Preparation method and application of amino-functionalized graphene oxide for wear-resistant coating
By covalently functionalizing graphene oxide with N,N-dimethylformamide and octadecamine, the environmental pollution and high cost problems of graphene oxide in wear-resistant coatings are solved, and graphene oxide is realized. The uniform dispersion in organic matrix and the wear resistance of the coating are improved.
Patent Information
- Application Number
- CN202411092335.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-22
AI Technical Summary
The prior art has the risk of environmental pollution and high costs when modified graphene oxide is used in wear-resistant coatings, and the curing speed of small molecule modification is slow, making it difficult to meet the actual application needs.
N,N-dimethylformamide and octadecamine were used to covalently functionalize graphene oxide, and aminofunctionalized graphene oxide was prepared by ultrasonic and magnetic stirring, forming stable amide bonds and enhancing interface binding force. Promotes its uniform dispersion in the organic matrix.
Good water dispersion and stability of graphene oxide is achieved, process time is shortened, cost is reduced, and the wear resistance of the coating is improved and practical application is practical.
Smart Images

Figure CN118994944A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of wear-resistant coatings, and in particular relates to a preparation method and application of amino-functionalized graphene oxide for wear-resistant coatings. Background Art
[0002] Graphene is a two-dimensional nanofiller with excellent physical and chemical properties. It has been widely used to improve the tribological properties of organic coatings. It can significantly improve the mechanical properties of polymer substrates, reduce friction, and is accompanied by the formation of self-lubricating and high-strength continuous transfer films, thus significantly improving the wear resistance of the substrate material. However, the nanofilling of graphene is often limited by its inherent large specific surface area and inherent van der Waals forces. Due to these factors, graphene has a tendency to aggregate in the organic coating matrix. As a graphene derivative, the introduction of oxygen-containing groups makes graphene oxide (GO) chemically stable, but produces large surface active sites and a high specific surface area for chemical modification, which provides great potential for improving the interfacial bonding between the coating substrate and graphene. At present, the surface modification of GO can be achieved by covalent functionalization. However, it is demanding, immature, and easy to pollute the environment. Therefore, it has been a huge challenge to expand the application of graphene in organic coatings by preparing and functionalizing GO using environmentally friendly, simple, and low-cost processes.
[0003] At present, the modification and utilization of graphene oxide is mostly in the field of corrosion protection. For example, CN107828307A discloses a preparation process of a modified graphene oxide / epoxy composite anti-corrosion coating, which introduces amide bonds and cross-linking structures by adding N,N-dimethylformamide, thereby improving the dispersion stability of graphene oxide in the resin system and the shielding ability of the coating against corrosion elements. For example, CN105820645A discloses a preparation method of ethylenediamine-modified graphene coating, which uses small molecule ethylenediamine to reduce and modify graphene, reduce the agglomeration of graphene, and thus improve the overall performance. However, this method is also limited to the field of corrosion protection, and when the amine group of the small molecule chain is used for the epoxy group, its curing speed is far less than that of the long-chain amine, and the time cost required for actual application is much higher. Summary of the invention
[0004] In order to solve the above technical problems, the present invention proposes a preparation method and application of amino-functionalized graphene oxide for wear-resistant coating.
[0005] To achieve the above object, the present invention provides the following technical solutions:
[0006] A method for preparing amino-functionalized graphene oxide for wear-resistant coating comprises the following steps:
[0007] The graphene oxide aqueous dispersion is mixed with N,N-dimethylformamide, and stirred in an ice bath to obtain an intermediate product A;
[0008] The intermediate product A is subjected to magnetic stirring, and octadecylamine is added at the same time, and the intermediate product B is obtained after magnetic stirring;
[0009] The intermediate product B is separated and purified, then subjected to ultrasound, the pH is adjusted to alkaline, and after centrifugal separation and purification, the precipitate is collected and vacuum dried to obtain the amino-functionalized graphene oxide for wear-resistant coating.
[0010] Preferably, the mass ratio of the graphene oxide aqueous dispersion to N,N-dimethylformamide is 1:27.
[0011] Preferably, the preparation method of the graphene oxide aqueous dispersion is: in a buffer system with pH = 7, graphene oxide sheets with a sheet diameter of 1-50 μm and a thickness of 0.5-2 nm are selected and added to the above buffer system, and ultrasonicated in an ice bath for 1 hour with an ultrasonic power of 120-150 w to obtain the graphene oxide aqueous dispersion.
