Method for improving edge frizz of thin strip steel
By controlling the atmosphere in the hot box during the continuous casting of thin strips and adjusting the temperature of thin strips, the problem of frizzy edges of hot-rolled thin strips is solved, and the surface quality and material yield are improved.
Patent Information
- Application Number
- CN202411024105.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-22
AI Technical Summary
The prior art cannot effectively solve the frizz problem of hot-rolled thin strip steel in the thin strip continuous casting process, which affects the surface quality and material yield.
By controlling the atmosphere in the 4-score hot box, adjusting the temperature of the thin strip, including setting appropriate nitrogen and air flow, pressure, as well as the derivation speed and hot rolling down pressure, the edge quality of the thin strip is improved.
It effectively reduces the temperature of thin strip steel, improves the stability and surface quality of the hot rolling process, solves the problem of frizz on the edges, and improves the yield rate of the product.
Smart Images

Figure CN118989261A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of thin strip continuous casting, relates to edge quality control technology of thin strip steel produced by thin strip continuous casting, and more specifically to a method for improving the roughness of the edge of thin strip steel. Background Art
[0002] The thin strip continuous casting process is to pass the molten steel through the distribution system, into a pair of crystallization rollers rotating in opposite directions, and output it into thin strip steel as the crystallization rollers rotate. Subsequently, the thin strip steel is rolled into ultra-thin strip steel products through one hot rolling. After the twin-roller continuous casting thin strip steel is output from the crystallization roller, the temperature of the thin strip steel is relatively high. In particular, in order to ensure a smooth casting process, the edge temperature of the continuous casting thin strip steel is even higher, which results in the defect of rough edges of the hot-rolled thin strip steel after hot rolling (for example, see Figure 1 As shown in the figure, it will seriously affect the edge surface quality of hot-rolled thin strip steel.
[0003] The existing technology controls the surface quality of thin strip steel during the hot rolling process of thick slabs. Patent document 202110347442.2 provides a method for improving the surface quality of automobile steel. By controlling the rolling mileage, rolling frequency, and side guide plate pressure, automobile steel with good surface quality is obtained. Patent document 201911196896.4 provides a water circulation method and system for improving the surface quality of hot-rolled thin strip steel. The reverse cross-water supply process is adopted, which can not only meet the comprehensive concentration multiples of clean and turbid ring water above 3, but also meet the laminar water quality requirements. Under the existing descaling conditions, hot-rolled thin strip steel that meets the requirements of different users can be produced. Patent document 202210893064.3 discloses a surface quality control method for Ni-containing high-strength shipbuilding steel. Through chemical composition optimization and production process control, it can effectively solve the surface quality problem of Ni-containing high-strength shipbuilding steel, improve the surface quality while ensuring the performance of the steel plate, and reduce the production cost.
[0004] It can be seen that the existing technology cannot solve the surface quality problem of hot-rolled thin strip steel produced by thin strip continuous casting, and cannot solve the edge roughness problem of hot-rolled thin strip steel caused by the production process. Therefore, how to improve the edge roughness defect of hot-rolled thin strip steel produced by thin strip continuous casting is still a problem that needs to be solved. Summary of the invention
[0005] The purpose of the present invention is to provide a method for improving the rough edge of thin strip steel. The method of the present invention controls the atmosphere in the four-stage hot box, thereby controlling the temperature of the thin strip steel in the hot box after continuous casting, improving the rough edge problem of the thin strip steel and improving the edge quality of the thin strip steel.
[0006] The purpose of the present invention is specifically achieved through the following technical solutions:
[0007] According to one aspect of the present invention, a method for improving the edge roughness of thin strip steel is proposed, the method comprising the following steps:
[0008] 1) The molten steel with qualified composition is obtained through electric furnace or converter steelmaking, and is led out into thin strip steel through the joint of a pair of crystallization rollers rotating in opposite directions. The leading speed is controlled to be 10-50m / min, and the thickness of the thin strip steel is controlled to be greater than 1.85mm;
[0009] 2) After being led out from the junction of the crystallization rollers, the thin strip steel passes through the protection of 4 sections of hot boxes in sequence, and then is sent to the hot rolling mill for one hot rolling to form the hot-rolled thin strip steel, wherein the No. 1 hot box is located below the crystallization roller, and the thin strip steel passes through the looper in the No. 1 hot box and is sent to the transmission roller, and then the thin strip steel enters the No. 2 hot box, is sent to the No. 3 hot box through the No. 1 pinch roller, and passes through the rolling line roller and the anti-wrinkle roller, and enters the hot rolling mill through the No. 4 hot box for one hot rolling to form the hot-rolled thin strip steel;
[0010] in:
[0011] The total nitrogen flow rate in the 4-stage heat box No. 1, No. 2, No. 3 and No. 4 is controlled at 900-4000m 3 / h;
[0012] The nitrogen flow rate in the No. 1 hot box is controlled at 300~1500m 3 / h;
[0013] The nitrogen flow rate in the No. 2 hot box is controlled at 200-1000m 3 / h, nitrogen pressure is controlled at 5~100Pa;
[0014] The temperature of the thin strip steel in the No. 2 hot box is controlled at 1151-1320°C;
[0015] No. 3 and No. 4 hot boxes are protected by a mixed atmosphere of air and nitrogen;
[0016] The nitrogen flow rate in the No. 3 heat box is controlled at 0~300m 3 / h, nitrogen pressure is controlled at 10~50Pa;
[0017] The air flow rate in the No. 3 heat box is controlled at 0~50m 3 / h, air pressure is controlled at 5~20Pa;
[0018] The nitrogen flow rate in the No. 4 heat box is controlled at 0~50m 3 / h, air flow rate is controlled at 50~500m 3 / h.
