Acrylate pressure-sensitive adhesive tape for fixing battery and preparation method of acrylate pressure-sensitive adhesive tape
By designing the three-layer structure of acrylate pressure-sensitive tape and a specific UV adhesive layer formula, the problem of light penetration and curing time of blue film tape during UV curing is solved, and high-intensity, heat resistance and flexibility tape is achieved , suitable for battery fixation, improving the fixing quality of the battery module.
Patent Information
- Application Number
- CN202411471189.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-22
- Publication Date
- 2024-11-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing blue film tape has light penetration problems during UV curing, which leads to inability to cure effectively, or the curing time is too long to affect the adhesion performance and affect the fixing quality of the battery module.
Using a three-layer structure design of acrylate pressure-sensitive adhesive tape, including release film, UV glue layer and substrate, using specific formula UV glue layer raw materials such as methyl methacrylate,-2-hydroxyethyl acrylate, and epoxy Acrylates, tackifying resins, reactive diluents and photoinitiators achieve delayed curing through back irradiation, and the glue layer initiation is completed after moderate irradiation, which is suitable for battery fixation.
It improves the peel strength, shear strength and heat resistance of the tape, reduces the risk of brittle fracture, enhances the adhesive performance and flexibility, extends storage stability, is suitable for battery fixation, and improves the fixing quality of the battery module.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of adhesive tapes, and more particularly to an acrylic pressure-sensitive adhesive tape for battery fixing and a preparation method thereof. Background Art
[0002] With the rapid development of new energy vehicles and electric equipment industries, the demand for power batteries has increased dramatically. As an important material for battery insulation and fixed protection, the market demand for blue film tape will continue to grow. The blue film has excellent insulation properties and can effectively isolate the battery cells to prevent the failure of a single battery cell from causing a chain reaction in other battery cells. In addition, the blue film also has excellent chemical resistance and shear strength, which can adapt to the use requirements of power batteries in various complex environments. It also has the characteristics of direct bonding and convenient operation, which can improve the production efficiency of power batteries. In the production process of power batteries, coating with blue film is one of the key processes. Traditional blue film tapes generally use modified acrylic PSA as resin. Although it has good adhesion and shear strength, it is easy to generate bubbles or mix with moisture in actual applications. These defects not only affect the pass rate of power batteries, but also may cause leakage risks in battery modules.
[0003] UV tackifier refers to a material that can quickly cure and form an adhesive layer under LED irradiation. It has the material properties of traditional PSA and is endowed with UV tackifier function, achieving excellent adhesion, heavy workability and stability of the product. It is widely used in battery fixation, optics, electronics and packaging. As the requirements of new energy vehicles for endurance and charging speed continue to increase, the market has higher and higher requirements for the insulation performance and voltage resistance of battery materials. Traditional PSA blue film tapes are gradually replaced by UV tackifier blue film tapes. Existing UV tackifiers are of free radical, cationic and anionic types. Although they can provide good physical properties under certain conditions, they all have their own limitations. For example, free radical UV tackifiers are prone to oxygen inhibition during the curing process, have large volume shrinkage, and have requirements for the light transmittance of the substrate; cationic and anionic UV tackifiers are sensitive to water vapor and alkaline substances and have poor storage stability. In addition, due to its deep blue color, if the blue film tape is irradiated from the front, light cannot penetrate and effective UV curing cannot be achieved; if the back is irradiated, the irradiation time is short and effective UV curing cannot be achieved. If the irradiation time is too long, the adhesive layer will harden, affecting the adhesive performance and the subsequent fixation quality of the battery module. Based on the above statements, the present invention proposes an acrylic pressure-sensitive tape for battery fixation and a preparation method thereof. Summary of the invention
[0004] In order to solve the problems that the existing blue film tape adopts front irradiation, light cannot penetrate and effective UV curing cannot be achieved; if back irradiation is adopted, the irradiation time is short and effective UV curing cannot be achieved, and too long irradiation time will lead to hardening of the adhesive layer and affect the adhesive performance, the present invention provides an acrylic pressure-sensitive tape for battery fixing and a preparation method thereof.
[0005] In a first aspect, the present invention provides an acrylic pressure-sensitive adhesive tape for battery fixing, which adopts the following technical solution: An acrylic pressure-sensitive adhesive tape for battery fixing comprises a three-layer structure of a release film, a UV adhesive layer and a substrate from the outside to the inside; the UV adhesive layer comprises the following raw materials in parts by weight: 45-55 parts of methyl methacrylate, 22-28 parts of 2-hydroxyethyl acrylate, 20-26 parts of epoxy acrylate, 14-18 parts of styrene, 10-15 parts of tackifying resin, 16-20 parts of active diluent, 5-12 parts of filler and 4-10 parts of photoinitiator.
[0006] Preferably, the mass ratio of methyl methacrylate, 2-hydroxyethyl acrylate, epoxy acrylate and styrene is 3:1.5:1.5:1.
[0007] Preferably, the UV adhesive layer comprises the following raw materials in parts by weight: 48 parts of methyl methacrylate, 24 parts of 2-hydroxyethyl acrylate, 24 parts of epoxy acrylate, 16 parts of styrene, 12 parts of tackifying resin, 18 parts of active diluent, 8 parts of filler, and 7 parts of photoinitiator.