[0012] Preferably, the concentration of the graphene oxide aqueous dispersion is 10 mg / mL.
[0013] Preferably, the buffer system with pH=7 is distilled water.
[0014] Preferably, the mass ratio of octadecylamine to the graphene oxide aqueous dispersion is (4-9):1.
[0015] Preferably, the step of adjusting the pH to alkaline is adjusting the pH to 7.5.
[0016] Preferably, the power of the ultrasound is 120-150w, and the ultrasound time is 2-4h;
[0017] The centrifugal speed is 6000-7000 r / min, and the centrifugal time is 10-20 min.
[0018] The present invention also provides amino-functionalized graphene oxide for wear-resistant coating prepared according to the above method.
[0019] The present invention also provides a wear-resistant coating, which contains the amino-functionalized graphene oxide for wear-resistant coating.
[0020] The present invention also provides the use of the amino-functionalized graphene oxide in the preparation of wear-resistant coatings.
[0021] For example, the preparation method of the wear-resistant coating is:
[0022] 1) mixing N,N-dimethylformamide, xylene and acetone in a mass ratio of 6:1:3 to obtain an intermediate solvent;
[0023] 2) adding epoxy resin to the intermediate solvent, stirring with a mechanical stirrer for 30 min until fully mixed, to obtain epoxy resin emulsion, adding curing agent polyamide to the epoxy resin emulsion and magnetically stirring for 30 min until the epoxy resin and the curing agent are completely dissolved, to obtain a mixed emulsion;
[0024] 3) adding amino-functionalized graphene oxide to N,N-dimethylformamide to obtain a mixed solution (the amino-functionalized graphene oxide accounts for 1 wt.% of the total mass of the mixed solution), and ultrasonicating at an ultrasonic power of 150 W for 30 min to obtain an amino-functionalized graphene oxide dispersion;
[0025] 4) adding the amino-functionalized graphene oxide dispersion to the mixed emulsion and magnetically stirring for 2 h, then ultrasonicating for 2 h at a power of 150 W, and drying for 28 h until it becomes viscous to obtain a wear-resistant coating.
[0026] The present invention also provides the use of the amino-functionalized graphene oxide in preparing a wear-resistant coating.
[0027] In the present invention, the method for preparing a wear-resistant coating using the wear-resistant coating is: coating the wear-resistant coating containing amino-functionalized graphene oxide on a substrate, and obtaining the wear-resistant coating after curing. For example, the wear-resistant coating can be uniformly coated on a martensitic stainless steel substrate using a wire rod coater, and the wear-resistant coating can be obtained after curing.
[0028] According to the chemical structure, the functionalization of graphene oxide is divided into covalent bonding and non-covalent bonding. Non-covalent bonding refers to the use of the ultra-large specific surface area of graphene, and through the method of surface adsorption, it is combined with other particles with excellent performance. Although this method does not destroy the basic structure of graphene, it maintains the inherent performance characteristics of graphene, but the dispersion effect is slightly inferior to covalent bonding, and generally requires the addition of stabilizers or ultrasonic dispersion, and the energy consumption is relatively high, and the production cost is also high. The present invention is covalently bonded by octadecylamine, which is through the destruction of the π bond structure on the surface of graphene oxide, so that its surface is activated, and the interface bonding strength is enhanced. Octadecylamine, as a powerful adhesive, can not only provide strong adhesion between inorganic nanofillers and organic matrix, but also can weaken the van der Waals force between graphene oxide nanosheets by the insertion of its molecular structure, thereby slowing down its aggregation in the organic matrix, and promoting its uniform dispersion in the matrix.
[0029] Compared with the prior art, the present invention has the following advantages and technical effects:
[0030] 1. The present invention prepares graphene oxide sheets into graphene oxide aqueous dispersions, and utilizes the cavitation and mechanical effects of ultrasound to enable the graphene oxide to have good water dispersibility and stability during the functionalization process. The preparation method is simple, safe, economical, easy to control, and highly repeatable.
[0031] 2. The present invention functionalizes graphene oxide by using a long-chain amine such as octadecylamine, and utilizes the presence of long-arm amino groups to cause GO layers to separate, providing larger channels between layers, thereby promoting heat transfer and being more conducive to coating curing in practical applications.
