Inorganic nano composite antibacterial material for ABS (acrylonitrile butadiene styrene) and preparation method of inorganic nano composite antibacterial material

By introducing inorganic nanoparticles and functional additives into ABS materials, the problem of ABS materials breeding bacteria in humid environments is solved, and long-term antibacterial and versatile are achieved, and it is suitable for high-demand fields such as medical and food packaging.

CN118994723APending Publication Date: 2024-11-22QIONGTAI TEACHERS COLLEGE
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410910183.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-08
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Existing ABS materials are prone to breed bacteria in humid and high-temperature environments, leading to cross-infection and product contamination. Traditional organic antibacterial agents are prone to degradation, have a short-lasting antibacterial effect and are potentially harmful to the environment and health.

Method used

Inorganic nanocomposite antibacterial materials are used, including matrix materials (such as silica, titanium oxide, hydroxyapatite), antibacterial nanoparticles (such as silver nanoparticles, zinc oxide nanoparticles, copper nanoparticles), interface coupling agents and functions Additives (such as activated carbon nanoparticles, graphene oxides, barium titanate) ensure uniform dispersion and high binding force through surface modification and melt blending techniques.

Benefits of technology

It significantly improves the antibacterial performance and service life of the material, enhances mechanical strength and biocompatibility, provides broad-spectrum antibacterial effect and versatility, and is suitable for medical and food packaging fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118994723A_ABST
    Figure CN118994723A_ABST
Patent Text Reader

Abstract

The invention discloses an inorganic nano composite antibacterial material for ABS (Acrylonitrile Butadiene Styrene) and a preparation method of the inorganic nano composite antibacterial material. The material comprises a base material group, an antibacterial nanoparticle group, an interface coupling agent and stabilizer group and a functional additive group. The base material group contains silicon dioxide, titanium dioxide and hydroxyapatite; the antibacterial nano-particle group contains silver nano-particles, zinc oxide nano-particles and copper nano-particles; the interface coupling agent and stabilizer group contains isocyanate compounds; the functional additive group contains activated carbon nanoparticles, graphene oxide, nano cerium oxide and barium titanate. The content and the particle size range of each component are respectively optimized. The preparation method comprises the steps of grinding of the base material, preparation and modification of the nanoparticles, preliminary mixing, adding of the interface coupling agent, adding of the functional additive, melt blending and cooling forming. Compared with the prior art, the antibacterial property, the mechanical property, the functionality and the biocompatibility of the material are improved, and the material is suitable for the fields of medical instruments, food packaging and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of antibacterial materials, in particular to an inorganic nano-composite antibacterial material for ABS and a preparation method thereof. Background Art

[0002] With the development of society and the improvement of people's living standards, antibacterial materials are increasingly used in the fields of medical treatment, food packaging, household appliances and public facilities. However, the existing ABS (acrylonitrile-butadiene-styrene copolymer) materials are prone to breed bacteria during use, leading to cross infection and product contamination, especially in humid and high temperature environments. This problem is more serious. Therefore, the development of ABS composite materials with excellent antibacterial properties has become an urgent problem to be solved.

[0003] Traditional antibacterial materials are usually achieved by adding organic antibacterial agents, but organic antibacterial agents have the following significant disadvantages:

[0004] Easy to degrade: Organic antimicrobial agents are easy to degrade during long-term use, resulting in weakened or even disappearance of the antibacterial effect.

[0005] The antibacterial effect is not long-lasting: Due to the easy degradation of organic antibacterial agents, their antibacterial effect is usually difficult to maintain for a long time.

[0006] Environmental and health impacts: Some organic antimicrobial agents may cause potential harm to the environment and human health, such as producing toxic by-products.

