Preparation process of high-heat-resistance ceramic with non-sticky glaze surface
The non-stick glaze surface prepared through specific raw materials composition and process uses potassium nitrate melt for ion exchange to form a dense structure, which solves the problem of decomposition of existing ceramic non-stick glaze at high temperatures, and achieves high heat resistance and non-stick water The effect is suitable for cooking utensils and is safe and reliable.
Patent Information
- Application Number
- CN202411455109.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-18
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-10-18
AI Technical Summary
Existing ceramic non-stick glaze will be used to distribute harmful substances at high temperatures, which poses safety risks and is difficult to use in barbecue and cooking utensils.
The non-stick glaze surface composed of specific raw materials, including spodumene, talc, sodium feldspar, zinc oxide, etc., is prepared by wet ball milling, and then fired at high temperature to ion exchange in potassium nitrate melt. Form a dense micro- and nano-scale composite structure to achieve a non-stick water effect.
The prepared ceramics have high heat resistance and water-free effect. They are suitable for ceramic appliances, woks, frying pans and other cooking utensils. After firing, the ceramic retains a certain temperature, reduces the glaze expansion coefficient, improves the binding force, and complete products. The rate is increased and no harmful substances are released.
Smart Images

Figure CN118993543A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of ceramic preparation, and in particular relates to a preparation process of highly heat-resistant ceramics with non-stick glaze. Background Art
[0002] Ceramic glaze is a colorless or colored glassy thin layer covering the surface of ceramic products. It is made of mineral raw materials and chemical raw materials in a certain proportion, finely ground into glaze slurry, coated on the ceramic body and calcined; the main function of ceramic glaze is anti-fouling and decorative, making the texture of the ceramic surface soft and elegant, or smooth and crystal clear. With the innovation of design, it gives ceramics culture, spirit and life, making ceramics more alive.
[0003] Non-stick glaze porcelain refers to a ceramic material that can spontaneously remove pollutants in the external natural environment (solar energy, rain, wind, etc.) without the need for strong external scrubbing or the use of chemical agents such as detergents, relying only on the physical or chemical properties of the ceramic surface itself.
[0004] So far, all ceramic non-stick glazes on the market are coatings, most of which are Teflon (polytetrafluoroethylene). They will decompose and release harmful substances when the temperature exceeds 300°C, making them unsafe to use as barbecue cooking utensils; further improvement is needed. Summary of the invention
[0005] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a preparation process for high heat-resistant ceramics with non-stick glaze.
[0006] The present invention adopts the following technical solution: A preparation process of a high-heat-resistant ceramic with a non-stick glaze, the high-heat-resistant ceramic comprising a green body and a non-stick glaze, the non-stick glaze comprising the following raw materials in parts by weight: 55-60 parts of spodumene, 10-15 parts of talc, 5-10 parts of albite, 5-10 parts of quartz, 3-5 parts of zinc oxide, 3-5 parts of kaolin, 0.5-1 parts of titanium oxide, and 1-2 parts of cerium oxide; The preparation process specifically comprises the following steps: Step 1, weighing ingredients according to the non-stick glaze formula, crushing, mixing, and wet ball milling the raw materials to obtain glaze slurry; Step 2, applying the glaze slurry prepared in step 1 on the surface of the prepared ceramic body, putting the glaze slurry into a kiln after it is dried, firing it at 1320-1360° C., then cooling it to 900-940° C., keeping it warm for 2.5-3.5 hours, then cooling it to 420-480° C., and transferring it to a potassium nitrate melt at 435-460° C. and soaking it for 50-70 minutes to perform glaze ion exchange; Step 3, taking out the soaked ceramic body, cooling it naturally to room temperature, and washing it with hot water at 50-70° C. to obtain the high heat-resistant ceramic with a non-stick glaze surface.
[0007] Furthermore, the potassium nitrate content of the potassium nitrate melt is greater than 99%.
[0008] Furthermore, the preparation method of the potassium nitrate melt is as follows: placing potassium nitrate solid in a container, heating it to 435-460° C. to make it molten, so as to obtain potassium nitrate melt.
