition metals are abundant in the earth's crust, low in price, and the preparation method is simple in steps, and the preparation and utilization of polymetallic sulfide electrocatalysts have good scalability. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 Flow chart of the preparation of the multimetallic sulfide catalyst in Example 1;
[0021] Figure 2 SEM image of CoZn-MOF in Example 1;
[0022] Figure 3 SEM image of NiFe-CoZn-LDH in Example 1;
[0023] Figure 4 SEM image of NiFeCoZn-S / NC in Example 1;
[0024] Figure 5 LSV curve diagram of HER test on NiFeCoZn-S / NC in Example 1;
[0025] Figure 6LSV curve of OER test on NiFeCoZn-S / NC in Example 1;
[0026] Figure 7 LSV curve diagram of UOR test on NiFeCoZn-S / NC in Example 1;
[0027] Figure 8 In Example 1, NiFeCoZn-S / NC was heated to 10 mA·cm -2 Stability test diagram under current density. DETAILED DESCRIPTION
[0028] The word "embodiment" used herein as an "exemplary" does not necessarily mean that any embodiment described is superior or better than other embodiments. Performance index tests in the embodiments of the present invention are performed using conventional test methods in the art unless otherwise specified. It should be understood that the terms described in the embodiments of the present invention are only used to describe specific implementation methods and are not intended to limit the contents disclosed in the embodiments of the present invention.
[0029] Unless otherwise specified, the technical and scientific terms used herein have the same meanings as commonly understood by ordinary technicians in the technical field to which the embodiments of the present invention belong; other experimental methods and technical means not specifically specified in the embodiments of the present invention refer to experimental methods and technical means commonly used by ordinary technicians in the field.
[0030] The terms "substantially" and "approximately" used herein are used to describe small fluctuations. For example, they can refer to less than or equal to ±5%, such as less than or equal to ±2%, such as less than or equal to ±1%, such as less than or equal to ±0.5%, such as less than or equal to ±0.2%, such as less than or equal to ±0.1%, such as less than or equal to ±0.05%. The numerical data represented or presented in the range format herein are used only for convenience and brevity, and should therefore be flexibly interpreted as including not only the values clearly listed as the limits of the range, but also all independent values or sub-ranges contained in the range. For example, the numerical range of "1-5%" should be interpreted as including not only the clearly listed values of 1% to 5%, but also the independent values and sub-ranges within the range shown. Therefore, independent values such as 2%, 3.5% and 4% and sub-ranges such as 1%-3%, 2%-4% and 3%-5% are included in this numerical range. This principle also applies to the range of only one numerical value. In addition, such an interpretation applies regardless of the width of the range or the characteristics described.
[0031] In this document, including in the claims, transitional words such as "comprises," "includes," "with," "having," "containing," "involving," "accommodating," etc. are understood to be open-ended, i.e., meaning "including but not limited to." Only the transitional words "consisting of" and "composed of" are closed transitional words.
[0032] In order to better illustrate the present invention, numerous specific details are provided in the specific examples below. It should be understood by those skilled in the art that the present invention can be implemented without certain specific details. In the embodiments, some methods, means, instruments, equipment, etc. well known to those skilled in the art are not described in detail in order to highlight the gist of the present invention.
[0033] Under the premise of no conflict, the technical features disclosed in the embodiments of the present invention may be arbitrarily combined, and the resulting technical solutions belong to the contents disclosed in the embodiments of the present invention.
[0034] In some embodiments, the method for preparing a multimetallic sulfide electrocatalyst comprises the steps of:
[0035] S1. Preparation of bimetallic MOF;
[0036] A solution containing a first transition metal salt and a second transition metal salt is mixed with an organic ligand solution to obtain a first mixed solution; wherein the first transition metal salt and the second transition metal salt are two types of XY with the same acid radical ion but different cations, X is Co, Fe, Ni, Mn, Zn or Cu, and Y is NO3, Cl - or SO4 2- ; Different cationic salts of the same acid radical ion can be Co(NO3)2, Fe(NO3)2, Ni(NO3)2, Mn(NO3)2, Zn(NO3)2 or Cu(NO3)2, or, CoCl2, FeCl2, NiCl2, MnCl2, Zn Cl2 or CuCl2, or, CoSO4, FeSO4, NiSO4, MnSO4, ZnSO4 or CuSO4;
[0037] The nickel foam is immersed in the first mixed solution to react, thereby obtaining a bimetallic MOF grown on the nickel foam.