[0008] Preferably, the tackifying resin is prepared by the following method: Add melamine and solvent into a dry reaction kettle, heat to 50-60°C, stir for 30-60 minutes until dissolved, keep stirring, add toluene diisocyanate and tetramethyl meta-xylylene diisocyanate into the reaction kettle, stir and react for 1-2 hours, add dehydroabietic acid, epichlorohydrin and dibutyltin oxide, heat the reaction system to 70-80°C, continue to keep warm and stir and react for 2-4 hours to obtain the desired tackifying resin.
[0009] Preferably, the tackifying resin contains the following raw materials in specific weight parts: 18-25 parts of melamine, 15-20 parts of toluene diisocyanate, 8-12 parts of tetramethyl meta-xylylene diisocyanate, 15-25 parts of dehydroabietic acid, 5-12 parts of epichlorohydrin, 0.1-0.5 parts of dibutyltin oxide, and 30-40 parts of solvent.
[0010] Preferably, the tackifying resin contains the following raw materials in specific weight parts: 22 parts of melamine, 18 parts of toluene diisocyanate, 10 parts of tetramethyl meta-xylylene diisocyanate, 20 parts of dehydroabietic acid, 8 parts of epichlorohydrin, 0.3 parts of dibutyltin oxide, and 35 parts of solvent.
[0011] Preferably, the reactive diluent comprises o-cresyl glycidyl ether and triethylene glycol divinyl ether in a mass ratio of 7-9:1-2.
[0012] Preferably, the filler is at least one of nano-silicon dioxide, nano-talc powder, nano-mica powder and nano-quartz powder.
[0013] Preferably, the photoinitiator comprises photoinitiator 907 and photoinitiator UVI-6976 in a mass ratio of 3-5:1.
[0014] In a second aspect, the present invention provides a method for preparing an acrylic pressure-sensitive adhesive tape for battery fixing, which adopts the following technical scheme: A method for preparing an acrylic pressure-sensitive adhesive tape for battery fixing comprises the following steps: S1. Weigh the raw materials of UV adhesive layer, methyl methacrylate, 2-hydroxyethyl acrylate, epoxy acrylate, styrene, tackifying resin, reactive diluent, filler, and photoinitiator, and mix them evenly to obtain a mixed adhesive; S2, firstly coating the mixed adhesive on the substrate to form a UV adhesive layer, and then attaching a release film to the other side of the UV adhesive layer to obtain a semi-finished product; S3. Bake the semi-finished product at 80-90° C. for 5-10 minutes to form the required acrylic pressure-sensitive tape for battery fixing.
[0015] In summary, the present invention has the following beneficial effects: 1. The present invention adopts methyl methacrylate and 2-hydroxyethyl acrylate as matrix monomers to provide initial strength and operability; epoxy acrylate and styrene are added to be fully compatible with the main matrix monomers, provide UV activity, and enhance the heat resistance and chemical stability of the pressure-sensitive adhesive tape; the addition of tackifying resin improves the initial tack and lasting tack of the pressure-sensitive adhesive and improves its adhesion performance; the addition of active diluent can not only adjust the viscosity of the pressure-sensitive adhesive, improve fluidity and coating performance, but also participate in polymerization reaction, and improve the comprehensive performance of the final pressure-sensitive adhesive; fillers can further increase mechanical strength, heat resistance and corrosion resistance; the pressure-sensitive adhesive tape prepared by the present invention has high peeling strength and shear strength, and has excellent heat resistance, water resistance, chemical solvent resistance and corrosion resistance, and has broad market prospects.
[0016] 2. The tackifying resin prepared by the present invention can significantly enhance the network density inside the pressure-sensitive adhesive, improve the cohesive force, and thus enhance the bonding performance and flexibility of the pressure-sensitive adhesive tape, reduce the risk of brittle fracture, and avoid the residual problem of the pressure-sensitive adhesive after peeling; wherein, toluene diisocyanate and tetramethyl meta-xylylene diisocyanate have different reactivities and viscosities, and their common use can regulate the reaction rate and the final chain structure, thereby improving the crosslinking degree and strength of the tackifying resin; dehydroabietic acid has high heat resistance, and can improve the toughness and adhesion of the tackifying resin, so that the final product is not easy to break under stress; epichlorohydrin, as an epoxy compound, can undergo a crosslinking reaction with isocyanate, thereby improving the heat resistance, chemical resistance, solvent resistance and mechanical properties of the tackifying resin, and is suitable for a variety of harsh environments.
[0017] 3. The present invention uses o-cresyl glycidyl ether and triethylene glycol divinyl ether as active diluents, which can reduce the viscosity of UV adhesive, improve fluidity, and thus improve coating performance; on the other hand, they can participate in the reaction during the curing process, enhance the crosslinking density of UV adhesive, and increase the heat resistance, water resistance, and chemical resistance of the final UV adhesive material. By controlling the combined ratio of the two, the reaction rate and time during the curing process can be adjusted to achieve the effect of delayed curing after irradiation, and improve the flexibility, bonding strength, and chemical resistance of the pressure-sensitive tape.
[0018] 4. The present invention uses a mixture of photoinitiator 907 and photoinitiator UVI-6976 as photoinitiators. During the UV curing process, both of them will undergo polymerization reaction. By controlling the mass ratio of the two, it is possible to control the curing rate to a certain extent and regulate the UV curing process. The synergistic effect between different initiators can also improve the mechanical strength, chemical resistance, heat resistance and other properties of the obtained pressure-sensitive adhesive; in addition, the mixed use can improve the storage stability of the pressure-sensitive adhesive and reduce the degradation or failure of the initiator during storage.