[0032] 3. The present invention utilizes a longer-arm amine precursor as a modifier, which greatly increases the attachment of amino groups. On the one hand, it has a greater accelerating effect on the cross-linking reaction and promotes the formation of a cross-linking network; on the other hand, more amino groups improve the dispersion state of graphene oxide nanosheets in the resin matrix.
[0033] 4. The present invention makes full use of the abundant oxygen-containing functional groups on the surface of graphene oxide. Due to this characteristic of graphene oxide, it is easy to be functionalized by organic molecules. The present invention uses octadecylamine and N,N-dimethylformamide to form amide covalent bonds between the amino groups on the N,N-dimethylformamide molecular chain and the carboxyl groups on the edge of graphene oxide to produce chemical crosslinking. At the same time, the amino groups of octadecylamine are attached to the surface of graphene oxide and combined with graphene oxide through the action of chemical bonds to prepare a large number of active sites available for reaction.
[0034] 5. The functionalized graphene oxide of the present invention does not contain heavy metal components, has a wider range of applications, is more practical, has fewer preparation steps, a simple process flow, and low equipment requirements. It can significantly shorten the process time, reduce the cost of raw materials and equipment, and is suitable for large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] The drawings constituting a part of the present application are used to provide a further understanding of the present application. The illustrative embodiments and descriptions of the present application are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:
[0036] Figure 1 The present invention is a flow chart of the preparation process of functionalized graphene oxide for wear-resistant coating.
[0037] Figure 2 Scanning electron microscope images of the functionalized graphene oxide for wear-resistant coating prepared in Example 1 at different magnifications.
[0038] Figure 3 Raman spectra of the functionalized graphene oxide for wear-resistant coating prepared in Example 1 and the raw graphene oxide (i.e., the graphene oxide sheet in Example 1).
[0039] Figure 4 This is the infrared spectrum of the functionalized graphene oxide for wear-resistant coating prepared in Example 1.
[0040] Figure 5XPS spectra of the functionalized graphene oxide for wear-resistant coating prepared in Example 1 and the raw graphene oxide (i.e., the graphene oxide sheet in Example 1).
[0041] Figure 6 The wear peak areas of pure EP coating (a) and RGO-EDA / EP composite coating (b) are shown. DETAILED DESCRIPTION
[0042] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0043] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0044] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.
[0045] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present invention description and examples are exemplary only.
[0046] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.
[0047] In the present invention, unless otherwise specified, normal temperature is 25±2°C.
[0048] All raw materials used in the present invention are commercially available. As an example, graphene oxide sheets are purchased from Shanghai Aladdin Biochemical Technology Co., Ltd. (the sheet diameter is 1-50 μm and the thickness is 0.5-2 nm).
[0049] The process flow chart of the preparation of functionalized graphene oxide for wear-resistant coating of the present invention is shown in Figure 1 .
[0050] The technical solution of the present invention is further illustrated by the following embodiments.
[0051] Example 1
[0052] In a buffer system of pH = 7 (distilled water at room temperature, the same below), graphene oxide sheets (GO) with a sheet diameter of 1-50 μm and a thickness of 0.5-2 nm were selected and added to distilled water, and ultrasonicated for 1 h in an ice bath with an ultrasonic power of 130 w to obtain a graphene oxide aqueous dispersion with a concentration of 10 mg / mL. 1 g of the above-mentioned graphene oxide aqueous dispersion was mixed with 27 g of N, N-dimethylformamide (i.e., the mass ratio of the graphene oxide aqueous dispersion to N, N-dimethylformamide was 1:27), and the intermediate product A was obtained after stirring in an ice bath for 30 minutes. The intermediate product A was magnetically stirred, and 4.3 g of octadecylamine was slowly added (i.e., the mass ratio of octadecylamine to the graphene oxide aqueous dispersion was 4.3:1). After magnetic stirring at 30° C. for 2 hours, the intermediate product B was obtained. After separation and purification of the intermediate product B, it was ultrasonicated at a power of 150 W for 2 hours, the pH was adjusted to 7.5, and after centrifugation at a speed of 7000 r / min for 10 minutes, the precipitate was collected and vacuum dried to obtain amino-functionalized graphene oxide (functionalized GO) for wear-resistant coating, which was in a powder state.
