Preparation method of bimetallic anchoring porous graphite phase carbon nitride photocatalyst
By anchoring FeNi bimetallic nanoparticles on graphite phase carbon nitride nanosheets, pg-C3N4-x-FeNi nanocomposites are constructed, and carrier separation and catalytic activity of traditional graphite phase carbon nitride materials in photoelectro-catalysis is solved. The problem of insufficient has achieved nanocomposites with stable structure, strong photoresponse ability and rich catalytic active sites, which are suitable for photoelectric catalytic hydrogen production and pollutant degradation.
Patent Information
- Application Number
- CN202411048142.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-08-01
AI Technical Summary
Traditional monomer-prepared graphite phase carbon nitride (g-C3N4) materials have poor performance in photoexcited carriers, weak carrier separation ability and low active surface area, and lack effective in photoelectric catalytic redox reactions. There is a lack of research on the combination of nanomaterials and metal-based composite catalysts.
Thermal synthesis method is used to anchor FeNi bimetallic nanoparticles on porous graphite phase carbon nitride (pg-C3N4-x) nanosheets to construct pg-C3N4-x-FeNi nanocomposites, optimize the electronic band structure, and expand light absorption and improve the structural stability and catalytic activity of the material through steps such as ultrasonic and hydrothermal reactions.
It significantly improves the light absorption capacity, carrier separation efficiency and redox activity of the material, provides strong thermodynamic and kinetic driving force, improves the photoelectrocatalytic performance, and is suitable for photoelectrocatalytic hydrogen production and synchronous degradation of organic pollutants.
Smart Images

Figure CN118988369A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of photoelectrocatalytic hydrogen production and environmental pollution control, and in particular to a method for preparing a bimetallic anchored porous graphite phase carbon nitride photocatalyst. Background Art
[0002] g-C3N4 has been widely studied due to its appropriate band structure, long-term stability and low cost. However, the g-C3N4 prepared from simple monomers such as traditional melamine, urea and dicyandiamide has a small specific surface area and poor dispersibility, resulting in poor photon absorption of photoexcited carriers above 460nm, weak carrier separation ability and low active surface area. Defect engineering is often used to inhibit the recombination of photogenerated carriers and expand the light capture area to visible light, enhancing the photocatalytic ability of g-C3N4. The construction of N defects can manipulate the changes in the periodic crystal structure, resulting in the optimization of the chemical and electronic properties of the material, thereby improving the catalytic activity. At present, a variety of methods have been successfully prepared for pg-C3N 4-x Nanomaterials and a large number of pg-C3N 4-x However, little is known about the performance of N-deficient g-C3N4 and metal-based composite catalysts in the simultaneous degradation of organic pollutants by photoelectrocatalytic hydrogen evolution.
[0003] The introduction of FeNi bimetallic nanoparticles into the catalyst matrix can optimize the electronic band structure and shorten the band gap to expand the light absorption range. It can also serve as an active site to promote the hydrogen evolution reaction, promote the effective transfer of carriers, and provide a strong thermodynamic and kinetic driving force for the photoelectrocatalytic redox reaction process, thereby improving the photoelectrocatalytic performance of the material. 4-x On nanosheets, further improving the carrier separation efficiency and redox activity is an effective strategy to improve catalytic efficiency. 4-x -FeNi nanocomposites and their use in photoelectrocatalytic hydrogen production and synergistic degradation have not been reported. Summary of the invention
[0004] In order to solve the above technical problems, the present invention proposes a method for preparing a bimetallic anchored porous graphite phase carbon nitride photocatalyst.