[0019] 5. The acrylic pressure-sensitive tape for battery fixation proposed in the present invention can achieve the effect of delayed curing by not initiating a reaction or only partially reacting after back irradiation through formula design. Before being used for battery fixation and winding, it only needs to be moderately irradiated to stimulate the adhesive layer to produce an initiator. After winding, a dark reaction can be carried out, that is, the curing is completed over time. The pressure-sensitive tape of the present invention can be better used for battery fixation and improve the fixing quality of the battery module. DETAILED DESCRIPTION
[0020] The present invention is further described in detail below with reference to the embodiments.
[0021] Unless otherwise specified, the materials, reagents, etc. used in the present invention can be obtained from commercial sources.
[0022] Preparation Examples 1-3 and Comparative Preparation Examples 1-4 provide methods for preparing tackifying resins.
[0023] Preparation Example 1: The tackifying resin is prepared by the following method: The tackifying resin contains the following raw materials in specific weight parts: 18 parts of melamine, 15 parts of toluene-2,4-diisocyanate, 8 parts of tetramethyl meta-xylylene diisocyanate, 15 parts of dehydroabietic acid, 5 parts of epichlorohydrin, 0.1 parts of dibutyltin oxide, and 30 parts of anhydrous ethanol; Add melamine and anhydrous ethanol into a dry reactor, heat to 50°C, stir at 400 r / min for 60 min until dissolved, keep stirring, add toluene-2,4-diisocyanate and tetramethyl meta-xylylene diisocyanate into the reactor, stir and react for 1 h, add dehydroabietic acid, epichlorohydrin and dibutyltin oxide, heat the reaction system to 70°C, continue to keep warm and stir for 4 h to obtain the desired tackifying resin.
[0024] Preparation Example 2: The tackifying resin is prepared by the following method: The tackifying resin contains the following raw materials in specific weight parts: 22 parts of melamine, 18 parts of toluene-2,4-diisocyanate, 10 parts of tetramethyl meta-xylylene diisocyanate, 20 parts of dehydroabietic acid, 8 parts of epichlorohydrin, 0.3 parts of dibutyltin oxide, and 35 parts of anhydrous ethanol; Add melamine and anhydrous ethanol into a dry reactor, heat to 55°C, stir at 500 r / min for 45 min until dissolved, keep stirring, add toluene-2,4-diisocyanate and tetramethyl-m-xylylene diisocyanate into the reactor, stir and react for 1.5 h, add dehydroabietic acid, epichlorohydrin and dibutyltin oxide, heat the reaction system to 75°C, continue to keep warm and stir and react for 3 h to obtain the desired tackifying resin.
[0025] Preparation Example 3: The tackifying resin is prepared by the following method: The tackifying resin contains the following raw materials in specific weight parts: 25 parts of melamine, 20 parts of toluene-2,4-diisocyanate, 12 parts of tetramethyl meta-xylylene diisocyanate, 25 parts of dehydroabietic acid, 12 parts of epichlorohydrin, 0.5 parts of dibutyltin oxide, and 40 parts of anhydrous ethanol; Add melamine and anhydrous ethanol into a dry reactor, heat to 60°C, stir at 600 r / min for 30 min until dissolved, keep stirring, add toluene-2,4-diisocyanate and tetramethyl meta-xylylene diisocyanate into the reactor, stir and react for 2 h, add dehydroabietic acid, epichlorohydrin and dibutyltin oxide, heat the reaction system to 80°C, continue to keep warm and stir and react for 2 h to obtain the desired tackifying resin.
[0026] Comparative Preparation Example 1: The tackifying resin is prepared by the following method: The tackifying resin contains the following raw materials in specific weight parts: 18 parts of melamine, 23 parts of toluene-2,4-diisocyanate, 15 parts of dehydroabietic acid, 5 parts of epichlorohydrin, 0.1 parts of dibutyltin oxide, and 30 parts of anhydrous ethanol; Add melamine and anhydrous ethanol into a dry reactor, heat to 50°C, stir at 400 r / min for 60 min until dissolved, keep stirring, add toluene-2,4-diisocyanate into the reactor, stir and react for 1 h, add dehydroabietic acid, epichlorohydrin and dibutyltin oxide, heat the reaction system to 70°C, continue to keep warm and stir and react for 4 h to obtain the desired tackifying resin.
[0027] Comparative Preparation Example 2: The tackifying resin is prepared by the following method: The tackifying resin contains the following raw materials in specific weight parts: 18 parts of melamine, 23 parts of tetramethyl meta-xylylene diisocyanate, 15 parts of dehydroabietic acid, 5 parts of epichlorohydrin, 0.1 parts of dibutyltin oxide, and 30 parts of anhydrous ethanol; Add melamine and anhydrous ethanol into a dry reactor, heat to 50°C, stir at 400 r / min for 60 min until dissolved, keep stirring, add tetramethyl meta-xylylene diisocyanate into the reactor, stir and react for 1 h, add dehydroabietic acid, epichlorohydrin and dibutyltin oxide, heat the reaction system to 70°C, continue to keep warm and stir and react for 4 h to obtain the desired tackifying resin.
[0028] Comparative Preparation Example 3: The tackifying resin is prepared by the following method: The tackifying resin contains the following raw materials in specific weight parts: 18 parts of melamine, 15 parts of toluene-2,4-diisocyanate, 8 parts of tetramethyl-m-xylylene diisocyanate, 5 parts of epichlorohydrin, 0.1 parts of dibutyltin oxide, and 30 parts of anhydrous ethanol; Add melamine and anhydrous ethanol into a dry reactor, heat to 50°C, stir at 400 r / min for 60 min until dissolved, keep stirring, add toluene-2,4-diisocyanate and tetramethyl-m-xylylene diisocyanate into the reactor, stir and react for 1 h, add epichlorohydrin and dibutyltin oxide, heat the reaction system to 70°C, continue to keep warm and stir and react for 4 h to obtain the desired tackifying resin.