[0009] Furthermore, the green body comprises the following raw materials in parts by weight: 20-30 parts of diopside, 15-18 parts of albite, 10-15 parts of kaolin, 18-25 parts of quartz, 5-8 parts of magnesium oxide, 3-5 parts of brucite, 6-10 parts of calcite, 2-3 parts of aluminum oxide, and 3-5 parts of calcium oxide.
[0010] Furthermore, the steps for preparing the green body are as follows: A. Weighing and mixing ingredients according to the green body formula, crushing, sieving, mixing, and wet ball milling the raw materials to obtain green body slurry; B. Make the green body into a rough ceramic body, then send it into a kiln and bisque-fire it at 920-950℃ for 3-4h to form a ceramic body.
[0011] Furthermore, during wet ball milling of the green slurry, the raw material is wet ground in a ball mill for 24-28 hours, the grinding matrix is water, and the raw material: ball: water = 1:1.2-1.5:1.5-1.8.
[0012] Further, in step 2, the firing of the glaze slurry and the green body is controlled as follows: Low temperature stage: the temperature in the kiln rises from room temperature to 420-450℃, and the kiln firing time is 30-40 minutes; Decomposition and oxidation stage: the temperature in the kiln rises to 920-960°C, and the kiln firing time is 2-3 hours; High temperature firing stage: The temperature in the kiln is controlled at 1320-1360℃, and the firing time is 5-6 hours.
[0013] Furthermore, during the high-temperature firing stage, the concentration of carbon monoxide in the kiln was 2.8-3.2%, and the concentration of free oxygen was 1.6-1.8%.
[0014] Furthermore, in step 1, when the glaze slurry is wet-milled, the raw materials are wet-milled in a ball mill for 32-36 hours, the grinding matrix is water, and the raw material: ball: water = 1:1.5-1.8:1.8-2.
[0015] Furthermore, in step 2, the glaze slurry is applied on the surface of the body by dipping.
[0016] It can be seen from the above description of the present invention that, compared with the prior art, the present invention has the following beneficial effects: The present invention limits the raw material composition of the non-stick glaze and the specific preparation process, so that the prepared ceramic glaze has the effect of non-stick water, and can be used for cooking utensils such as ceramic home appliance inner pots, woks, frying pans, baking trays, etc., and has a broad market prospect; wherein, the fired ceramic is kept at a certain temperature, and then soaked in potassium nitrate melt, and the K in the solution + It is more active at a certain temperature and can exchange Li on the glaze surface. + and Na + , K + The radius is larger than Li + and Na + , K + The large ions "crowd" into the original positions of the small Li+ and Na+ ions, making the glaze surface more compact. SEM observations show that the glaze surface produces nipples with a micron- and nano-scale composite structure. Water will not spread to other directions on the glaze surface on these nano-scale tiny particles, making the glaze surface non-wetted by water, producing a water-resistant lotus leaf effect. Specifically control the firing process of ceramics. After firing, the ceramics are cooled to 900-940℃ and kept warm for 2.5-3.5h to purify the glaze surface and precipitate tiny crystals, thereby reducing the expansion coefficient of the glaze surface and controlling the expansion coefficient of the glaze surface to 1.0*10 -6 -1.3*10 -6 , which is slightly smaller than the body, resulting in a good combination of body and glaze, and can improve the strength of the ceramic. Among them, titanium oxide and cerium oxide are introduced into the glaze with other raw materials, so that when the fired ceramic is cooled to 900-940℃, tiny crystals can be quickly precipitated on the glaze surface; The raw material composition and biscuit firing process of the green body are specifically limited, so that the expansion coefficient of the green body after biscuit firing is controlled within 1.8*10 -6 -2.1*10 -6 , which is slightly larger than the non-stick glaze, resulting in a good combination of the body and glaze, thereby ensuring that the prepared ceramic glaze surface is smooth and crack-free, greatly improving the yield rate. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 This is a SEM electron microscope scanning image of the high heat-resistant ceramic prepared in Example 3; Figure 2 This is a SEM electron microscope scanning image of the high heat-resistant ceramic prepared in Comparative Example 1; Figure 3 This is a diagram showing the results of a water-wetting experiment on high heat-resistant ceramics prepared in Example 3; Figure 4 This is a graph showing the results of the water-wetting experiment on the high-heat-resistant ceramics prepared in Comparative Example 1. DETAILED DESCRIPTION
[0018] The present invention is further described below through specific implementation modes.