[0019] According to the method for improving the edge roughness of thin strip steel of the present invention, preferably, in step 1), the molten steel is low carbon steel, high carbon steel, low alloy steel, high alloy steel or high silicon steel.
[0020] According to the method for improving edge roughness of thin strip steel of the present invention, preferably, the method further comprises: controlling the reduction amount of the hot rolling in one pass to be not less than 40%.
[0021] According to the method for improving edge roughness of thin strip steel of the present invention, preferably, the method further comprises: controlling the reduction amount of the hot rolling in one pass to be 40-65%.
[0022] According to the method for improving the roughness of the edge of thin strip steel of the present invention, preferably, the method further comprises: in step 1), the speed of the thin strip steel being discharged through the crystallization roller is controlled to be 20-48 m / min.
[0023] According to the method for improving the edge roughness of thin strip steel of the present invention, preferably, the method further comprises: controlling the total flow rate of nitrogen in the No. 1 heat box, the No. 2 heat box, the No. 3 heat box and the No. 4 heat box of the four sections to be within 1000-2800m 3 / h.
[0024] According to the method for improving the edge roughness of thin strip steel of the present invention, preferably, the method further comprises: controlling the total flow rate of nitrogen in the No. 1 heat box, the No. 2 heat box, the No. 3 heat box and the No. 4 heat box of the four sections to be between 1400 and 2700 m 3 / h.
[0025] According to the method for improving the edge roughness of thin strip steel of the present invention, preferably, the method further comprises: controlling the nitrogen flow rate in the No. 1 hot box to be between 500 and 1200 m / s; 3 / h.
[0026] According to the method for improving the edge roughness of thin strip steel of the present invention, preferably, the method further comprises: controlling the nitrogen flow rate in the No. 2 hot box to be between 200 and 980 m / s; 3 / h, the nitrogen pressure is controlled at 8~32Pa.
[0027] According to the method for improving the roughness of the edge of thin strip steel of the present invention, preferably, the method further comprises: the temperature of the thin strip steel in the No. 2 hot box is controlled at 1190-1270°C.
[0028] Beneficial technical effects
[0029] Compared with the prior art, the technical concept and corresponding technical solution of the present invention can at least achieve the following beneficial technical effects:
[0030] The method of the present invention fully considers the problem of rough edges of the continuously cast thin strip steel after one hot rolling, controls the temperature of the continuously cast thin strip steel for the first time, and particularly involves process control of controlling the atmosphere in the hot box to control the temperature of the casting strip.
[0031] The method of the present invention controls the process parameters such as the strip steel outlet speed, the total nitrogen flow rate in the No. 1 to No. 4 hot boxes, the nitrogen flow rate in the No. 1 hot box, the nitrogen flow rate and pressure in the No. 2 hot box, the strip steel temperature in the No. 2 hot box, the flow rate and pressure of nitrogen and air in the No. 3 and No. 4 hot boxes, and the hot rolling reduction amount, so as to adjust the exchange between the atmosphere in the hot box and the atmosphere outside the hot box, control the atmosphere temperature in the hot box, and then control the temperature of the continuously cast thin strip steel.
[0032] In summary, the method of the present invention reduces the temperature of the continuously cast thin strip steel by adjusting the hot box atmosphere, promotes the rolling stability of the hot rolling process and improves the surface quality, solves the problem of rough edges of hot-rolled thin strip steel, and improves the surface quality of the thin strip steel and the product yield rate. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings of the embodiments are briefly introduced below. Obviously, the drawings in the following description only relate to some embodiments of the present invention, but are not intended to limit the present invention.
[0034] Figure 1 This is a rough edge diagram of a thin steel strip according to the prior art.