[0038] Generally, a first transition metal salt and a second transition metal salt can be selected first, and an aqueous solution can be prepared according to a set ratio. Then, the aqueous solutions of the two salts are mixed to obtain a first mixed solution. Then, the cleaned nickel foam is immersed in the first mixed solution and reacted at room temperature. The reaction is usually completed after 2-6 hours. The nickel foam is removed, washed with deionized water and dried to obtain a bimetallic MOF sample grown on the nickel foam substrate.
[0039] Generally, by regulating the types of metal ions, such as copper salts, manganese salts, iron salts, etc., and the types of non-metallic particles, such as NO3 - , Cl - 、SO4 2- The morphology and performance of the formed MOF can be regulated by adjusting conditions such as reaction time; for example, by selecting different acid ions, the bimetallic MOF product will show different morphological changes such as nanosheets, nanorods, and nanoflowers. By selecting different metal ions, the HER / OER / UOR performance can be optimized.
[0040] In some embodiments, the molar concentration ratio of the first transition metal salt to the second transition metal salt in the first mixed solution is 2:3-5, the molar concentration of the organic ligand solution is 0.2-0.4M, and the reaction time of the nickel foam in the first mixed solution is 2-6h; wherein the organic ligand solution can be dimethylimidazole, 1,2,4-benzenetricarboxylic acid or 2,2'-biphenyldicarboxylic acid.
[0041] Usually, the nickel foam can be washed and treated with hydrochloric acid, ethanol and water in sequence to remove impurities on the surface of the nickel foam and obtain pure nickel foam as a base material.
[0042] S2. The bimetallic MOF grown on the nickel foam is immersed in a second mixed solution to perform a doping and substitution reaction of bimetallic ions, and a multimetal hydroxide nanostructure is grown on the bimetallic MOF; wherein the second mixed solution contains a third transition metal salt and a fourth transition metal salt different from the first transition metal salt and the second transition metal salt, and the third transition metal salt and the fourth transition metal salt are two types of XY with the same acid radical ion but different cations, X is Co, Fe, Ni, Mn, Zn or Cu, and Y is NO3 2- , Cl - or SO4 2- ; Different cationic salts of the same acid radical ion can be Co(NO3)2, Fe(NO3)2, Ni(NO3)2, Mn(NO3)2, Zn(NO3)2 or Cu(NO3)2, or, CoCl2, FeCl2, NiCl2, MnCl2, ZnCl2 or CuCl2, or CoSO4, FeSO4, NiSO4, MnSO4, ZnSO4 or CuSO4.
[0043] Generally, two acid radical ion salts of different cations can be selected as the third transition metal salt and the fourth transition metal salt, and are configured into an aqueous solution according to a set ratio to obtain a second mixed solution. The obtained multi-metal hydroxide nanostructure is then immersed in the second mixed solution and reacted at an ambient temperature of 15 to 40°C. The third transition metal ion and the fourth transition metal ion enter the bimetallic MOF structure by doping or substitution. After a reaction time of 30 to 120 minutes, the obtained sample is vacuum dried at 60 to 90°C to grow a multi-metal hydroxide nanostructure on the bimetallic MOF. Usually, the third transition metal ion is different from the first transition metal ion and the second transition metal ion, and the fourth transition metal ion is different from the first transition metal ion and the second transition metal ion.
[0044] Typically, the polymetallic hydroxide nanostructures grown on bimetallic MOFs are based on bimetallic MOF organic frameworks, and generate nanostructures with different morphologies such as nanoparticles, nanosheets, nanowires or nanoclusters on the surface; the nanostructures are typically layered double hydroxide nanosheets, i.e., LDH nanosheets, and the shapes of LDH nanosheets are typically triangles, rhombuses, rectangles, etc.
[0045] Generally, the selection of doped / substituted salt ion species has an important influence on the shape of LDH nanosheets formed on the surface of MOF. The reaction time of immersion in the solution has a great influence on the density and size of the formed LDH nanosheets, nanowires, etc. If the immersion time in the solution is too short, nanosheets that meet the required size and density cannot be formed. If the immersion time in the solution is too long, the density of the grown nanosheets is too high, which is not conducive to the next reaction. Generally, the appropriate density of the nanosheets has an important influence on the morphology and position of the load generated in the next reaction, so the reaction time is controlled within a reasonable range, for example, 30 to 120 minutes.