[0029] Comparative Preparation Example 4: The tackifying resin is prepared by the following method: The tackifying resin contains the following raw materials in specific weight parts: 18 parts of melamine, 15 parts of toluene-2,4-diisocyanate, 8 parts of tetramethyl meta-xylylene diisocyanate, 15 parts of dehydroabietic acid, 0.1 parts of dibutyltin oxide, and 30 parts of anhydrous ethanol; Add melamine and anhydrous ethanol into a dry reactor, heat to 50°C, stir at 400 r / min for 60 min until dissolved, keep stirring, add toluene-2,4-diisocyanate and tetramethyl meta-xylylene diisocyanate into the reactor, stir and react for 1 h, add dehydroabietic acid and dibutyltin oxide, heat the reaction system to 70°C, continue to keep warm and stir and react for 4 h to obtain the desired tackifying resin.
[0030] Embodiments 1-4 provide an acrylic pressure-sensitive adhesive tape for battery fixing and a preparation method thereof.
[0031] Embodiment 1:
[0032] An acrylic pressure-sensitive adhesive tape for battery fixing, comprising a three-layer structure of a PET release film, a UV adhesive layer and a blue PVC substrate from the outside to the inside; wherein the UV adhesive layer comprises the following raw materials in parts by weight: 45 parts of methyl methacrylate, 22 parts of 2-hydroxyethyl acrylate, 20 parts of epoxy acrylate, 14 parts of styrene, 10 parts of tackifying resin, 16 parts of active diluent, 5 parts of filler, and 4 parts of photoinitiator; Among them, epoxy acrylate CAS No. 71281-65-7; tackifying resin is prepared by Preparation Example 1; active diluent includes o-cresyl glycidyl ether and triethylene glycol divinyl ether in a mass ratio of 7:1; filler is nano-scale silica; photoinitiator includes photoinitiator 907 and photoinitiator UVI-6976 in a mass ratio of 3:1.
[0033] A method for preparing an acrylic pressure-sensitive adhesive tape for battery fixing comprises the following steps: S1. Weigh the raw materials of UV adhesive layer, methyl methacrylate, 2-hydroxyethyl acrylate, epoxy acrylate, styrene, tackifying resin, reactive diluent, filler, and photoinitiator, and mix them evenly to obtain a mixed adhesive; S2, firstly coating the mixed adhesive on the blue PVC to form a UV adhesive layer, and then laminating the PET release film on the other side of the UV adhesive layer to obtain a semi-finished product; S3. Bake the semi-finished product at 80° C. for 10 minutes to form the required acrylic pressure-sensitive tape for battery fixing.
[0034] Embodiment 2:
[0035] An acrylic pressure-sensitive adhesive tape for battery fixing, comprising a three-layer structure of a PET release film, a UV adhesive layer and a blue PVC substrate from the outside to the inside; wherein the UV adhesive layer comprises the following raw materials in parts by weight: 48 parts of methyl methacrylate, 24 parts of 2-hydroxyethyl acrylate, 24 parts of epoxy acrylate, 16 parts of styrene, 12 parts of tackifying resin, 18 parts of active diluent, 8 parts of filler, and 7 parts of photoinitiator; Among them, epoxy acrylate CAS No. 71281-65-7; tackifying resin is prepared by Preparation Example 2; active diluent includes o-cresyl glycidyl ether and triethylene glycol divinyl ether in a mass ratio of 8:1.5; filler is nano-scale silica; photoinitiator includes photoinitiator 907 and photoinitiator UVI-6976 in a mass ratio of 4:1.
[0036] A method for preparing an acrylic pressure-sensitive adhesive tape for battery fixing comprises the following steps: S1. Weigh the raw materials of UV adhesive layer, methyl methacrylate, 2-hydroxyethyl acrylate, epoxy acrylate, styrene, tackifying resin, reactive diluent, filler, and photoinitiator, and mix them evenly to obtain a mixed adhesive; S2, firstly coating the mixed adhesive on the blue PVC to form a UV adhesive layer, and then laminating the PET release film on the other side of the UV adhesive layer to obtain a semi-finished product; S3. Bake the semi-finished product at 85° C. for 8 minutes to form the required acrylic pressure-sensitive tape for battery fixing.
[0037] Embodiment 3:
[0038] An acrylic pressure-sensitive adhesive tape for battery fixing, comprising a three-layer structure of a PET release film, a UV adhesive layer and a blue PVC substrate from the outside to the inside; wherein the UV adhesive layer comprises the following raw materials in parts by weight: 55 parts of methyl methacrylate, 28 parts of 2-hydroxyethyl acrylate, 26 parts of epoxy acrylate, 18 parts of styrene, 15 parts of tackifying resin, 20 parts of active diluent, 12 parts of filler, and 10 parts of photoinitiator; Among them, epoxy acrylate CAS No. 71281-65-7; tackifying resin is prepared by Preparation Example 3; active diluent includes o-cresyl glycidyl ether and triethylene glycol divinyl ether in a mass ratio of 9:2; filler is nano-scale silica; photoinitiator includes photoinitiator 907 and photoinitiator UVI-6976 in a mass ratio of 5:1.