[0035] Figure 2 3 is a surface diagram of the edge of a thin strip steel produced according to Example 1 of the present invention. DETAILED DESCRIPTION
[0036] In order to make the purpose, technical solution and advantages of the embodiment of the present invention clearer, the technical solution of the embodiment of the present invention will be clearly and completely described below. Obviously, the described embodiment is a part of the embodiment of the present invention, not all of the embodiments. Based on the described embodiment of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0037] Unless otherwise defined, technical or scientific terms used in the present invention shall have the common meanings understood by one of ordinary skill in the art to which the present invention belongs.
[0038] The following are embodiments of the present invention. The described embodiments are only a part of the embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments that can be obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0039] Example 1
[0040] The molten steel with qualified composition is obtained through electric furnace or converter steelmaking, and is discharged into a continuous casting thin strip with a thickness of 2.6mm through a pair of counter-rotating crystallizers at a discharge speed of 26m / min.
[0041] Subsequently, the continuous cast thin strip steel passes through a hot box with atmosphere protection. The total nitrogen flow rate of the hot box is 2700m 3 / h. The protective atmosphere of the No. 1 hot box located below the crystallizer is nitrogen, and the nitrogen flow rate is 1180m 3 / h, the continuous casting thin strip steel is fed into the No. 2 hot box by the loop guide. The protective atmosphere of the No. 2 hot box is nitrogen, and the nitrogen flow rate is 950m 3 / h, nitrogen pressure is 30Pa.
[0042] Subsequently, the continuous casting thin strip steel is fed into the No. 3 and No. 4 hot boxes through the No. 1 pinch roller. The protective atmosphere of the No. 3 and No. 4 hot boxes is a mixture of nitrogen and air. The nitrogen flow rate of the No. 3 hot box is 295m 3 / h, nitrogen pressure is 43Pa, air flow rate is 28m 3 / h, the air pressure is 8Pa. The nitrogen flow rate of the No. 4 hot box is 8m 3 / h, air flow rate is 57m 3 / h.
[0043] Through the atmosphere control in the hot box, the temperature of the continuous casting thin strip steel is 1268℃, and then the thin strip steel enters the hot rolling mill for rolling, and the hot rolling reduction is 64%. The edge surface of the hot rolled thin strip steel produced is smooth, without frizzy areas, such as Figure 2 shown.
[0044] Example 2
[0045] The molten steel with qualified composition is obtained through electric furnace or converter steelmaking, and is discharged into a continuous casting thin strip with a thickness of 2.1mm through a pair of counter-rotating crystallizers at a discharge speed of 39m / min.
[0046] Subsequently, the continuous cast thin strip steel passes through a hot box with atmosphere protection. The total nitrogen flow rate of the hot box is 2200m 3 / h. The protective atmosphere of the No. 1 hot box located below the crystallizer is nitrogen, and the nitrogen flow rate is 830m 3 / h, the continuous casting thin strip steel is fed into the No. 2 hot box by the loop guide. The protective atmosphere of the No. 2 hot box is nitrogen, and the nitrogen flow rate is 766m 3 / h, nitrogen pressure is 26Pa.
[0047] Subsequently, the continuous casting thin strip steel is fed into the No. 3 and No. 4 hot boxes through the No. 1 pinch roller. The protective atmosphere of the No. 3 and No. 4 hot boxes is a mixture of nitrogen and air. The nitrogen flow rate of the No. 3 hot box is 189m 3 / h, nitrogen pressure is 37Pa, air flow rate is 22m 3 / h, the air pressure is 12Pa. The nitrogen flow rate of the No. 4 hot box is 33m 3 / h, air flow rate is 350m 3 / h.
[0048] Through the atmosphere control in the hot box, the temperature of the continuous casting thin strip steel is 1232℃, and then the thin strip steel enters the hot rolling mill for rolling, and the hot rolling reduction is 56%. The edge surface of the hot rolled thin strip steel produced is smooth without frizzy areas.
[0049] Example 3
[0050] The molten steel with qualified composition is obtained through electric furnace or converter steelmaking, and is discharged into a continuous casting thin strip with a thickness of 1.89mm through a pair of counter-rotating crystallizers at a discharge speed of 47m / min.
[0051] Subsequently, the continuous cast thin strip steel passes through a hot box with atmosphere protection. The total nitrogen flow rate of the hot box is 1400m 3 / h. The protective atmosphere of the No. 1 hot box located below the crystallizer is nitrogen, and the nitrogen flow rate is 557m 3 / h, the continuous casting thin strip steel is fed into the No. 2 hot box by the loop guide. The protective atmosphere of the No. 2 hot box is nitrogen, and the nitrogen flow rate is 278m 3 / h, nitrogen pressure is 13Pa.