[0005] The preparation method of the bimetallic anchored porous graphite phase carbon nitride photocatalyst proposed in the present invention adopts a thermal synthesis method to anchor FeNi bimetallic nanoparticles on pg-C3N 4-x On the nanosheets, pg-C3N with stable structure, strong visible light response ability, large electrochemical active surface area, high carrier separation efficiency and redox potential, and abundant catalytic active sites was obtained. 4-x-FeNi nanocomposite material, the preparation method thereof is as follows:
[0006] Step 1: Take a certain amount of urea and dissolve it in KOH aqueous solution under stirring, and continue stirring at 30-80°C for 10-90 minutes, then put the solution into an oven to dry;
[0007] Step 2: placing the solid mixture obtained after drying in step 1 into a box furnace, heating it to 300-450°C at a certain heating rate, and calcining it for 0.5-5h, then heating it to 450-600°C at the same heating rate, and keeping it at that temperature for 1-5h, and then cooling it naturally;
[0008] Step 3: Grind the cooled material into powder, wash it alternately with deionized water and ethanol, centrifuge it to remove the residual alkali, and then vacuum dry it to obtain pg-C3N 4-x ;
[0009] Step 4: Dissolve a certain amount of Fe(NO3)3·9H2O, NiSO4·6H2O and urea in an appropriate amount of deionized water and stir for 10-120 min;
[0010] Step 5: Pour the completely dissolved solution in step 4 into the inner lining of the hydrothermal reactor, react at a certain temperature for 6-24 hours, and then cool to room temperature. Wash and vacuum dry the obtained product to obtain FeNi-LDH;
[0011] Step 6: Add a certain amount of pg-C3N obtained in step 3 4-x The mixture was thoroughly mixed and ground with a certain amount of FeNi-LDH obtained in step 5, and then dispersed in an appropriate amount of ethanol, ultrasonicated for 0.5-3h, and stirred for 1-8h;
[0012] Step 7: Place the stirred and mixed solution into a vacuum drying oven and dry it at a certain temperature for 8-36 hours;
[0013] Step 8: Place the dried powder in a tube furnace, heat it to a certain temperature under N2 atmosphere, and keep it warm for 1-5 hours. After cooling naturally, wash and dry it to finally obtain a yellow-green solid powder, namely pg-C3N 4-x -FeNi nanocomposite materials.
[0014] Preferably, the mass of urea used in step 1 is 1-50 g, and the concentration of the KOH aqueous solution is 0.1-50 mM.
[0015] Preferably, the heating rate in step 2 is 1-30°C·min -1 .
[0016] Preferably, in step three, the vacuum drying temperature is 35-85° C. and the time is 4-24 h.
[0017] Preferably, the mass of Fe(NO3)3·9H2O used in step 4 is 1-10 g, the mass of NiSO4·6H2O is 1-20 g, the mass of urea is 0.5-10 g, and the volume of deionized water is 10-200 mL.
[0018] Preferably, the heating temperature of the hydrothermal reaction kettle in step 5 is 70-280° C.; the vacuum drying temperature is 35-95° C., and the time is 8-24 h.
[0019] Preferably, the pg-C3N used in step 6 4-x The mass of is 0.1-10 g, the mass of FeNi-LDH is 0.1-10 g, and the volume of ethanol is 40-200 mL.
[0020] Preferably, the vacuum drying temperature in step seven is 40-90°C.
[0021] Preferably, the heating temperature in step eight is 300-500°C.
[0022] Compared with the related art, the preparation method of the bimetallic anchored porous graphite phase carbon nitride photocatalyst proposed in the present invention has the following beneficial effects:
[0023] The present invention proposes a method for preparing a bimetallic anchored porous graphite phase carbon nitride photocatalyst:
[0024] Anchoring of FeNi bimetallic nanoparticles on pg-CN by thermal synthesis 4-x On the nanosheet, pg-C3N was constructed 4-x -FeNi nanocomposite material significantly improved the light absorption capacity of g-C3N4 matrix material, and successfully improved its band structure and the separation and migration capacity of photogenerated electrons and holes. 4-x -FeNi nanocomposites have the advantages of stable structure, strong visible light response ability, large electrochemical active surface area, high carrier separation efficiency and redox potential, and abundant catalytic active sites. They are expected to be applied in photoelectrocatalytic hydrogen production and simultaneous degradation of organic pollutants. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is an XRD diagram of a sample prepared in accordance with an embodiment of a method for preparing a bimetallic anchored porous graphite phase carbon nitride photocatalyst of the present invention;
[0026] Figure 2 The pg-C3N prepared in the preparation method of the bimetallic anchored porous graphite phase carbon nitride photocatalyst of the present invention is 4-x-TEM images of FeNi nanocomposites at different magnifications (the inset is a local magnified image);
[0027] Figure 3 The present invention is a (a) pg-C3N4, (b) pg-C3N 4-x and (c) 0.675-pg-C3N 4-x -Electrochemically active surface area of FeNi composites and (d) the corresponding fitting curves;
[0028] Figure 4 It is a hydrogen production rate diagram of a sample obtained in an embodiment of a method for preparing a bimetallic anchored porous graphite phase carbon nitride photocatalyst of the present invention;
[0029] Figure 5 This is a graph of the efficiency of hydrogen production and simultaneous formaldehyde oxidation of a sample obtained in an embodiment of a method for preparing a bimetallic anchored porous graphite phase carbon nitride photocatalyst of the present invention. DETAILED DESCRIPTION
[0030] The preferred embodiments of the present invention are described in detail below in conjunction with the accompanying drawings so that the advantages and features of the present invention can be more easily understood by those skilled in the art, thereby making a clearer and more definite definition of the protection scope of the present invention.