[0019] A highly heat-resistant ceramic with a non-stick glaze surface comprises a body and a non-stick glaze.
[0020] The green body comprises the following raw materials in parts by weight: 20-30 parts of diopside, 15-18 parts of albite, 10-15 parts of kaolin, 18-25 parts of quartz, 5-8 parts of magnesium oxide, 3-5 parts of brucite, 6-10 parts of calcite, 2-3 parts of aluminum oxide and 3-5 parts of calcium oxide.
[0021] The non-stick glaze comprises the following raw materials in parts by weight: 55-60 parts of spodumene, 10-15 parts of talc, 5-10 parts of albite, 5-10 parts of quartz, 3-5 parts of zinc oxide, 3-5 parts of kaolin, 0.5-1 parts of titanium oxide and 1-2 parts of cerium oxide.
[0022] The preparation process specifically comprises the following steps: Step 1, preparing a ceramic body: A. Weighing and mixing ingredients according to the green body formula, crushing, sieving, mixing, and wet ball milling the raw materials to obtain green body slurry; B. Make the green slurry into a ceramic rough green body, then send it into a kiln and bisque-fire it at 920-950℃ for 3-4h to form a ceramic green body; Step 2, weighing ingredients according to the non-stick glaze formula, crushing, mixing, and wet ball milling the raw materials to obtain glaze slurry; Step 3, applying the glaze slurry prepared in step 1 on the surface of the prepared ceramic body by dipping, putting the glaze slurry into a kiln after drying, firing at 1320-1360° C., then cooling to 900-940° C., keeping the temperature for 2.5-3.5 hours, then cooling to 420-480° C., and transferring to a potassium nitrate melt at 435-460° C. and soaking for 50-70 minutes to perform glaze ion exchange; Step 4, taking out the soaked ceramic body, cooling it naturally to room temperature, and washing it with hot water at 50-70° C. to obtain the high heat-resistant ceramic with a non-stick glaze surface.
[0023] Among them, when the green slurry is wet-milled, the raw material is wet-milled in a ball mill for 24-28 hours, the grinding matrix is water, and the raw material: ball: water = 1:1.2-1.5:1.5-1.8.
[0024] During wet ball milling of the glaze slurry, the raw materials are wet ground in a ball mill for 32-36 hours, the grinding matrix is water, and the raw material: ball: water = 1:1.5-1.8:1.8-2.
[0025] The firing control of glaze slurry and green body is as follows: Low temperature stage: the temperature in the kiln rises from room temperature to 420-450℃, and the kiln firing time is 30-40 minutes; Decomposition and oxidation stage: the temperature in the kiln rises to 920-960°C, and the kiln firing time is 2-3 hours; High temperature firing stage: The temperature in the kiln is controlled at 1320-1360℃, and the firing time is 5-6 hours.
[0026] Specifically, during the high-temperature firing stage, the concentration of carbon monoxide in the kiln is 2.8-3.2%, and the concentration of free oxygen is 1.6-1.8%.
[0027] The potassium nitrate molten liquid has a potassium nitrate content of more than 99%, and its preparation method is as follows: placing potassium nitrate solid in a container, heating it to 435-460° C. to make it molten, so as to obtain potassium nitrate molten liquid.
[0028] Example 1 A highly heat-resistant ceramic with a non-stick glaze surface comprises a body and a non-stick glaze.
[0029] The green body comprises the following raw materials in parts by weight: 20 parts of diopside, 18 parts of albite, 10 parts of kaolin, 25 parts of quartz, 5 parts of magnesium oxide, 5 parts of brucite, 6 parts of calcite, 3 parts of aluminum oxide and 3 parts of calcium oxide.
[0030] The non-stick glaze comprises the following raw materials in parts by weight: 55 parts of spodumene, 15 parts of talc, 5 parts of albite, 5 parts of quartz, 5 parts of zinc oxide, 3 parts of kaolin, 1 part of titanium oxide, and 2 parts of cerium oxide.