[0039] A method for preparing an acrylic pressure-sensitive adhesive tape for battery fixing comprises the following steps: S1. Weigh the raw materials of UV adhesive layer, methyl methacrylate, 2-hydroxyethyl acrylate, epoxy acrylate, styrene, tackifying resin, reactive diluent, filler, and photoinitiator, and mix them evenly to obtain a mixed adhesive; S2, firstly coating the mixed adhesive on the blue PVC to form a UV adhesive layer, and then laminating the PET release film on the other side of the UV adhesive layer to obtain a semi-finished product; S3. Bake the semi-finished product at 90° C. for 5 minutes to form the required acrylic pressure-sensitive tape for battery fixing.
[0040] Embodiment 4:
[0041] An acrylic pressure-sensitive adhesive tape for battery fixing, comprising a three-layer structure of a PET release film, a UV adhesive layer and a blue PVC substrate from the outside to the inside; wherein the UV adhesive layer comprises the following raw materials in parts by weight: 50 parts of methyl methacrylate, 22 parts of 2-hydroxyethyl acrylate, 26 parts of epoxy acrylate, 14 parts of styrene, 12 parts of tackifying resin, 18 parts of active diluent, 8 parts of filler, and 7 parts of photoinitiator; Among them, epoxy acrylate CAS No. 71281-65-7; tackifying resin is prepared by Preparation Example 2; active diluent includes o-cresyl glycidyl ether and triethylene glycol divinyl ether in a mass ratio of 8:1.5; filler is nano-scale silica; photoinitiator includes photoinitiator 907 and photoinitiator UVI-6976 in a mass ratio of 4:1.
[0042] A method for preparing an acrylic pressure-sensitive adhesive tape for battery fixing comprises the following steps: S1. Weigh the raw materials of UV adhesive layer, methyl methacrylate, 2-hydroxyethyl acrylate, epoxy acrylate, styrene, tackifying resin, reactive diluent, filler, and photoinitiator, and mix them evenly to obtain a mixed adhesive; S2, firstly coating the mixed adhesive on the blue PVC to form a UV adhesive layer, and then laminating the PET release film on the other side of the UV adhesive layer to obtain a semi-finished product; S3. Bake the semi-finished product at 85° C. for 8 minutes to form the required acrylic pressure-sensitive tape for battery fixing.
[0043] In order to verify the performance of the acrylic pressure-sensitive adhesive tape for battery fixing obtained in Examples 1-4 of the present invention, the present invention set up Comparative Examples 1-8.
[0044] Comparative Example 1: Comparative Example 1 is different from Example 1 only in that the tackifying resin is prepared from Comparative Preparation Example 1, which is as follows: An acrylic pressure-sensitive adhesive tape for battery fixing, comprising a three-layer structure of a PET release film, a UV adhesive layer and a blue PVC substrate from the outside to the inside; wherein the UV adhesive layer comprises the following raw materials in parts by weight: 45 parts of methyl methacrylate, 22 parts of 2-hydroxyethyl acrylate, 20 parts of epoxy acrylate, 14 parts of styrene, 10 parts of tackifying resin, 16 parts of active diluent, 5 parts of filler, and 4 parts of photoinitiator; Among them, epoxy acrylate CAS No. 71281-65-7; tackifying resin is prepared by comparative preparation example 1; active diluent includes o-cresyl glycidyl ether and triethylene glycol divinyl ether in a mass ratio of 7:1; filler is nano-scale silica; photoinitiator includes photoinitiator 907 and photoinitiator UVI-6976 in a mass ratio of 3:1.
[0045] A method for preparing an acrylic pressure-sensitive adhesive tape for battery fixing comprises the following steps: S1. Weigh the raw materials of UV adhesive layer, methyl methacrylate, 2-hydroxyethyl acrylate, epoxy acrylate, styrene, tackifying resin, reactive diluent, filler, and photoinitiator, and mix them evenly to obtain a mixed adhesive; S2, firstly coating the mixed adhesive on the blue PVC to form a UV adhesive layer, and then laminating the PET release film on the other side of the UV adhesive layer to obtain a semi-finished product; S3. Bake the semi-finished product at 80° C. for 10 minutes to form the required acrylic pressure-sensitive tape for battery fixing.
[0046] Comparative Example 2: Comparative Example 2 is different from Example 1 only in that the tackifying resin is prepared from Comparative Preparation Example 2, which is as follows: An acrylic pressure-sensitive adhesive tape for battery fixing, comprising a three-layer structure of a PET release film, a UV adhesive layer and a blue PVC substrate from the outside to the inside; wherein the UV adhesive layer comprises the following raw materials in parts by weight: 45 parts of methyl methacrylate, 22 parts of 2-hydroxyethyl acrylate, 20 parts of epoxy acrylate, 14 parts of styrene, 10 parts of tackifying resin, 16 parts of active diluent, 5 parts of filler, and 4 parts of photoinitiator; Among them, epoxy acrylate CAS No. 71281-65-7; tackifying resin is prepared by comparative preparation example 2; active diluent includes o-cresyl glycidyl ether and triethylene glycol divinyl ether in a mass ratio of 7:1; filler is nano-scale silica; photoinitiator includes photoinitiator 907 and photoinitiator UVI-6976 in a mass ratio of 3:1.