[0052] Subsequently, the continuous casting thin strip steel is fed into the No. 3 and No. 4 hot boxes through the No. 1 pinch roller. The protective atmosphere of the No. 3 and No. 4 hot boxes is a mixture of nitrogen and air. The nitrogen flow rate of the No. 3 hot box is 88m 3 / h, nitrogen pressure is 15Pa, air flow rate is 47m 3 / h, the air pressure is 19Pa. The nitrogen flow rate of the No. 4 hot box is 41m 3 / h, air flow rate is 475m 3 / h.
[0053] Through the atmosphere control in the hot box, the temperature of the continuous casting thin strip steel is 1193℃, and then the thin strip steel enters the hot rolling mill for rolling, and the hot rolling reduction is 43%. The edge surface of the hot rolled thin strip steel produced is smooth without frizzy areas.
[0054] The above description is only a specific implementation of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for improving the edge roughness of thin strip steel, characterized in that: The method comprises the following steps: 1) The molten steel with qualified composition is obtained through electric furnace or converter steelmaking, and is led out into thin strip steel through the joint point of a pair of crystallization rollers rotating in opposite directions. The leading speed is controlled to be 10-50m / min, and the thickness of the thin strip steel is controlled to be greater than 1.85mm; 2) After being led out from the junction of the crystallization rollers, the thin strip steel passes through the protection of 4 sections of hot boxes in sequence, and then is sent to the hot rolling mill for one hot rolling to form the hot-rolled thin strip steel, wherein the No. 1 hot box is located below the crystallization roller, and the thin strip steel passes through the looper in the No. 1 hot box and is sent to the transmission roller, and then the thin strip steel enters the No. 2 hot box, is sent to the No. 3 hot box through the No. 1 pinch roller, and passes through the rolling line roller and the anti-wrinkle roller, and enters the hot rolling mill through the No. 4 hot box for one hot rolling to form the hot-rolled thin strip steel; in: The total nitrogen flow rate in the 4-stage heat box No. 1, No. 2, No. 3 and No. 4 is controlled at 900-4000m 3 / h; The nitrogen flow rate in the No. 1 hot box is controlled at 300~1500m 3 / h; The nitrogen flow rate in the No. 2 hot box is controlled at 200-1000m 3 / h, nitrogen pressure is controlled at 5~100Pa; The temperature of the thin strip steel in the No. 2 hot box is controlled at 1151-1320°C; No. 3 and No. 4 hot boxes are protected by a mixed atmosphere of air and nitrogen; The nitrogen flow rate in the No. 3 heat box is controlled at 0~300m 3 / h, nitrogen pressure is controlled at 10~50Pa; The air flow rate in the No. 3 heat box is controlled at 0~50m 3 / h, air pressure is controlled at 5~20Pa; The nitrogen flow rate in the No. 4 heat box is controlled at 0~50m 3 / h, air flow rate is controlled at 50~500m 3 / h.
2. The method for improving the edge roughness of thin strip steel according to claim 1, characterized in that: In step 1), the molten steel is low carbon steel, high carbon steel, low alloy steel, high alloy steel or high silicon steel.
3. The method for improving the edge roughness of thin strip steel according to claim 1, characterized in that: The method further comprises: The reduction in the hot rolling pass is controlled to be not less than 40%.
4. The method for improving the edge roughness of thin strip steel according to claim 3, characterized in that: The method further comprises: The reduction in the first hot rolling pass is controlled to be 40 to 65%.
5. The method for improving the edge roughness of thin strip steel according to claim 1, characterized in that: The method further comprises: In step 1), the speed at which the thin strip steel is discharged through the crystallization roller is controlled to be 20 to 48 m / min.
6. The method for improving the edge roughness of thin strip steel according to claim 1, characterized in that: The method further comprises: The total nitrogen flow rate in the 4-stage heat box No. 1, No. 2, No. 3 and No. 4 is controlled within 1000-2800m 3 / h.
7. The method for improving the edge roughness of thin strip steel according to claim 6, characterized in that: The method further comprises: The total nitrogen flow rate in the 4-stage heat box No. 1, No. 2, No. 3 and No. 4 is controlled within 1400-2700m 3 / h.
8. The method for improving edge roughness of thin strip steel according to any one of claims 1 to 7, characterized in that: The method further comprises: The nitrogen flow rate in the No. 1 hot box is controlled at 500-1200m 3 / h.
9. The method for improving edge roughness of thin strip steel according to any one of claims 1 to 7, characterized in that: The method further comprises: The nitrogen flow rate in the No. 2 hot box is controlled at 200~980m 3 / h, the nitrogen pressure is controlled at 8~32Pa.