[0053] Example 2
[0054] In a buffer system of pH=7, graphene oxide sheets with a sheet diameter of 1-50 μm and a thickness of 0.5-2 nm were selected and added to distilled water, and ultrasonicated for 1 h in an ice bath with an ultrasonic power of 120 w to obtain a graphene oxide aqueous dispersion with a concentration of 10 mg / mL. 1 g of the above-mentioned graphene oxide aqueous dispersion was mixed with 27 g of N,N-dimethylformamide (i.e., the mass ratio of the graphene oxide aqueous dispersion to N,N-dimethylformamide was 1:27), and the intermediate product A was obtained after stirring in an ice bath for 30 minutes. The intermediate product A was magnetically stirred, and 6.5 g of octadecylamine was slowly added (i.e., the mass ratio of octadecylamine to the graphene oxide aqueous dispersion was 6.5:1). The intermediate product B was obtained after magnetic stirring at 50°C for 2 hours. The intermediate product B was separated and purified, and then ultrasonicated at a power of 130 W for 3 hours, the pH was adjusted to 7.5, and the precipitate was collected and vacuum dried after centrifugation at a speed of 6500 r / min for 15 minutes to obtain amino-functionalized graphene oxide for wear-resistant coating.
[0055] Example 3
[0056] In a buffer system of pH=7, graphene oxide sheets with a sheet diameter of 1-50 μm and a thickness of 0.5-2 nm are selected and added to distilled water, and ultrasonicated in an ice bath for 1 hour at an ultrasonic power of 150 W to obtain a graphene oxide aqueous dispersion with a concentration of 10 mg / mL. 1 g of the above graphene oxide aqueous dispersion is mixed with 27 g of N, N-dimethylformamide (i.e., the mass ratio of graphene oxide aqueous dispersion to N, N-dimethylformamide is 1:27), and stirred in an ice bath for 30 minutes to obtain an intermediate product A, and the intermediate product A is magnetically stirred, and 9 g of octadecylamine is slowly added at the same time (i.e., the mass ratio of octadecylamine to graphene oxide aqueous dispersion is 9:1), and magnetically stirred at 80°C for 2 hours to obtain an intermediate product B, and the intermediate product B is separated and purified, and ultrasonicated at a power of 120 W for 4 hours, the pH is adjusted to 7.5, and after centrifugation at a speed of 6000 r / min for 20 minutes, the precipitate is collected and vacuum dried to obtain amino-functionalized graphene oxide for wear-resistant coating.
[0057] Comparative Example 1
[0058] Same as Example 1, except that the graphene oxide aqueous dispersion is replaced by an equal mass of graphene oxide powder (passed through a 60-mesh sieve).
[0059] Since the graphene oxide powder has not undergone ultrasonic treatment to become an aqueous dispersion, it agglomerates severely in the resin matrix when preparing wear-resistant coatings. The powder dispersibility is not as good as that of the graphene oxide aqueous dispersion, resulting in poor overall performance of the functionalized graphene oxide.
[0060] Comparative Example 2
[0061] The preparation method of graphene oxide aqueous dispersion is the same as that in Example 1. The graphene oxide aqueous dispersion, octadecylamine and N,N-dimethylformamide are mixed in a mass ratio of 1:4.3:27 (the mixing method is the same as that in Example 1), and magnetically stirred at 30°C for 1 hour. After stirring evenly, ultrasonic treatment is performed for 2 hours, and then filtration is performed. During the filtration, the precipitate is washed alternately with alcohol and distilled water for 3 times. After the filtration is completed, the precipitate is collected and vacuum dried at 70°C for 36 hours to obtain amino-functionalized graphene oxide.
[0062] Comparative Example 3
[0063] The preparation method of graphene oxide aqueous dispersion is the same as that in Example 2. The graphene oxide aqueous dispersion, octadecylamine and N,N-dimethylformamide are mixed in a mass ratio of 1:6.5:27 (the mixing method is the same as that in Example 2), and magnetically stirred at 30°C for 1 hour. After stirring evenly, ultrasonic treatment is performed for 2 hours, and then filtration is performed. During the filtration, the precipitate is washed alternately with alcohol and distilled water for 3 times. After the filtration is completed, the precipitate is collected and vacuum dried at 70°C for 36 hours to obtain amino-functionalized graphene oxide.