[0047] A method for preparing an acrylic pressure-sensitive adhesive tape for battery fixing comprises the following steps: S1. Weigh the raw materials of UV adhesive layer, methyl methacrylate, 2-hydroxyethyl acrylate, epoxy acrylate, styrene, tackifying resin, reactive diluent, filler, and photoinitiator, and mix them evenly to obtain a mixed adhesive; S2, firstly coating the mixed adhesive on the blue PVC to form a UV adhesive layer, and then laminating the PET release film on the other side of the UV adhesive layer to obtain a semi-finished product; S3. Bake the semi-finished product at 80° C. for 10 minutes to form the required acrylic pressure-sensitive tape for battery fixing.
[0048] Comparative Example 3: Comparative Example 3 is different from Example 1 only in that the tackifying resin is prepared from Comparative Preparation Example 3, which is as follows: An acrylic pressure-sensitive adhesive tape for battery fixing, comprising a three-layer structure of a PET release film, a UV adhesive layer and a blue PVC substrate from the outside to the inside; wherein the UV adhesive layer comprises the following raw materials in parts by weight: 45 parts of methyl methacrylate, 22 parts of 2-hydroxyethyl acrylate, 20 parts of epoxy acrylate, 14 parts of styrene, 10 parts of tackifying resin, 16 parts of active diluent, 5 parts of filler, and 4 parts of photoinitiator; Among them, epoxy acrylate CAS No. 71281-65-7; tackifying resin is prepared by comparative preparation example 3; active diluent includes o-cresyl glycidyl ether and triethylene glycol divinyl ether in a mass ratio of 7:1; filler is nano-scale silica; photoinitiator includes photoinitiator 907 and photoinitiator UVI-6976 in a mass ratio of 3:1.
[0049] A method for preparing an acrylic pressure-sensitive adhesive tape for battery fixing comprises the following steps: S1. Weigh the raw materials of UV adhesive layer, methyl methacrylate, 2-hydroxyethyl acrylate, epoxy acrylate, styrene, tackifying resin, reactive diluent, filler, and photoinitiator, and mix them evenly to obtain a mixed adhesive; S2, firstly coating the mixed adhesive on the blue PVC to form a UV adhesive layer, and then laminating the PET release film on the other side of the UV adhesive layer to obtain a semi-finished product; S3. Bake the semi-finished product at 80° C. for 10 minutes to form the required acrylic pressure-sensitive tape for battery fixing.
[0050] Comparative Example 4: Comparative Example 4 is different from Example 1 only in that the tackifying resin is prepared from Comparative Preparation Example 4, specifically as follows: An acrylic pressure-sensitive adhesive tape for battery fixing, comprising a three-layer structure of a PET release film, a UV adhesive layer and a blue PVC substrate from the outside to the inside; wherein the UV adhesive layer comprises the following raw materials in parts by weight: 45 parts of methyl methacrylate, 22 parts of 2-hydroxyethyl acrylate, 20 parts of epoxy acrylate, 14 parts of styrene, 10 parts of tackifying resin, 16 parts of active diluent, 5 parts of filler, and 4 parts of photoinitiator; Among them, epoxy acrylate CAS No. 71281-65-7; tackifying resin is prepared by comparative preparation example 4; active diluent includes o-cresyl glycidyl ether and triethylene glycol divinyl ether in a mass ratio of 7:1; filler is nano-scale silica; photoinitiator includes photoinitiator 907 and photoinitiator UVI-6976 in a mass ratio of 3:1.
[0051] A method for preparing an acrylic pressure-sensitive adhesive tape for battery fixing comprises the following steps: S1. Weigh the raw materials of UV adhesive layer, methyl methacrylate, 2-hydroxyethyl acrylate, epoxy acrylate, styrene, tackifying resin, reactive diluent, filler, and photoinitiator, and mix them evenly to obtain a mixed adhesive; S2, firstly coating the mixed adhesive on the blue PVC to form a UV adhesive layer, and then laminating the PET release film on the other side of the UV adhesive layer to obtain a semi-finished product; S3. Bake the semi-finished product at 80° C. for 10 minutes to form the required acrylic pressure-sensitive tape for battery fixing.
[0052] Comparative Example 5: Comparative Example 5 is different from Example 1 only in that the active diluent is only o-cresyl glycidyl ether, as follows: An acrylic pressure-sensitive adhesive tape for battery fixing, comprising a three-layer structure of a PET release film, a UV adhesive layer and a blue PVC substrate from the outside to the inside; wherein the UV adhesive layer comprises the following raw materials in parts by weight: 45 parts of methyl methacrylate, 22 parts of 2-hydroxyethyl acrylate, 20 parts of epoxy acrylate, 14 parts of styrene, 10 parts of tackifying resin, 16 parts of active diluent, 5 parts of filler, and 4 parts of photoinitiator; Among them, epoxy acrylate CAS No. 71281-65-7; the tackifying resin is prepared by Preparation Example 1; the active diluent is o-cresyl glycidyl ether; the filler is nano-scale silica; and the photoinitiator includes photoinitiator 907 and photoinitiator UVI-6976 in a mass ratio of 3:1.
[0053] A method for preparing an acrylic pressure-sensitive adhesive tape for battery fixing comprises the following steps: S1. Weigh the raw materials of UV adhesive layer, methyl methacrylate, 2-hydroxyethyl acrylate, epoxy acrylate, styrene, tackifying resin, reactive diluent, filler, and photoinitiator, and mix them evenly to obtain a mixed adhesive; S2, firstly coating the mixed adhesive on the blue PVC to form a UV adhesive layer, and then laminating the PET release film on the other side of the UV adhesive layer to obtain a semi-finished product; S3. Bake the semi-finished product at 80° C. for 10 minutes to form the required acrylic pressure-sensitive tape for battery fixing.