[0046] In some embodiments, the molar concentration ratio of the third transition metal salt to the fourth transition metal salt in the second mixed solution is 3:1-4.
[0047] S3. Sulfurization doping is performed on the polymetallic hydroxide nanostructure to obtain a nitrogen-doped carbon-supported polymetallic sulfide electrocatalyst; typically, the nitrogen-doped carbon-supported polymetallic sulfide is a sulfide nanocluster formed on the LDH nanosheet, with a size between 200 and 400 nm.
[0048] Generally, the concentration of the dopant has a great influence on the size and number of the sulfide clusters formed. Too low or too high a concentration is not conducive to the generation of nanoclusters of appropriate size. The time for the sulfur substitution reaction has a great influence on whether nanoclusters can be formed, the size of the nanoclusters and the density of the nanoclusters. If the sulfurization time is not enough, the morphology of the multi-metal hydroxide nanostructure sample remains basically unchanged, and the required nanoclusters cannot be obtained. If the sulfurization time is too long, the generated nanoclusters will gradually aggregate and fall off, which is not conducive to the generation of multi-level nanoclusters. In short, the concentration of the sulfurizing agent and the sulfurization time are adjusted to prepare sulfide nanoclusters of appropriate size and load. Only when the sulfurization time is appropriate, the prepared material has excellent stability. The sulfurization temperature also has an important influence on the morphology of the sample. When the temperature is too high, the morphology of the original multi-metal hydroxide nanostructure will be destroyed. When the temperature is low, the sulfurization effect is not obvious.
[0049] In some embodiments, the polymetallic hydroxide nanostructure is sulfided and doped with a dopant C2H5SH, S(CH3)2 or C2H5NS to obtain a nitrogen-doped carbon-supported polymetallic sulfide electrocatalyst. Generally, the polymetallic hydroxide nanostructure is subjected to an alcohol thermal method or a hydrothermal method for hybridization with a dopant C2H5SH, S(CH3)2 or C2H5NS, and the carbon, sulfur and nitrogen elements in the dopant enter the polymetallic hydroxide nanostructure to obtain a nitrogen-doped carbon-supported polymetallic sulfide, which can be used as an electrocatalyst, i.e., a nitrogen-doped carbon-supported polymetallic sulfide electrocatalyst.
[0050] In some embodiments, sulfide doping is to immerse the polymetallic hydroxide nanostructure in a dopant alcohol solution with a concentration of 0.25-1 mg / mL, hydrothermally heat the dopant and the polymetallic hydroxide nanostructure at 60-200° C., react for 3-15 hours, cool and dry.
[0051] In some embodiments, the solvent of the alcohol solution is methanol, ethanol or propanol. Usually, the dopant C2H5SH, S(CH3)2 or C2H5NS is configured with a solvent to form an alcohol solution, such as C2H5SH ethanol solution, S(CH3)2 ethanol solution or C2H5NS ethanol solution.
[0052] Some embodiments disclose multi-metal sulfide electrocatalysts obtained by the preparation method of the multi-metal sulfide electrocatalyst disclosed in the embodiments of the present invention.
[0053] Some embodiments disclose the use of a multimetallic sulfide catalyst as an electrocatalyst for a hydrogen evolution reaction, an oxygen evolution reaction, or a urea oxidation reaction.
[0054] Generally, the nitrogen-doped nitrogen-loaded multi-metal sulfide electrocatalyst obtained by the preparation method of the multi-metal sulfide electrocatalyst can be used as an electrocatalyst for hydrogen evolution reaction, oxygen evolution reaction or urea oxidation reaction.
[0055] The technical details are further illustrated below in conjunction with embodiments.