[0031] The preparation process specifically comprises the following steps: Step 1, preparing a ceramic body: A. Weighing and mixing ingredients according to the green body formula, crushing, sieving, mixing, and wet ball milling the raw materials to obtain green body slurry; B. Make the green slurry into a ceramic green body, then send it into a kiln and bisque-fire it at 920°C for 4 hours to form a ceramic green body; Step 2, weighing ingredients according to the non-stick glaze formula, crushing, mixing, and wet ball milling the raw materials to obtain glaze slurry; Step 3, applying the glaze slurry prepared in step 1 on the surface of the prepared ceramic body by dipping, putting the glaze slurry into a kiln after drying, firing at 1320° C., then cooling to 900° C., keeping the temperature for 3.5 hours, then cooling to 420° C., and transferring to a potassium nitrate melt at 435° C. and soaking for 70 minutes to perform glaze ion exchange; Step 4, taking out the soaked ceramic body, cooling it naturally to room temperature, and washing it with hot water at 50° C. to obtain the high heat-resistant ceramic with a non-stick glaze surface.
[0032] Among them, when the green slurry is wet-milled, the raw material is wet-milled in a ball mill for 24 hours, the grinding matrix is water, and the raw material: ball: water = 1:1.5:1.5.
[0033] During wet ball milling of the glaze slurry, the raw materials were wet ground in a ball mill for 32 hours, the grinding matrix was water, and the raw material: ball: water = 1:1.8:2.
[0034] The firing control of glaze slurry and green body is as follows: Low temperature stage: the temperature in the kiln rises from room temperature to 420℃, and the kiln firing time is 40 minutes; Decomposition and oxidation stage: the temperature in the kiln rises to 920°C and the kiln firing time is 3 hours; High temperature firing stage: the temperature in the kiln is controlled at 1320℃ and the firing time is 6 hours.
[0035] Specifically, during the high-temperature firing stage, the concentration of carbon monoxide in the kiln was 2.8% and the concentration of free oxygen was 1.8%.
[0036] The potassium nitrate melt has a potassium nitrate content of more than 99%, and its preparation method is as follows: placing potassium nitrate solid in a container, heating it to 435° C. to make it molten, so as to obtain potassium nitrate melt.
[0037] The high heat-resistant ceramics prepared in Example 1 were subjected to corresponding tests, wherein the water absorption rate was less than 0.5%, the green body expansion coefficient was 1.8*10 -6 , the glaze expansion coefficient is 1.3*10 -6 , the flexural strength is 128MPa.
[0038] Example 2 A highly heat-resistant ceramic with a non-stick glaze surface comprises a body and a non-stick glaze.
[0039] The green body comprises the following raw materials in parts by weight: 30 parts of diopside, 15 parts of albite, 15 parts of kaolin, 18 parts of quartz, 8 parts of magnesium oxide, 3 parts of brucite, 10 parts of calcite, 2 parts of aluminum oxide and 5 parts of calcium oxide.
[0040] The non-stick glaze comprises the following raw materials in parts by weight: 60 parts of spodumene, 10 parts of talc, 10 parts of albite, 5 parts of quartz, 3 parts of zinc oxide, 5 parts of kaolin, 0.5 parts of titanium oxide and 1 part of cerium oxide.
[0041] The preparation process specifically comprises the following steps: Step 1, preparing a ceramic body: A. Weighing and mixing ingredients according to the green body formula, crushing, sieving, mixing, and wet ball milling the raw materials to obtain green body slurry; B. Make the green slurry into a ceramic green body, then send it into a kiln and bisque-fire it at 950°C for 3 hours to form a ceramic green body; Step 2, weighing ingredients according to the non-stick glaze formula, crushing, mixing, and wet ball milling the raw materials to obtain glaze slurry; Step 3, applying the glaze slurry prepared in step 1 on the surface of the prepared ceramic body by dipping, putting the glaze slurry into a kiln after it is dried, firing it at 1360° C., then cooling it to 940° C., keeping it warm for 2.5 hours, then cooling it to 480° C., and transferring it to a potassium nitrate melt at 460° C. and soaking it for 50 minutes to perform glaze ion exchange; Step 4, taking out the soaked ceramic body, cooling it naturally to room temperature, and washing it with hot water at 70° C. to obtain the high heat-resistant ceramic with a non-stick glaze surface.