[0031] Embodiment 1:
[0032] The present invention provides a method for preparing a bimetallic anchored porous graphite phase carbon nitride photocatalyst, comprising the following steps:
[0033] (1) 10 g of urea was added to a 6.2 mM KOH aqueous solution under stirring, and the mixture was stirred at 80 °C for 20 min. The resulting solution was then placed in an oven for drying. The dried solid mixture was heated in a box furnace at 10 °C / min -1 The heating rate was 10 °C·min and the temperature was heated to 350 °C, kept at this temperature for 40 min, and then heated at 10 °C·min -1 The sample was heated to 450°C at a heating rate of 100 °C, kept at this temperature for 90 min, and then cooled naturally. The cooled product was ground into powder, and then washed alternately with deionized water and ethanol to remove the residual alkali. Finally, the sample was placed in a vacuum drying oven and dried at 60°C for 24 h to obtain 0.350-pg-C3N 4-x (where 0.350 is the mass of KOH used, in g);
[0034] (2) 1.52 g Fe(NO3)3·9H2O, 2.96 g NiSO4·6H2O and 0.9 g urea were used as raw materials and dissolved in 30 mL deionized water. The completely dissolved solution was poured into the lining of a hydrothermal reactor and reacted at 120°C for 12 h and then cooled to room temperature. The obtained product was washed with deionized water and ethanol and centrifuged, and then dried in a vacuum environment at 50°C for 12 h to obtain FeNi-LDH.
[0035] (3) 1g 0.350-pg-C3N 4-x After being fully mixed and ground with 1g FeNi-LDH, the mixture was dispersed in 40mL ethanol, ultrasonicated for 30min, stirred for 2h, and then dried in a vacuum environment at 50℃ for 24h. The dried product was then placed in a tube furnace, heated to 300℃ under N2 atmosphere, kept warm for 3h, cooled naturally, washed and dried, and 0.350-pCN was obtained. 4-x -FN nanocomposites.
[0036] Embodiment 2:
[0037] The present invention provides a method for preparing a bimetallic anchored porous graphite phase carbon nitride photocatalyst, comprising the following steps:
[0038] (1) 22.5 g of urea was added to a 12 mM KOH aqueous solution under stirring, and the mixture was stirred at 50 °C for 30 min. The resulting solution was then placed in an oven for drying. The dried solid mixture was heated in a box furnace at 15 °C / min -1 The heating rate was 15 °C·min and the temperature was kept at 400 °C for 1 h. -1 The sample was heated to 5000°C at a heating rate of 1000 °C, kept at this temperature for 2 h, and then cooled naturally. The cooled product was ground into powder, and then washed alternately with deionized water and ethanol to remove the residual alkali. Finally, the sample was placed in a vacuum drying oven and dried at 80°C for 12 h to obtain 0.675-pg-C3N 4-x (where 0.675 is the mass of KOH used, in g);
[0039] (2) 3.03 g Fe(NO3)3·9H2O, 5.91 g NiSO4·6H2O and 1.8 g urea were used as raw materials and dissolved in 60 mL deionized water. The completely dissolved solution was poured into the lining of a hydrothermal reactor and reacted at 140°C for 14 h and then cooled to room temperature. The obtained product was washed with deionized water and ethanol and centrifuged, and then dried in a vacuum environment at 60°C for 10 h to obtain FeNi-LDH.