[0064] Comparative Example 4
[0065] The preparation method of the graphene oxide aqueous dispersion is the same as that in Example 3. The graphene oxide aqueous dispersion, octadecylamine, and N,N-dimethylformamide are mixed in a mass ratio of 1:9:27 (the mixing method is the same as in Example 3), and magnetically stirred at 30°C for 1 hour. After stirring evenly, ultrasonic treatment is performed for 2 hours, and then filtration is performed. During the filtration, the precipitate is washed alternately with alcohol and distilled water for 3 times. After the filtration is completed, the precipitate is collected and vacuum dried at 70°C for 36 hours to obtain amino-functionalized graphene oxide.
[0066] In Comparative Examples 2 to 4, impurities are easily mixed in due to insufficient stirring time and insufficient suction filtration and washing, resulting in a decrease in the comprehensive performance of the functionalized graphene oxide.
[0067] Comparative Example 5
[0068] Same as Example 1, except that octadecylamine is replaced with ethylenediamine of equal mass. Due to the length of the amino chain, the functionalized product occupies a dominant position in the dispersed state in the organic matrix. Therefore, compared with the long-chain octadecylamine functionalized graphene oxide, the activation energy of the short-chain ethylenediamine functionalized graphene oxide is lower, resulting in its weak promotion effect on the network formation in the nanocomposite material, which makes the ethylenediamine functionalized graphene oxide less effective in practical applications.
[0069] Effect Example 1
[0070] The scanning electron microscope image of the functionalized graphene oxide for wear-resistant coating prepared in Example 1 is as follows: Figure 2 As shown in the figure, the surface of the functionalized graphene oxide for wear-resistant coating prepared in Example 1 shows obvious shrinkage, with bud-like structures protruding from the surface and full of gaps, indicating that the grafting of amino groups has significantly enhanced the surface dispersibility of the functionalized graphene oxide. At the same time, these structural features also suggest that the functionalized GO surface may have more surface sites available for reaction. The Raman spectra of the functionalized graphene oxide for wear-resistant coating prepared in Example 1 and the raw graphene oxide (i.e., the graphene oxide sheet in Example 1) are shown in Figure 1. Figure 3 , the structural changes of the two carbon-like materials can be further observed. The spectra of GO and functionalized graphene oxide are at 1350 cm -1 and 1580cm -1 There are two prominent peaks at 1350cm -1 and 1580cm -1The characteristic peaks at 100 nm and 100 nm became wider, and their ID / IG values increased from 0.80 of unmodified GO to 0.93. This is because more defects are introduced between the graphene oxide layers after modification. With the formation of surface functional groups or the introduction of active polar groups such as NH, the charge distribution between GO molecules is uneven, resulting in electrostatic forces between them, thereby increasing polarity, confirming that octadecylamine was successfully grafted onto graphene oxide. The infrared spectrum of the functionalized graphene oxide for wear-resistant coating prepared in Example 1 is shown in Figure 2. Figure 4 As shown, in functionalized GO, at 720 cm -1 Nearby and 2985cm -1 A NH group peak was detected at 1460 cm -1 The peak at 1648 cm indicates that it produces CN stretching. -1 The XPS spectra of the functionalized graphene oxide for wear-resistant coating prepared in Example 1 and the raw graphene oxide (i.e., the graphene oxide sheet in Example 1) are shown in FIG. Figure 5 As shown in the figure, an N1s peak appeared in the functionalized GO graph, indicating that the amino group was successfully grafted onto the graphene oxide, which is consistent with the above results. The above results all show that octadecylamine reacted with graphene oxide and successfully introduced highly active amino functional groups.