[0042] Among them, when the green slurry is wet ball milled, the raw material is wet ground in a ball mill for 28 hours, the grinding matrix is water, and the raw material: ball: water = 1:1.2:1.8.
[0043] During wet ball milling of the glaze slurry, the raw materials were wet ground in a ball mill for 36 hours, the grinding matrix was water, and the raw material: ball: water = 1:1.5:1.8.
[0044] The firing control of glaze slurry and green body is as follows: Low temperature stage: the temperature in the kiln rises from room temperature to 450°C, and the kiln firing time is 30 minutes; Decomposition and oxidation stage: the temperature in the kiln rises to 960°C and the kiln firing time is 2 hours; High temperature firing stage: The temperature in the kiln is controlled at 1360℃ and the firing time is 6 hours.
[0045] Specifically, during the high-temperature firing stage, the concentration of carbon monoxide in the kiln was 3.2% and the concentration of free oxygen was 1.6%.
[0046] The potassium nitrate melt has a potassium nitrate content of more than 99%, and its preparation method is as follows: placing potassium nitrate solid in a container, heating it to 460° C. to make it molten, so as to obtain the potassium nitrate melt.
[0047] The high heat-resistant ceramics prepared in Example 2 were subjected to corresponding tests, wherein the water absorption rate was less than 0.5%, the green body expansion coefficient was 2.1*10 -6 , the glaze expansion coefficient is 1.0*10 -6 , the flexural strength is 126MPa.
[0048] Example 3 A highly heat-resistant ceramic with a non-stick glaze surface comprises a body and a non-stick glaze.
[0049] The green body comprises the following raw materials in parts by weight: 25 parts of diopside, 10 parts of albite, 12 parts of kaolin, 22 parts of quartz, 6 parts of magnesium oxide, 4 parts of brucite, 8 parts of calcite, 2.5 parts of aluminum oxide and 4 parts of calcium oxide.
[0050] The non-stick glaze comprises the following raw materials in parts by weight: 58 parts of spodumene, 12 parts of talc, 8 parts of albite, 7 parts of quartz, 4 parts of zinc oxide, 4 parts of kaolin, 0.7 parts of titanium oxide, and 1.5 parts of cerium oxide.
[0051] The preparation process specifically comprises the following steps: Step 1, preparing a ceramic body: A. Weighing and mixing ingredients according to the green body formula, crushing, sieving, mixing, and wet ball milling the raw materials to obtain green body slurry; B. Make the green slurry into a ceramic green body, then send it into a kiln and bisque-fire it at 935°C for 3.5 hours to form a ceramic green body; Step 2, weighing ingredients according to the non-stick glaze formula, crushing, mixing, and wet ball milling the raw materials to obtain glaze slurry; Step 3, applying the glaze slurry prepared in step 1 on the surface of the prepared ceramic body by dipping, putting the glaze slurry into a kiln after drying, firing at 1350° C., then cooling to 920° C., keeping the temperature for 3 hours, then cooling to 450° C., and transferring to a 450° C. potassium nitrate melt to soak for 60 minutes for glaze ion exchange; Step 4, taking out the soaked ceramic body, cooling it naturally to room temperature, and washing it with hot water at 60° C. to obtain the high heat-resistant ceramic with a non-stick glaze surface.
[0052] Among them, when the green slurry is wet ball milled, the raw material is wet ground in a ball mill for 26 hours, the grinding matrix is water, and the raw material: ball: water = 1:1.3:1.6.
[0053] During wet ball milling of the glaze slurry, the raw materials were wet ground in a ball mill for 34 hours, the grinding matrix was water, and the raw material: ball: water = 1:1.6:1.9.
[0054] The firing control of glaze slurry and green body is as follows: Low temperature stage: the temperature in the kiln rises from room temperature to 435°C, and the kiln firing time is 35 minutes; Decomposition and oxidation stage: the temperature in the kiln rises to 940°C and the kiln firing time is 2.5 hours; High temperature firing stage: The temperature in the kiln is controlled at 1350℃ and the firing time is 5.5 hours.
[0055] Specifically, during the high-temperature firing stage, the concentration of carbon monoxide in the kiln was 3.0% and the concentration of free oxygen was 1.7%.