[0040] (3) 2 g 0.675-pg-C3N 4-xAfter being fully mixed and ground with 2g FeNi-LDH, the mixture was dispersed in 80mL ethanol, ultrasonicated for 1h, stirred for 4h, and then dried in a vacuum environment at 60℃ for 18h. The dried product was then placed in a tube furnace, heated to 350℃ under N2 atmosphere, kept warm for 2h, cooled naturally, washed and dried, and 0.675-pCN was obtained. 4-x -FN nanocomposites.
[0041] Embodiment 3:
[0042] The present invention provides a method for preparing a bimetallic anchored porous graphite phase carbon nitride photocatalyst, comprising the following steps:
[0043] (1) 30 g of urea was added to a 17.8 mM KOH aqueous solution under stirring, and the mixture was stirred at 40 °C for 80 min. The resulting solution was then placed in an oven for drying. The dried solid mixture was heated in a box furnace at 20 °C / min -1 The heating rate was 30 °C·min -1 The sample was heated to 550°C at a heating rate of 1.000 °C, kept at this temperature for 4 h, and then cooled naturally. The cooled product was ground into powder, and then washed alternately with deionized water and ethanol to remove the residual alkali. Finally, the sample was placed in a vacuum drying oven and dried at 70°C for 18 h to obtain 1.000-pg-C3N 4-x (where 1.000 is the mass of KOH used, in g);
[0044] (2) 4.55 g Fe(NO3)3·9H2O, 8.87 g NiSO4·6H2O and 2.7 g urea were used as raw materials and dissolved in 90 mL deionized water. The completely dissolved solution was poured into the lining of a hydrothermal reactor and reacted at 200°C for 20 h and then cooled to room temperature. The obtained product was washed with deionized water and ethanol and centrifuged, and then dried in a vacuum environment at 80°C for 8 h to obtain FeNi-LDH.
[0045] (3) 3g 1.000-pg-C3N 4-x After being fully mixed and ground with 3g FeNi-LDH, the mixture was dispersed in 120mL ethanol, ultrasonicated for 2h, stirred for 6h, and then dried in a vacuum environment at 80℃ for 12h. The dried product was then placed in a tube furnace, heated to 400℃ in a N2 atmosphere, kept warm for 4h, cooled naturally, washed and dried, and 1.000-pCN was obtained. 4-x -FN nanocomposites.
[0046] Example 4
[0047] The photoelectrocatalytic performance test was carried out by preparing a 1M KOH+0.5M HCHO mixed solution as the electrolyte in the anode chamber and a 1M KOH solution as the electrolyte in the cathode chamber. 4-x -FeNi nanocomposite material was uniformly loaded on the surface of nickel foam as working electrode, Ag / AgCl electrode as reference electrode, and platinum sheet as counter electrode. The amount of H2 produced was measured every half an hour using a gas chromatograph. The concentration of formaldehyde during electrolysis was determined by UV-visible absorption using the Hantzsch reaction. Specifically, 20.0 μL of the anode chamber solution with different oxidation times was taken and acidified with 20 μL 2.0M HCl, and then diluted 2500 times. 2.0 mL of the diluted solution was mixed with 2.0 mL of acetylacetone mixed solution (wherein the acetylacetone mixed solution was prepared by mixing 15.4 g of ammonium acetate with 50 mL of water, 0.3 mL of glacial acetic acid, and 0.2 mL of acetylacetone and then diluting it with 49.5 mL of water), and then further heated to 60 ° C and kept warm for 10 min. After the solution was cooled, the absorbance of the sample solution at 413 nm was measured using a UV-visible absorption spectrometer. The concentration of HCHO was obtained from a calibration curve using a commercially available pure HCHO standard solution of known concentration.
[0048] The above descriptions are merely embodiments of the present invention and are not intended to limit the patent scope of the present invention. Any equivalent structure or equivalent process transformation made using the contents of the present invention specification and drawings, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.