[0007] In view of the above problems, inorganic nanocomposite antibacterial materials have gradually become a hot topic of research due to their advantages such as high stability, long-lasting antibacterial effect, and environmental and human-friendly properties. Inorganic nanomaterials, such as silver nanoparticles, zinc oxide nanoparticles, and copper nanoparticles, have excellent broad-spectrum antibacterial properties, high stability in the material, and are not easily degraded. By introducing these inorganic nanoparticles into the ABS matrix, the antibacterial properties and service life of the material can be significantly improved.

[0008] However, how to evenly disperse inorganic nanoparticles in the ABS matrix and ensure that they do not aggregate during use remains a technical challenge. In addition, the surface modification of different types of inorganic nanoparticles, the interfacial bonding strength with the matrix material, and the optimized design of functional additives are also important technical links in achieving efficient antibacterial ABS composite materials.

[0009] In order to solve the above problems, the present invention provides an inorganic nano-composite antibacterial material for ABS and a preparation method thereof. Summary of the invention

[0010] The object of the present invention is to provide an inorganic nano-composite antibacterial material for ABS and a preparation method thereof, which has antibacterial properties and material stability, and solves the problem that the antibacterial effect of ABS materials in the prior art is not durable.

[0011] To achieve the above object, the present invention provides the following technical solution: an inorganic nano-composite antibacterial material for ABS, the material comprising the following components:

[0012] Base material group;

[0013] antimicrobial nanoparticle group;

[0014] Interface coupling agent and stabilizer group;

[0015] Functional additives group.

[0016] Preferably, the matrix material group, the antibacterial nanoparticle group, the interface coupling agent and stabilizer group and the functional additive group include the following components:

[0017] Matrix material group: silica, titania, hydroxyapatite;

[0018] Antibacterial nanoparticle group: silver nanoparticles, zinc oxide nanoparticles, copper nanoparticles;

[0019] Interface coupling agent and stabilizer group: isocyanate compounds;

[0020] Functional additive group: activated carbon nanoparticles, graphene oxide, nano-cerium oxide, barium titanate.

[0021] Preferably, the content range of each component is as follows:

[0022] Silicon dioxide: 40%-60%;

[0023] Titanium dioxide: 15%-25%;

[0024] Hydroxyapatite: 5%-15%;

[0025] Silver nanoparticles: 0.5%-3%;

[0026] Zinc oxide nanoparticles: 1%-4%;

[0027] Copper nanoparticles: 0.5%-2%;

[0028] Activated carbon nanoparticles: 0.2%-1%;

[0029] Graphene oxide: 0.2%-1%;

[0030] Nano cerium oxide: 0.5%-2%;

[0031] Barium titanate: 1%-5%;

[0032] Isocyanate compounds: 0.1%-1%.

[0033] Preferably, the content range of each component is as follows:

[0034] Silicon dioxide: 45%-55%;

[0035] Titanium dioxide: 18%-22%;

[0036] Hydroxyapatite: 8%-12%;

[0037] Silver nanoparticles: 1%-2%;

[0038] Zinc oxide nanoparticles: 1.5%-2.5%;

[0039] Copper nanoparticles: 0.8%-1.2%;

[0040] Activated carbon nanoparticles: 0.4%-0.6%;

[0041] Graphene oxide: 0.4%-0.6%;

[0042] Nano cerium oxide: 0.8%-1.2%;

[0043] Barium titanate: 2.5%-3.5%;

[0044] Isocyanate compounds: 0.2%-0.4%.

[0045] Preferably, the particle size ranges of the silicon dioxide, titanium dioxide, hydroxyapatite, silver nanoparticles, zinc oxide nanoparticles, copper nanoparticles, activated carbon nanoparticles, graphene oxide, nano-cerium oxide and barium titanate are as follows:

[0046] Silicon dioxide: 50-200 nanometers;

[0047] Titanium dioxide: 20-100 nanometers;

[0048] Hydroxyapatite: 20-150 nm;

[0049] Silver nanoparticles: 10-50 nanometers;

[0050] Zinc oxide nanoparticles: 20-60 nanometers;

[0051] Copper nanoparticles: 10-30 nanometers;

[0052] Activated carbon nanoparticles: 5-20 nanometers;

[0053] Graphene oxide: 1-10 nanometers;

[0054] Nano cerium oxide: 10-40 nanometers;

[0055] Barium titanate: 20-100 nanometers.