[0071] Effect Example 2
[0072] The amino-functionalized graphene oxide prepared in the above examples and comparative examples is applied to wear-resistant paint / wear-resistant coating, specifically comprising:
[0073] 1) mixing N,N-dimethylformamide, xylene and acetone in a mass ratio of 6:1:3 to obtain an intermediate solvent;
[0074] 2) adding epoxy resin to the intermediate solvent, stirring with a mechanical stirrer for 30 min until fully mixed, to obtain epoxy resin emulsion, adding curing agent polyamide to the epoxy resin emulsion and magnetically stirring for 30 min until the epoxy resin and the curing agent are completely dissolved, to obtain a mixed emulsion;
[0075] 3) adding the amino-functionalized graphene oxide prepared in each embodiment and each comparative example to N,N-dimethylformamide to obtain a mixed solution (the amino-functionalized graphene oxide accounts for 1 wt.% of the total mass of the mixed solution), and ultrasonicating at an ultrasonic power of 150 W for 30 min to obtain an amino-functionalized graphene oxide dispersion;
[0076] 4) adding the amino-functionalized graphene oxide dispersion to the mixed emulsion and magnetically stirring for 2 h, then ultrasonicating for 2 h at a power of 150 W, and drying for 28 h until it becomes viscous to obtain a wear-resistant coating;
[0077] 5) The wear-resistant coating was evenly coated on the martensitic stainless steel substrate using a wire rod coater, and the wear-resistant coating was obtained after curing. The tribological properties were tested using a UMT-3 friction and wear tester.
[0078] The tribological performance results are as follows:
[0079] like Figure 6 As shown in the figure, with the addition of amino-functionalized graphene oxide, the area of the wear peak is significantly reduced, because the amino groups on the surface covalently bond the functionalized graphene oxide and the epoxy groups of the epoxy resin, making the amino-functionalized graphene oxide have high strength and high epoxy resin matrix interface bonding force. As the wear intensifies, when the microcracks inside the coating extend to the vicinity of the well-dispersed functionalized graphene oxide, the functionalized graphene oxide embedded in the resin matrix will deflect the crack path, absorb energy, and prevent the further expansion of the microcracks. At the same time, the functionalized graphene oxide forms a continuous and stable transfer film during the sliding process, avoiding direct contact with the coupling surface, producing a lubricating effect, and ultimately improving the wear resistance of the composite coating.
[0080] The above are only preferred specific implementations of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.
Claims
1. A method for preparing amino-functionalized graphene oxide for wear-resistant coating, characterized in that: The following steps are involved: The graphene oxide aqueous dispersion is mixed with N,N-dimethylformamide, and stirred in an ice bath to obtain an intermediate product A; The intermediate product A is subjected to magnetic stirring, and octadecylamine is added at the same time, and the intermediate product B is obtained after magnetic stirring; The intermediate product B is separated and purified, then subjected to ultrasound, the pH is adjusted to alkaline, and after centrifugal separation and purification, the precipitate is collected and vacuum dried to obtain the amino-functionalized graphene oxide for wear-resistant coating.
2. The method for preparing amino-functionalized graphene oxide for wear-resistant coating according to claim 1, characterized in that: The mass ratio of the graphene oxide aqueous dispersion to N,N-dimethylformamide is 1:
27.
3. The method for preparing amino-functionalized graphene oxide for wear-resistant coating according to claim 2, characterized in that: The preparation method of the graphene oxide aqueous dispersion is as follows: in a buffer system with pH=7, graphene oxide sheets with a sheet diameter of 1-50 μm and a thickness of 0.5-2 nm are selected and added to the buffer system, and ultrasonicated in an ice bath for 1 hour with an ultrasonic power of 120-150 w to obtain the graphene oxide aqueous dispersion.
4. The method for preparing amino-functionalized graphene oxide for wear-resistant coating according to claim 1, characterized in that: The mass ratio of the octadecylamine to the graphene oxide aqueous dispersion is (4-9):
1.
5. The method for preparing amino-functionalized graphene oxide for wear-resistant coating according to claim 1, characterized in that: The step of adjusting the pH to alkaline is adjusting the pH to 7.
5.
6. The method for preparing amino-functionalized graphene oxide for wear-resistant coating according to claim 1, characterized in that: The power of the ultrasound is 120-150w, and the time of the ultrasound is 2-4h; The centrifugal speed is 6000-7000 r / min, and the centrifugal time is 10-20 min.
7. An amino-functionalized graphene oxide for wear-resistant coating, characterized in that: Prepared according to the method according to any one of claims 1 to 6.
8. A wear-resistant coating, characterized in that: Containing the amino-functionalized graphene oxide for wear-resistant coating as claimed in claim 7.
9. Use of the amino-functionalized graphene oxide according to claim 7 in the preparation of wear-resistant coatings.
10. Use of the amino-functionalized graphene oxide according to claim 7 in preparing a wear-resistant coating.
Citation Information
Cited By
Graphene wear-resistant anticorrosive paint and preparation method thereof
CN120399517A