[0056] The high heat-resistant ceramics prepared in Example 3 were subjected to corresponding tests, wherein the water absorption rate was less than 0.5%, the green body expansion coefficient was 2.0*10 -6 , the glaze expansion coefficient is 1.1*10 -6 , the flexural strength is 132MPa.
[0057] The potassium nitrate melt has a potassium nitrate content of more than 99%, and its preparation method is as follows: placing potassium nitrate solid in a container, heating it to 450° C. to make it molten, so as to obtain the potassium nitrate melt.
[0058] Comparative Example 1 The raw material composition and preparation method are basically the same as those in Example 3, except that: The preparation process specifically comprises the following steps: Step 1, preparing a ceramic body: A. Weighing and mixing ingredients according to the green body formula, crushing, sieving, mixing, and wet ball milling the raw materials to obtain green body slurry; B. Make the green slurry into a ceramic green body, then send it into a kiln and bisque-fire it at 935°C for 3.5 hours to form a ceramic green body; Step 2, weighing ingredients according to the non-stick glaze formula, crushing, mixing, and wet ball milling the raw materials to obtain glaze slurry; Step 3, applying the glaze slurry prepared in step 1 on the surface of the prepared ceramic body by dipping, putting the glaze slurry into a kiln after it is dried, firing it at 1350°C, then cooling it to 920°C, keeping it warm for 3 hours, and then naturally cooling it to room temperature to obtain the high heat-resistant ceramic with a non-stick glaze surface.
[0059] The high heat-resistant ceramics prepared in Example 3 and the high heat-resistant ceramics prepared in Comparative Example 1 were subjected to glaze micromorphology analysis and water-wetting test. The specific results are shown in Figure 1 , Figure 2 , Figure 3 and Figure 4 ,pass Figure 1 and Figure 3 It can be seen that the surface of the high heat-resistant ceramic glaze prepared in Example 3 produces nipples of a micron- and nano-scale composite structure, and water will not spread to other directions on the glaze surface on these nano-scale tiny particles, so that the glaze surface is not wetted by water, and a water-free lotus leaf effect is produced; Figure 2 and Figure 4 It can be seen that the surface of the high heat-resistant ceramic glaze prepared in Comparative Example 1 does not produce nipples of micron- and nano-scale composite structures, so its glaze surface will be wetted by water and does not have a water-resistant effect.
[0060] In summary, the present application defines the raw material composition of the non-stick glaze and the specific preparation process, so that the prepared ceramic glaze has a water-resistant effect, which can be used for cooking utensils such as ceramic home appliance inner pots, woks, frying pans, baking trays, etc., and has a broad market prospect; wherein, the fired ceramic is kept at a certain temperature and then immersed in a potassium nitrate melt, and the K in the solution + It is more active at a certain temperature and can exchange Li on the glaze surface. + and Na + , K + The radius is larger than Li +and Na + , K + The large ions "crowd" into the original positions of the small Li+ and Na+ ions, making the glaze surface denser. SEM observations show that nipples of micron- and nano-scale composite structures are produced on the glaze surface. Water will not spread to other directions on the glaze surface on these nano-scale tiny particles, so that the glaze surface is not wetted by water, creating a lotus leaf effect that does not stick to water.
[0061] The above description is only a preferred embodiment of the present invention, and therefore cannot be used to limit the scope of implementation of the present invention. That is, equivalent changes and modifications made according to the application scope of the present invention and the contents of the specification should still fall within the scope of the present invention.
Claims
1. A preparation process of non-stick glaze high heat-resistant ceramics, characterized in that: The high heat-resistant ceramic comprises a body and a non-stick glaze, wherein the non-stick glaze comprises the following raw materials in parts by weight: 55-60 parts of spodumene, 10-15 parts of talc, 5-10 parts of albite, 5-10 parts of quartz, 3-5 parts of zinc oxide, 3-5 parts of kaolin, 0.5-1 parts of titanium oxide, and 1-2 parts of cerium oxide; The preparation process specifically comprises the following steps: Step 1, weighing ingredients according to the non-stick glaze formula, crushing, mixing, and wet ball milling the raw materials to obtain glaze slurry; Step 2, applying the glaze slurry prepared in step 1 on the surface of the prepared ceramic body, putting the glaze slurry into a kiln after it is dried, firing it at 1320-1360° C., then cooling it to 900-940° C., keeping it warm for 2.5-3.5 hours, then cooling it to 420-480° C., and transferring it to a potassium nitrate melt at 435-460° C. and soaking it for 50-70 minutes to perform glaze ion exchange; Step 3, taking out the soaked ceramic body, cooling it naturally to room temperature, and washing it with hot water at 50-70° C. to obtain the high heat-resistant ceramic with a non-stick glaze surface.