[0056] Example 1
[0057] In Example 1, the method for preparing the multimetallic sulfide electrocatalyst comprises the steps of:
[0058] S1. Preparation of bimetallic MOF;
[0059] Cobalt salt Co(NO3)2 and zinc salt Zn(NO3)2 are dissolved in water to prepare solution A;
[0060] The organic ligand is configured into solution B;
[0061] Solution A is mixed with solution B to obtain a uniform mixed solution, wherein the molar concentration ratio of Co(NO3)2 to Zn(NO3)2 is 2:3, and the molar concentration of dimethylimidazole in the organic ligand solution is 0.2M;
[0062] The nickel foam was washed with 3M HCl, C2H5OH, and deionized water in sequence;
[0063] The nickel foam is immersed in the uniform mixed solution for reaction at room temperature for 6 hours, and a sample X, namely CoZnMOF, is grown on the nickel foam; Figure 2 is the SEM image of CoZnMOF;
[0064] S2, the bimetallic MOF grown on the nickel foam is immersed in the second mixed solution to perform a doping / substitution reaction of the bimetallic ions;
[0065] Nickel salt Ni(NO3)2 and iron salt Fe(NO3)2 are dissolved in water to form solution C; the molar concentration ratio of nickel salt Ni(NO3)2 to iron salt Fe(NO3)2 is 3:1;
[0066] Sample X enters solution C and reacts at room temperature for 120 min. Then the obtained sample is dried in vacuum at 60-90°C to obtain sample Y, i.e., multimetal hydroxide nanowires NiFe-CoZnLDH grown on bimetallic MOF. Figure 3 is the SEM image of NiFe-CoZnLDH;
[0067] S3. Sulfurization-doping the polymetallic hydroxide nanostructures to obtain nitrogen-doped carbon-supported polymetallic sulfide electrocatalysts; using a dopant C2H5SH ethanol solution to sulfidize-dope the polymetallic hydroxide nanostructures to obtain nitrogen-doped carbon-supported polymetallic sulfide electrocatalysts; the concentration of the dopant C2H5SH ethanol solution is 0.25 mg / mL, and the reaction is hydrothermally heated at 60°C for 3 hours, cooled, and dried; sulfide nanoclusters with a size of 200 nm are obtained, and nitrogen-doped carbon-supported polymetallic sulfide electrocatalysts NiFeCoZn-S / NC are obtained. Figure 4 This is the SEM image of NiFeCoZn-S / N.
[0068] The performance of the nitrogen-doped carbon-supported multimetallic sulfide electrocatalyst NiFeCoZn-S / NC obtained in Example 1 was tested, and its catalytic performance as an electrocatalyst for hydrogen evolution reaction HER, oxygen evolution reaction OER, and urea oxidation reaction UOR was tested respectively. Figure 5 This is the LSV curve of the HER test. Figure 6 LSV curve diagram for OER test, Figure 7 LSV curve diagram for UOR test, Figure 8 At a current density of 10 mA cm -2 The stability test diagram below.
[0069] The nitrogen-doped carbon-supported polymetallic sulfide electrocatalyst obtained by the preparation method of the polymetallic sulfide electrocatalyst disclosed in the embodiment of the present invention has a stable structure, and the three-dimensional structure nickel foam provides a porous structure, which is not only conducive to the contact between the catalyst and the reactant, but also conducive to the transmission of gas; the sulfide nanoclusters are stably anchored on the nickel foam, maintaining a low urea oxidation overpotential, and at the same time have excellent urea catalytic performance, high-efficiency electron transmission efficiency and ultra-long stability, with ultra-stable performance, and can meet the application needs of industrialization; it has three catalytic activities of HER / OER / UOR, and has a low overpotential for HER, OER and UOR, so it can be used in a variety of application fields, for example, it can be used as a catalyst for electrolysis of water to produce hydrogen and oxygen, and can be used for the degradation of urea in environmental governance, etc.; the multifunctionality makes the metal sulfide electrocatalyst have a wide range of potential in practical applications and can adapt to different needs. Moreover, transition metals are abundant in the earth's crust, low in price, and the preparation method is simple in steps, and the preparation and utilization of polymetallic sulfide electrocatalysts have good scalability.
[0070] The technical solutions disclosed in the embodiments of the present invention and the technical details disclosed in the embodiments are merely illustrative of the inventive concept of the present invention and do not constitute a limitation on the technical solutions of the embodiments of the present invention. Any conventional changes, replacements or combinations of the technical details disclosed in the embodiments of the present invention have the same inventive concept as the present invention and are within the protection scope of the claims of the present invention.