[0056] A method for preparing an inorganic nano-composite antibacterial material for ABS comprises the following steps:

[0057] S1. Preparation of matrix materials: Prepare matrix materials of silicon dioxide, titanium dioxide and hydroxyapatite, mix the matrix materials in proportion, and grind them by a ball mill to ensure uniform dispersion, and the grinding time is 4-6 hours;

[0058] S2. Preparation and modification of nanoparticles: preparing silver nanoparticles, zinc oxide nanoparticles and copper nanoparticles, and performing surface modification treatments on them respectively, wherein the surface modifiers of the silver nanoparticles and zinc oxide nanoparticles are silane coupling agents, and the surface modifier of the copper nanoparticles is stearic acid, and the modification time is 2-4 hours;

[0059] S3, preliminary mixing: the modified silver nanoparticles, zinc oxide nanoparticles and copper nanoparticles are mixed with the matrix material in a proportion of matrix material: silver nanoparticles: zinc oxide nanoparticles: copper nanoparticles = 95:2:2:1, and stirred by a high-speed stirrer at a stirring speed of 1500-2000 rpm for 30-60 minutes;

[0060] S4. Adding an interface coupling agent: adding an isocyanate compound as an interface coupling agent and stabilizer to the mixture in an amount of 0.3% of the total mass of the mixture, stirring evenly for 20-30 minutes;

[0061] S5. Adding functional additives: adding activated carbon nanoparticles, graphene oxide, nano-cerium oxide and barium titanate as functional additives to the above mixture, with the addition ratio of each additive being 0.5%, 0.4%, 1% and 3% respectively, and dispersing the mixture by ultrasonic dispersion instrument for 30-45 minutes;

[0062] S6, melt blending: after all the ingredients are uniformly mixed, they are fed into a twin-screw extruder for melt blending, the melt temperature is 180-230°C, the shear rate is 100-200rpm, and the blending time is 10-15 minutes;

[0063] S7, cooling and molding: the blended material is extruded through a mold, and cooled by water cooling or air cooling, and the cooling temperature is controlled at 15-25° C., and finally an inorganic nano-composite antibacterial material for ABS is obtained.

[0064] Preferably, in the grinding step, the rotation speed of the ball mill is 200-400 rpm, and the grinding medium is zirconia beads with a diameter of 0.5-1 mm.

[0065] Preferably, in the ultrasonic dispersion treatment step, the ultrasonic frequency of the ultrasonic disperser is 20-40 kHz, the ultrasonic power is 500-1000 W, and the treatment environment temperature is controlled at 20-30°C.

[0066] Preferably, in the melt blending step, the residence time of the blended materials in the twin-screw extruder is 5-10 minutes to ensure adequate mixing and uniform dispersion.

[0067] Preferably, in the cooling step, the cooling water temperature of the water cooling method is 10-20° C., the cooling air temperature of the air cooling method is 15-25° C., and the cooling time is 5-10 minutes.

[0068] Compared with the prior art, the present invention has the following beneficial effects:

[0069] 1. The present invention significantly enhances the antibacterial effect of the material by providing an antibacterial nanoparticle group, including silver nanoparticles, zinc oxide nanoparticles and copper nanoparticles. These nanoparticles can effectively destroy bacterial cell membranes, inhibit bacterial growth, achieve a broad-spectrum antibacterial effect, and make the application of the material in medical devices and food packaging safer and more reliable.

[0070] 2. The present invention adds silicon dioxide, titanium dioxide and hydroxyapatite to the matrix material group, and introduces functional additives such as graphene oxide and barium titanate, which significantly improves the tensile strength and bending strength of the material, making it more durable when subjected to external forces, and suitable for high-demand application scenarios.