[0054] Comparative Example 6: Comparative Example 6 is different from Example 1 only in that the reactive diluent is triethylene glycol divinyl ether, which is as follows: An acrylic pressure-sensitive adhesive tape for battery fixing, comprising a three-layer structure of a PET release film, a UV adhesive layer and a blue PVC substrate from the outside to the inside; wherein the UV adhesive layer comprises the following raw materials in parts by weight: 45 parts of methyl methacrylate, 22 parts of 2-hydroxyethyl acrylate, 20 parts of epoxy acrylate, 14 parts of styrene, 10 parts of tackifying resin, 16 parts of active diluent, 5 parts of filler, and 4 parts of photoinitiator; Among them, epoxy acrylate CAS No. 71281-65-7; tackifying resin is prepared by Preparation Example 1; the active diluent is triethylene glycol divinyl ether; the filler is nano-scale silica; the photoinitiator includes photoinitiator 907 and photoinitiator UVI-6976 in a mass ratio of 3:1.
[0055] A method for preparing an acrylic pressure-sensitive adhesive tape for battery fixing comprises the following steps: S1. Weigh the raw materials of UV adhesive layer, methyl methacrylate, 2-hydroxyethyl acrylate, epoxy acrylate, styrene, tackifying resin, reactive diluent, filler, and photoinitiator, and mix them evenly to obtain a mixed adhesive; S2, firstly coating the mixed adhesive on the blue PVC to form a UV adhesive layer, and then laminating the PET release film on the other side of the UV adhesive layer to obtain a semi-finished product; S3. Bake the semi-finished product at 80° C. for 10 minutes to form the required acrylic pressure-sensitive tape for battery fixing.
[0056] Comparative Example 7: Comparative Example 7 is different from Example 1 only in that the photoinitiator is photoinitiator 907, as follows: An acrylic pressure-sensitive adhesive tape for battery fixing, comprising a three-layer structure of a PET release film, a UV adhesive layer and a blue PVC substrate from the outside to the inside; wherein the UV adhesive layer comprises the following raw materials in parts by weight: 45 parts of methyl methacrylate, 22 parts of 2-hydroxyethyl acrylate, 20 parts of epoxy acrylate, 14 parts of styrene, 10 parts of tackifying resin, 16 parts of active diluent, 5 parts of filler, and 4 parts of photoinitiator; Among them, epoxy acrylate CAS No. 71281-65-7; the tackifying resin is prepared by Preparation Example 1; the active diluent includes o-cresyl glycidyl ether and triethylene glycol divinyl ether in a mass ratio of 7:1; the filler is nano-scale silica; and the photoinitiator is photoinitiator 907.
[0057] A method for preparing an acrylic pressure-sensitive adhesive tape for battery fixing comprises the following steps: S1. Weigh the raw materials of UV adhesive layer, methyl methacrylate, 2-hydroxyethyl acrylate, epoxy acrylate, styrene, tackifying resin, reactive diluent, filler, and photoinitiator, and mix them evenly to obtain a mixed adhesive; S2, firstly coating the mixed adhesive on the blue PVC to form a UV adhesive layer, and then laminating the PET release film on the other side of the UV adhesive layer to obtain a semi-finished product; S3. Bake the semi-finished product at 80° C. for 10 minutes to form the required acrylic pressure-sensitive tape for battery fixing.
[0058] Comparative Example 8: Comparative Example 8 is different from Example 1 only in that the photoinitiator is only photoinitiator UVI-6976, as follows: An acrylic pressure-sensitive adhesive tape for battery fixing, comprising a three-layer structure of a PET release film, a UV adhesive layer and a blue PVC substrate from the outside to the inside; wherein the UV adhesive layer comprises the following raw materials in parts by weight: 45 parts of methyl methacrylate, 22 parts of 2-hydroxyethyl acrylate, 20 parts of epoxy acrylate, 14 parts of styrene, 10 parts of tackifying resin, 16 parts of active diluent, 5 parts of filler, and 4 parts of photoinitiator; Among them, epoxy acrylate CAS No. 71281-65-7; tackifying resin is prepared by Preparation Example 1; active diluent includes o-cresyl glycidyl ether and triethylene glycol divinyl ether in a mass ratio of 7:1; filler is nano-scale silica; photoinitiator is photoinitiator UVI-6976.
[0059] A method for preparing an acrylic pressure-sensitive adhesive tape for battery fixing comprises the following steps: S1. Weigh the raw materials of UV adhesive layer, methyl methacrylate, 2-hydroxyethyl acrylate, epoxy acrylate, styrene, tackifying resin, reactive diluent, filler, and photoinitiator, and mix them evenly to obtain a mixed adhesive; S2, firstly coating the mixed adhesive on the blue PVC to form a UV adhesive layer, and then laminating the PET release film on the other side of the UV adhesive layer to obtain a semi-finished product; S3. Bake the semi-finished product at 80° C. for 10 minutes to form the required acrylic pressure-sensitive tape for battery fixing.