2. The preparation process of the non-stick glaze high heat-resistant ceramic according to claim 1, characterized in that: The potassium nitrate content of the potassium nitrate melt is greater than 99%.
3. The preparation process of the non-stick glaze high heat-resistant ceramic according to claim 2, characterized in that: The preparation method of the potassium nitrate melt is as follows: placing potassium nitrate solid in a container, heating it to 435-460° C. to make it molten, so as to obtain the potassium nitrate melt.
4. The preparation process of the non-stick glaze high heat-resistant ceramic according to claim 1, characterized in that: The green body comprises the following raw materials in parts by weight: 20-30 parts of diopside, 15-18 parts of albite, 10-15 parts of kaolin, 18-25 parts of quartz, 5-8 parts of magnesium oxide, 3-5 parts of brucite, 6-10 parts of calcite, 2-3 parts of aluminum oxide, and 3-5 parts of calcium oxide.
5. The process for preparing a non-stick glaze high heat-resistant ceramic according to claim 4, characterized in that: The steps for preparing the green body are as follows: A. Weighing and mixing ingredients according to the green body formula, crushing, sieving, mixing, and wet ball milling the raw materials to obtain green body slurry; B. Make the green body into a rough ceramic body, then send it into a kiln and bisque-fire it at 920-950℃ for 3-4h to form a ceramic body.
6. The preparation process of the non-stick glaze high heat-resistant ceramic according to claim 1, characterized in that: During wet ball milling of the green slurry, the raw materials are wet ground in a ball mill for 24-28 hours, the grinding matrix is water, and the raw material: ball: water = 1:1.2-1.5:1.5-1.
8.
7. The process for preparing a non-stick glaze high heat-resistant ceramic according to claim 1, characterized in that: Step 2, the firing control of the glaze slurry and the green body is as follows: Low temperature stage: the temperature in the kiln rises from room temperature to 420-450℃, and the kiln firing time is 30-40 minutes; Decomposition and oxidation stage: the temperature in the kiln rises to 920-960°C, and the kiln firing time is 2-3 hours; High temperature firing stage: The temperature in the kiln is controlled at 1320-1360℃, and the firing time is 5-6 hours.
8. The process for preparing a non-stick glaze high heat-resistant ceramic according to claim 7, characterized in that: During the high-temperature firing stage, the concentration of carbon monoxide in the kiln is 2.8-3.2%, and the concentration of free oxygen is 1.6-1.8%.
9. The process for preparing a non-stick glaze high heat-resistant ceramic according to claim 1, characterized in that: In step 1, when the glaze slurry is wet-milled, the raw materials are wet-milled in a ball mill for 32-36 hours, the grinding matrix is water, and the raw material: ball: water = 1:1.5-1.8:1.8-2.
10. The process for preparing a non-stick glaze high heat-resistant ceramic according to claim 1, characterized in that: In step 2, the glaze slurry is applied to the surface of the body by dipping.
Citation Information
Patent Citations
Environmentally friendly ceramic tile for kitchen and preparation method of environmentally friendly ceramic tile
CN108383495A
Negative ion easy-cleaning functional ceramic additive
CN108774069A
High strength antifouling tile and preparation method of same
CN109020481A
Long afterglow ceramic with non-cracking glazed surface and preparation process
CN109206013A
High-hardness wear-resistant satin glazed tile and preparation method thereof
CN113582662A
Cited By
Anti-fouling ceramic glaze water, anti-fouling ceramic and preparation method of anti-fouling ceramic
CN119306393A
Anti-fouling ceramic glaze, anti-fouling ceramic and preparation method thereof
CN119306393B