[0071] 3. By adding a functional additive group, including activated carbon nanoparticles, graphene oxide, nano-cerium oxide and barium titanate, the material of the present invention has multiple functions such as odor absorption, increased conductivity and anti-oxidation performance. These improvements enable the material to keep food fresh in food packaging and provide more added value in other applications.

[0072] 4. The addition of hydroxyapatite and zinc oxide nanoparticles not only provides antibacterial properties, but also significantly improves the biocompatibility of the material, making it more suitable for applications such as medical devices that require direct contact with organisms, reducing potential adverse effects on the human body. BRIEF DESCRIPTION OF THE DRAWINGS

[0073] Figure 1 The component structure diagram of the inorganic nano-composite antibacterial material for ABS of the present invention;

[0074] Figure 2 The composition diagram of the inorganic nano-composite antibacterial material for ABS of the present invention;

[0075] Figure 3Schematic diagram of the component content range of the inorganic nano-composite antibacterial material for ABS of the present invention;

[0076] Figure 4 Schematic diagram of the optimized component content range of the inorganic nano-composite antibacterial material for ABS of the present invention;

[0077] Figure 5 This is a diagram showing the particle size range of the inorganic nano-composite antibacterial material for ABS of the present invention;

[0078] Figure 6 The flowchart of the preparation method of the inorganic nano-composite antibacterial material for ABS of the present invention;

[0079] Figure 7 Detailed parameter diagram of the grinding step of the present invention;

[0080] Figure 8 Detailed parameter diagram of ultrasonic dispersion treatment of the present invention;

[0081] Fig. 9 Detailed parameter diagram of the melt blending step of the present invention;

[0082] Fig.10 Detailed parameter diagram of the cooling step of the present invention. DETAILED DESCRIPTION

[0083] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0084] See also Figures 1 to 10 The present invention provides a technical solution: an inorganic nano-composite antibacterial material for ABS, the material comprising the following components:

[0085] Matrix material group: The main component of the material, providing basic physical and chemical properties.

[0086] Antimicrobial nanoparticle group: Nanoparticles have antimicrobial properties and can inhibit or kill bacteria.

[0087] Interface coupling agent and stabilizer group: used to improve the bonding strength and stability between the components inside the material.

[0088] Functional additive group: These additives can give materials additional functions, including odor absorption and increased conductivity;

[0089] Specifically, the base material group, the antibacterial nanoparticle group, the interface coupling agent and stabilizer group and the functional additive group include the following components:

[0090] Matrix material group: includes silica, titanium dioxide, hydroxyapatite, these materials provide strong structure and chemical resistance.

[0091] Antibacterial nanoparticle group: including silver nanoparticles, zinc oxide nanoparticles, and copper nanoparticles. These nanoparticles have strong antibacterial properties.

[0092] Interface coupling agent and stabilizer group: including isocyanate compounds, mainly used to enhance the internal bonding force of the material and prevent the separation of components.

[0093] Functional additive group: including activated carbon nanoparticles, graphene oxide, nano-cerium oxide, and barium titanate. These ingredients give the material the function of absorbing odors, increasing conductivity and heat resistance;

[0094] Furthermore, the content range of each component is as follows:

[0095] Silicon dioxide: 40%-60%, provides the basic structure and chemical resistance of the material.

[0096] Titanium dioxide: 15%-25%, increases the strength and corrosion resistance of the material.

[0097] Hydroxyapatite: 5%-15%, enhances the biocompatibility and mechanical strength of the material.

[0098] Silver nanoparticles: 0.5%-3%, providing broad-spectrum antibacterial effects.

[0099] Zinc oxide nanoparticles: 1%-4%, with antibacterial and photocatalytic properties.

[0100] Copper nanoparticles: 0.5%-2%, further enhancing the antibacterial properties.

[0101] Activated carbon nanoparticles: 0.2%-1%, absorb odor and harmful gases.