Claims
1. A method for preparing a bimetallic anchored porous graphite phase carbon nitride photocatalyst, characterized in that: The preparation method comprises the following steps: Step 1: Take a certain amount of urea and dissolve it in KOH aqueous solution under stirring, and continue stirring at 30-80°C for 10-90 minutes, then put the solution into an oven to dry; Step 2: placing the solid mixture obtained after drying in step 1 into a box furnace, heating it to 300-450°C at a certain heating rate, and calcining it for 0.5-5h, then heating it to 450-600°C at the same heating rate, and keeping it at that temperature for 1-5h, and then cooling it naturally; Step 3: Grind the cooled material into powder, wash it alternately with deionized water and ethanol, centrifuge it to remove the residual alkali, and then vacuum dry it to obtain pg-C3N 4-x ; Step 4: Dissolve a certain amount of Fe(NO3)3·9H2O, NiSO4·6H2O and urea in an appropriate amount of deionized water and stir for 10-120 min; Step 5: Pour the completely dissolved solution in step 4 into the inner lining of the hydrothermal reactor, react at a certain temperature for 6-24 hours, and then cool to room temperature. Wash and vacuum dry the obtained product to obtain FeNi-LDH; Step 6: Add a certain amount of pg-C3N obtained in step 3 4-x The mixture was thoroughly mixed and ground with a certain amount of FeNi-LDH obtained in step 5, and then dispersed in an appropriate amount of ethanol, ultrasonicated for 0.5-3h, and stirred for 1-8h; Step 7: Place the stirred and mixed solution into a vacuum drying oven and dry it at a certain temperature for 8-36 hours; Step 8: Place the dried powder in a tube furnace, heat it to a certain temperature under N2 atmosphere, and keep it warm for 1-5 hours. After cooling naturally, wash and dry it to finally obtain a yellow-green solid powder, namely pg-C3N 4-x -FeNi nanocomposite materials.
2. The method for preparing the bimetallic anchored porous graphite phase carbon nitride photocatalyst according to claim 1, characterized in that: The mass of urea used in the step 1 is 1-50 g, and the concentration of the KOH aqueous solution is 0.1-50 mM.
3. The method for preparing the bimetallic anchored porous graphite phase carbon nitride photocatalyst according to claim 1, characterized in that: The heating rate in step 2 is 1-30°C·min -1 .
4. The method for preparing the bimetallic anchored porous graphite phase carbon nitride photocatalyst according to claim 1, characterized in that: In the step 3, the vacuum drying temperature is 35-85° C. and the time is 4-24 hours.
5. The method for preparing the bimetallic anchored porous graphite phase carbon nitride photocatalyst according to claim 1, characterized in that: The mass of Fe(NO3)3·9H2O used in step 4 is 1-10 g, the mass of NiSO4·6H2O is 1-20 g, the mass of urea is 0.5-10 g, and the volume of deionized water is 10-200 mL.
6. The method for preparing the bimetallic anchored porous graphite phase carbon nitride photocatalyst according to claim 1, characterized in that: In the step 5, the heating temperature of the hydrothermal reaction kettle is 70-280° C.; the vacuum drying temperature is 35-95° C., and the time is 8-24 hours.
7. The method for preparing the bimetallic anchored porous graphite phase carbon nitride photocatalyst according to claim 1, characterized in that: The pg-C3N used in step 6 4-x The mass of is 0.1-10 g, the mass of FeNi-LDH is 0.1-10 g, and the volume of ethanol is 40-200 mL.
8. The method for preparing the bimetallic anchored porous graphite phase carbon nitride photocatalyst according to claim 1, characterized in that: The vacuum drying temperature in step seven is 40-90°C.
9. The method for preparing the bimetallic anchored porous graphite phase carbon nitride photocatalyst according to claim 1, characterized in that: The heating temperature in step eight is 300-500°C.
Citation Information
Patent Citations
Preparation method of graphite phase carbon nitride-transition metal-based semiconductor composite photocatalytic material based on amino coordination stability
CN113713842A
Preparation method of porous carbon nitride-ferrite composite catalyst with nitrogen / oxygen dual defect structure and light nitrogen fixation application
CN113976155A
Cited By
Bimetal nanoparticle photocatalytic hydrogen evolution catalyst and preparation method thereof