Claims
1. A method for preparing a multimetallic sulfide electrocatalyst, characterized in that: Includes steps: S1. Preparation of bimetallic MOF; A solution containing a first transition metal salt and a second transition metal salt is mixed with an organic ligand solution to obtain a first mixed solution; wherein the first transition metal salt and the second transition metal salt are XY with the same acid radical ion but different cations, X is Co, Fe, Ni, Mn, Zn or Cu, and Y is NO3 2- , Cl - or SO4 2- ; The nickel foam is immersed in the first mixed solution to react, thereby obtaining a bimetallic MOF grown on the nickel foam; S2. The bimetallic MOF grown on the nickel foam is immersed in a second mixed solution to perform a doping / substitution reaction of bimetallic metal ions, and a multimetal hydroxide nanostructure is grown on the bimetallic MOF; wherein the second mixed solution contains a third transition metal salt and a fourth transition metal salt that are different from the first transition metal salt and the second transition metal salt, and the third transition metal salt and the fourth transition metal salt are XY with the same acid radical ion but different cations, where X is Co, Fe, Ni, Mn, Zn or Cu, and Y is NO3 2- , Cl - or SO4 2- ; S3. Sulfurization doping is performed on the polymetallic hydroxide nanostructure to obtain a nitrogen-doped carbon-supported polymetallic sulfide electrocatalyst.
2. The method for preparing a multimetallic sulfide electrocatalyst according to claim 1, characterized in that: In step S1, the molar concentration ratio of the first transition metal salt to the second transition metal salt in the first mixed solution is 2:3-5, the molar concentration of the organic ligand solution is 0.2-0.4M; and the reaction time of the nickel foam in the first mixed solution is 2-6h.
3. The method for preparing a multimetallic sulfide electrocatalyst according to claim 1, characterized in that: In step S2, the concentration ratio of the third transition metal salt to the fourth transition metal salt in the second mixed solution is 3:1-4.
4. The method for preparing a multimetallic sulfide electrocatalyst according to claim 1, characterized in that: In step S2, the polymetallic hydroxide nanostructures are nanoparticles, nanosheets, nanowires, and nanoclusters.
5. The method for preparing a multimetallic sulfide electrocatalyst according to claim 1, characterized in that: In step S2, the doping / substitution reaction is carried out at 15-40°C for 30-120 minutes, and then the obtained sample is vacuum dried at 60-90°C to grow a multi-metal hydroxide nanostructure on the bimetallic MOF.
6. The method for preparing a multimetallic sulfide electrocatalyst according to claim 1, characterized in that: In step S3, the polymetallic hydroxide nanostructure is sulfided and doped using a dopant C2H5SH, S(CH3)2 or C2H5NS to obtain a nitrogen-doped carbon-supported polymetallic sulfide electrocatalyst.
7. The method for preparing a multimetallic sulfide electrocatalyst according to claim 6, characterized in that: In step S3, the sulfide doping includes: immersing the multi-metal hydroxide nanostructure in a dopant alcohol solution with a concentration of 0.25-1 mg / mL, hydrothermally heating at 60-200° C. for 3-15 hours, cooling and drying.
8. The method for preparing a multimetallic sulfide electrocatalyst according to claim 7, characterized in that: In step S3, the solvent of the alcohol solution is methanol, ethanol or propanol.
9. A multimetallic sulfide electrocatalyst, characterized in that The method is obtained by the preparation method according to any one of claims 1 to 8.
10. Use of a multimetallic sulfide catalyst, characterized in that: The multimetal sulfide catalyst is used as an electrocatalyst for hydrogen evolution reaction, oxygen evolution reaction or urea oxidation reaction.
Citation Information
Patent Citations
Hollow core-shell structure supercapacitor material Fe-Co-S / NF as well as preparation method and application thereof
CN110176360A
Cobalt zinc bimetallic sulfide based composite electrocatalyst, and preparation method and applications thereof
CN110465310A
Preparation method of bismuth-doped bimetallic sulfide electrode for electro-catalytic oxidation of urea
CN112080759A
Preparation method and application of cobalt-based bimetallic sulfur / carbon catalyst derived from MOFs
CN113522317A
Multi-dimensional nickel-cobalt-based sulfide heterojunction electro-catalysis composite material and preparation method thereof
CN113981468A
Cited By
ZIF-derived CoZnS electrode material and preparation method and application thereof
CN119491261A
Copper modified graphite phase carbon nitride cathode catalytic material, urea electrooxidation device and application
CN122377508A