[0102] Graphene oxide: 0.2%-1%, provides conductivity and mechanical strength.

[0103] Nano-cerium oxide: 0.5%-2%, provides antioxidant properties.

[0104] Barium titanate: 1%-5%, increases the piezoelectric properties of the material.

[0105] Isocyanate compounds: 0.1%-1%, enhance internal bonding strength and stability.

[0106] Among them, the particle size ranges of silicon dioxide, titanium dioxide, hydroxyapatite, silver nanoparticles, zinc oxide nanoparticles, copper nanoparticles, activated carbon nanoparticles, graphene oxide, nano-cerium oxide and barium titanate are as follows:

[0107] Silica: 50-200 nanometers, ensuring good dispersion and mechanical properties.

[0108] Titanium Dioxide: 20-100 nanometers, provides excellent strength and corrosion resistance.

[0109] Hydroxyapatite: 20-150 nanometers, enhances biocompatibility and mechanical strength.

[0110] Silver nanoparticles: 10-50 nanometers, ensuring optimal antibacterial properties.

[0111] Zinc oxide nanoparticles: 20-60 nanometers, provide antimicrobial and photocatalytic properties.

[0112] Copper nanoparticles: 10-30 nanometers, enhanced antibacterial effect.

[0113] Activated carbon nanoparticles: 5-20 nanometers, optimize the adsorption of odors and harmful gases.

[0114] Graphene oxide: 1-10 nanometers, improves conductivity and mechanical strength.

[0115] Nano cerium oxide: 10-40 nanometers, ensuring antioxidant properties.

[0116] Barium titanate: 20-100 nanometers, provides good piezoelectric properties.

[0117] A method for preparing an inorganic nano-composite antibacterial material for ABS comprises the following steps:

[0118] Preparation of base material:

[0119] S1: Prepare the matrix materials of silica, titanium dioxide and hydroxyapatite. After mixing these matrix materials in proportion, grind them through a ball mill to ensure that the components are evenly dispersed. The grinding time is 4-6 hours, so that the matrix materials can be fully mixed to form a uniform composite material base.

[0120] Preparation and modification of nanoparticles:

[0121] S2: Prepare silver nanoparticles, zinc oxide nanoparticles and copper nanoparticles, and perform surface modification treatment on them respectively. The surface modifiers of silver nanoparticles and zinc oxide nanoparticles are silane coupling agents, while the surface modifier of copper nanoparticles is stearic acid. The modification treatment time is 2-4 hours, and the purpose of this is to improve the dispersibility of the nanoparticles and the binding force with the matrix material.

[0122] Initial mixing:

[0123] S3: The modified silver nanoparticles, zinc oxide nanoparticles and copper nanoparticles are mixed with the matrix material in a proportion of matrix material: silver nanoparticles: zinc oxide nanoparticles: copper nanoparticles = 95:2:2:1. The mixture is stirred at a speed of 1500-2000 rpm for 30-60 minutes by a high-speed stirrer to ensure that the nanoparticles are evenly distributed in the matrix material.

[0124] Add interface coupling agent:

[0125] S4: Add isocyanate compounds as interface coupling agents and stabilizers to the mixture, with the addition amount being 0.3% of the total mass of the mixture. Stir evenly for 20-30 minutes. The purpose of this step is to enhance the bonding force between the components within the material and improve the stability of the material.

[0126] Adding functional additives:

[0127] S5: Add activated carbon nanoparticles, graphene oxide, nano cerium oxide and barium titanate to the above mixture in proportion. The addition ratio of each additive is 0.5%, 0.4%, 1% and 3% respectively. Dispersion treatment is performed by ultrasonic dispersion instrument for 30-45 minutes, so that these functional additives are evenly distributed in the material, giving the material more functional properties.

[0128] Melt Blending:

[0129] S6: After all the ingredients are evenly mixed, they are sent to a twin-screw extruder for melt blending. The melt temperature is 180-230°C, the shear rate is 100-200rpm, and the blending time is 10-15 minutes. This step ensures that the material components are fully integrated to form a uniform composite material.

[0130] Cooling molding:

[0131] S7: The blended material is extruded through a die and cooled by water cooling or air cooling. The cooling temperature is controlled at 15-25°C, and finally an inorganic nano-composite antibacterial material for ABS is obtained. This step ensures the stability and performance of the material after molding.

[0132] During the grinding process, the ball mill rotates at a speed of 200-400rpm, a speed range that ensures that the materials are fully mixed without over-crushing. Using zirconia beads with a diameter of 0.5-1 mm as grinding media helps improve grinding efficiency and dispersion, making the particles in the matrix material more evenly distributed.

[0133] During the ultrasonic dispersion process, the frequency of the ultrasonic disperser is set to 20-40kHz, which can effectively disperse the nanoparticles and prevent them from agglomerating. The ultrasonic power is 500-1000W to ensure sufficient energy to break up the particle agglomerates. The processing environment temperature is controlled at 20-30℃ to prevent the material from overheating and causing performance degradation.

[0134] During the melt blending process, the residence time of the blended materials in the twin-screw extruder is 5-10 minutes. This time range ensures that the ingredients of the materials are fully mixed and the nanoparticles are evenly dispersed in the matrix material, while avoiding the material from staying at high temperature for too long and causing degradation.

[0135] In the cooling step, the cooling water temperature is controlled at 10-20°C for water cooling and 15-25°C for air cooling. The cooling time is 5-10 minutes. These parameters ensure that the material maintains good shape and performance during the cooling process and avoids material defects caused by too fast or too slow cooling.

[0136] Example 1: Application in medical devices

[0137] In medical devices, the antibacterial property of materials is particularly important to avoid infection and cross contamination. The inorganic nano-composite antibacterial material for ABS provided by the present invention significantly improves the antibacterial property and stability of the material by introducing antibacterial nano-particles and functional additives. The application of the material in medical devices can not only inhibit bacterial growth, but also extend the service life of the device.

[0138] This embodiment focuses on the application of the present invention in medical devices. In this embodiment, by adding the inorganic nano-composite antibacterial material of the present invention to the ABS material, a broad-spectrum antibacterial effect is provided, and by adding functional additives, the biocompatibility and mechanical strength of the material are further enhanced.

[0139] Antibacterial performance test:

[0140] Sampling: The material of the present invention and the traditional ABS material are respectively made into medical device samples.

[0141] Test strains: Escherichia coli, Staphylococcus aureus.

[0142] Method: The samples were inoculated with the above strains respectively, and the colony counts were determined after culturing at 37℃ for 24 hours.

[0143]

[0144] Mechanical properties test:

[0145] Sampling: The material of the present invention and the traditional ABS material are respectively made into medical device samples.

[0146] Method: Use a universal material testing machine to test the tensile strength and flexural strength of the material.

[0147] sample Tensile strength(MPa) Flexural strength(MPa) Traditional ABS material 45 65 Material of the present invention 52 72

[0148] Biocompatibility testing:

[0149] Sampling: The material of the present invention and the traditional ABS material are respectively made into medical device samples.

[0150] Methods: The toxicity of the materials to cells was tested by MTT method.

[0151] sample Cell survival rate (%) Traditional ABS material 85 Material of the present invention 95

[0152] Example 2: Application in food packaging materials

[0153] Food packaging materials need to have excellent antibacterial properties to ensure food safety and extend shelf life. The inorganic nano-composite antibacterial material for ABS of the present invention combines antibacterial nanoparticles and functional additives, significantly improving the antibacterial effect and mechanical properties of the material, and is particularly suitable for the field of food packaging.

[0154] This embodiment demonstrates the application of the present invention in food packaging materials. In this embodiment, the inorganic nano-composite antibacterial material of the present invention is added to the ABS material to provide effective antibacterial protection, while activated carbon nanoparticles are added to further absorb odors and maintain the freshness of food.

[0155] Antibacterial performance test:

[0156] Sampling: The material of the present invention and the traditional ABS material are respectively made into food packaging material samples.

[0157] Test strains: Escherichia coli, Staphylococcus aureus.

[0158] Method: The samples were inoculated with the above strains respectively, and the colony counts were determined after culturing at 37℃ for 24 hours.

[0159]

[0160] Mechanical properties test:

[0161] Sampling: The material of the present invention and the traditional ABS material are respectively made into food packaging material samples.

[0162] Method: Use a universal material testing machine to test the tensile strength and flexural strength of the material.

[0163] sample Tensile strength(MPa) Flexural strength(MPa) Traditional ABS material 43 63 Material of the present invention 50 70

[0164] Odor adsorption test:

[0165] Sampling: The material of the present invention and the traditional ABS material are respectively made into food packaging material samples.

[0166] Method: The odor adsorption capacity of the materials was tested by gas chromatography.

[0167] sample Odor adsorption rate (%) Traditional ABS material 45 Material of the present invention 90

[0168] in conclusion:

[0169] Through the above examples and comparative experiments, it can be seen that the inorganic nano-composite antibacterial material for ABS of the present invention has shown significant superiority in the application of medical devices and food packaging materials. Compared with traditional ABS materials, the material of the present invention has significantly improved antibacterial properties, mechanical properties and functionality, and has a wide range of application prospects.

[0170] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. An inorganic nano-composite antibacterial material for ABS, characterized in that: The material includes the following components: Base material group; Antimicrobial nanoparticle group; Interface coupling agent and stabilizer group; Functional additives group.

2. The inorganic nano-composite antibacterial material for ABS according to claim 1, characterized in that: The matrix material group, the antibacterial nanoparticle group, the interface coupling agent and stabilizer group and the functional additive group include the following components: Matrix material group: silica, titania, hydroxyapatite; Antibacterial nanoparticle group: silver nanoparticles, zinc oxide nanoparticles, copper nanoparticles; Interface coupling agent and stabilizer group: isocyanate compounds; Functional additive group: activated carbon nanoparticles, graphene oxide, nano-cerium oxide, barium titanate.

3. The inorganic nano-composite antibacterial material for ABS according to claim 2, characterized in that: The content range of each ingredient is as follows: Silicon dioxide: 40%-60%; Titanium dioxide: 15%-25%; Hydroxyapatite: 5%-15%; Silver nanoparticles: 0.5%-3%; Zinc oxide nanoparticles: 1%-4%; Copper nanoparticles: 0.5%-2%; Activated carbon nanoparticles: 0.2%-1%; Graphene oxide: 0.2%-1%; Nano cerium oxide: 0.5%-2%; Barium titanate: 1%-5%; Isocyanate compounds: 0.1%-1%.

4. The inorganic nano-composite antibacterial material for ABS according to claim 3, characterized in that: The content range of each ingredient is as follows: Silicon dioxide: 45%-55%; Titanium dioxide: 18%-22%; Hydroxyapatite: 8%-12%; Silver nanoparticles: 1%-2%; Zinc oxide nanoparticles: 1.5%-2.5%; Copper nanoparticles: 0.8%-1.2%; Activated carbon nanoparticles: 0.4%-0.6%; Graphene oxide: 0.4%-0.6%; Nano cerium oxide: 0.8%-1.2%; Barium titanate: 2.5%-3.5%; Isocyanate compounds: 0.2%-0.4%.

5. The inorganic nano-composite antibacterial material for ABS according to claim 2, characterized in that: The particle size ranges of the silicon dioxide, titanium dioxide, hydroxyapatite, silver nanoparticles, zinc oxide nanoparticles, copper nanoparticles, activated carbon nanoparticles, graphene oxide, nano-cerium oxide and barium titanate are as follows: Silicon dioxide: 50-200 nanometers; Titanium dioxide: 20-100 nanometers; Hydroxyapatite: 20-150 nm; Silver nanoparticles: 10-50 nanometers; Zinc oxide nanoparticles: 20-60 nanometers; Copper nanoparticles: 10-30 nanometers; Activated carbon nanoparticles: 5-20 nanometers; Graphene oxide: 1-10 nanometers; Nano cerium oxide: 10-40 nanometers; Barium titanate: 20-100 nanometers.

6. A method for preparing an inorganic nano-composite antibacterial material for ABS, applied to an inorganic nano-composite antibacterial material for ABS according to any one of claims 1 to 5, characterized in that: The following steps are involved: S1. Preparation of matrix materials: Prepare matrix materials of silicon dioxide, titanium dioxide and hydroxyapatite, mix the matrix materials in proportion, and grind them by a ball mill to ensure uniform dispersion, and the grinding time is 4-6 hours; S2. Preparation and modification of nanoparticles: preparing silver nanoparticles, zinc oxide nanoparticles and copper nanoparticles, and performing surface modification treatments on them respectively, wherein the surface modifiers of the silver nanoparticles and zinc oxide nanoparticles are silane coupling agents, and the surface modifier of the copper nanoparticles is stearic acid, and the modification time is 2-4 hours; S3, preliminary mixing: the modified silver nanoparticles, zinc oxide nanoparticles and copper nanoparticles are mixed with the matrix material in a proportion of matrix material: silver nanoparticles: zinc oxide nanoparticles: copper nanoparticles = 95:2:2:1, and stirred by a high-speed stirrer at a stirring speed of 1500-2000 rpm for 30-60 minutes; S4. Adding an interface coupling agent: adding an isocyanate compound as an interface coupling agent and stabilizer to the mixture in an amount of 0.3% of the total mass of the mixture, stirring evenly for 20-30 minutes; S5. Adding functional additives: adding activated carbon nanoparticles, graphene oxide, nano-cerium oxide and barium titanate as functional additives to the above mixture, with the addition ratio of each additive being 0.5%, 0.4%, 1% and 3% respectively, and dispersing the mixture by ultrasonic dispersion instrument for 30-45 minutes; S6, melt blending: after all the ingredients are uniformly mixed, they are fed into a twin-screw extruder for melt blending, the melt temperature is 180-230°C, the shear rate is 100-200rpm, and the blending time is 10-15 minutes; S7, cooling and molding: the blended material is extruded through a mold, and cooled by water cooling or air cooling, and the cooling temperature is controlled at 15-25° C., and finally an inorganic nano-composite antibacterial material for ABS is obtained.

7. The method for preparing an inorganic nano-composite antibacterial material for ABS according to claim 6, characterized in that: In the grinding step, the rotation speed of the ball mill is 200-400 rpm, and the grinding medium is zirconia beads with a diameter of 0.5-1 mm.

8. The method for preparing an inorganic nano-composite antibacterial material for ABS according to claim 6, characterized in that: In the ultrasonic dispersion treatment step, the ultrasonic frequency of the ultrasonic disperser is 20-40kHz, the ultrasonic power is 500-1000W, and the treatment environment temperature is controlled at 20-30°C.

9. The method for preparing an inorganic nano-composite antibacterial material for ABS according to claim 6, characterized in that: In the melt blending step, the residence time of the blended materials in the twin-screw extruder is 5-10 minutes to ensure adequate mixing and uniform dispersion.

10. The method for preparing an inorganic nano-composite antibacterial material for ABS according to claim 6, characterized in that: In the cooling step, the cooling water temperature of the water cooling method is 10-20° C., the cooling air temperature of the air cooling method is 15-25° C., and the cooling time is 5-10 minutes.

Citation Information

Cited By

  • A bactericidal preparation for protecting structures against microbial degradation

    EP4840312A1