[0060] Performance testing: The acrylic pressure-sensitive adhesive tape for battery fixing in Examples 1-4 of the present invention and Comparative Examples 1-8 was made into test specimens with an outer PET release film thickness of 50 μm, a middle UV adhesive layer thickness of 55 μm, and an inner blue PVC substrate thickness of 45 μm, and the following performance tests were performed: 180° peel strength: Referring to the national standard GB / T 2792-2014 "Test Method for Peel Strength of Adhesive Tapes", the test was conducted according to the test method of Method 1 for the 180° peel strength between adhesive tape and stainless steel. The test sample was cut to a width of 24 mm. The peel strength of the tape was tested before UV, 20 minutes after UV, and after full curing (24 hours at room temperature). The specific UV conditions were: 365 nm, energy 2000 mj / cm 2 LED irradiation; Residual glue rate: After removing the PET release film of the test sample, the tape was heated at 365 nm and an energy of 2000 mj / cm 2 The LED was irradiated for 20 seconds. Within 2 minutes, the UV adhesive layer after LED irradiation was attached to the stainless steel plate. The pressure was pressed down with a pressure of 0.1 MPa. After 2 hours, 4 hours and 24 hours of pressing, the pressure-sensitive tape was continuously peeled off from the steel plate at a rate of 5 mm / s. The residual adhesive and the residual adhesive rate on the steel plate after the pressure-sensitive tape was peeled off were observed. The residual adhesive rate (%) = residual adhesive area / total area covered by the pressure-sensitive tape × 100%; The results are shown in Table 1 below.
[0061] Table 1:
[0062] After removing the PET release film of the test sample, the tape was heated at 365 nm and an energy of 2000 mj / cm 2 The LED was irradiated for 20 seconds, and the UV adhesive layer after LED irradiation was attached to the aluminum plate within 2 minutes. The blue PVC substrate was torn off, and the UV adhesive layer was attached to another aluminum plate. After pressing at a pressure of 0.1 MPa for 72 hours, the sample to be tested was obtained.
[0063] Shear Strength: Referring to the national standard GB / T 7124-2008 "Determination of tensile shear strength of adhesives", the initial shear strength of the test sample, the shear strength after the test sample is placed in an environment of -40℃ to 85℃ for 200 cycles, and the shear strength after the test sample is subjected to a double 85 aging test (placed in an environment of temperature 85℃ and humidity 85% for 2000h) are tested respectively; Initial viscosity: Refer to the national standard GB / T 4852-2002 "Pressure-sensitive Adhesive Tape Initial Adhesion Test Method (Rolling Ball Method)", and carry out the initial adhesion test of the sample to be tested according to the inclined rolling ball method of method A. The pressure-sensitive tape sample to be tested is 280×70mm, and the tilt angle is 30°; Stickiness: Refer to the national standard GB / T 4851-2014 "Test method for adhesive tape adhesion", and perform the test sample adhesion test according to the test method A for adhesive tape and vertical standard steel plate adhesion; The results are shown in Table 2 below.
[0064] Table 2:
[0065] Combining the data shown in Table 1 and Table 2 above, it can be seen that the comprehensive performance of the pressure-sensitive tape obtained in Examples 1-4 of the present invention is significantly better than that in Comparative Examples 1-8. The pressure-sensitive tape prepared in the examples of the present invention has high peeling strength and shear strength, no residual adhesive after peeling, good repairability and reworkability, and excellent heat resistance, water resistance, chemical solvent resistance, corrosion resistance and other properties. It can be used for battery fixation to achieve excellent product adhesion, heavy workability and stability, and has broad application prospects.
[0066] This specific embodiment is merely an explanation of the present invention and is not a limitation of the present invention. After reading this specification, those skilled in the art may make non-creative modifications to the present embodiment as needed. However, as long as they are within the scope of the claims of the present invention, they are protected by the patent law.
Claims
1. An acrylic pressure-sensitive adhesive tape for battery fixing, characterized in that: The invention comprises a three-layer structure including a release film, a UV adhesive layer and a substrate from the outside to the inside; the UV adhesive layer comprises the following raw materials in parts by weight: 45-55 parts of methyl methacrylate, 22-28 parts of 2-hydroxyethyl acrylate, 20-26 parts of epoxy acrylate, 14-18 parts of styrene, 10-15 parts of tackifying resin, 16-20 parts of active diluent, 5-12 parts of filler and 4-10 parts of photoinitiator.
2. The acrylic pressure-sensitive adhesive tape for battery fixing according to claim 1, characterized in that: The mass ratio of the methyl methacrylate, 2-hydroxyethyl acrylate, epoxy acrylate and styrene is 3:1.5:1.5:
1.
3. The acrylic pressure-sensitive adhesive tape for battery fixing according to claim 2, characterized in that: The UV adhesive layer comprises the following raw materials in parts by weight: 48 parts of methyl methacrylate, 24 parts of 2-hydroxyethyl acrylate, 24 parts of epoxy acrylate, 16 parts of styrene, 12 parts of tackifying resin, 18 parts of active diluent, 8 parts of filler, and 7 parts of photoinitiator.
4. The acrylic pressure-sensitive adhesive tape for battery fixing according to claim 1, characterized in that: The tackifying resin is prepared by the following method: Add melamine and solvent into a dry reaction kettle, heat to 50-60°C, stir for 30-60 minutes until dissolved, keep stirring, add toluene diisocyanate and tetramethyl meta-xylylene diisocyanate into the reaction kettle, stir and react for 1-2 hours, add dehydroabietic acid, epichlorohydrin and dibutyltin oxide, heat the reaction system to 70-80°C, continue to keep warm and stir and react for 2-4 hours to obtain the desired tackifying resin.
5. The acrylic pressure-sensitive adhesive tape for battery fixing according to claim 4, characterized in that: The tackifying resin comprises the following raw materials in specific weight parts: 18-25 parts of melamine, 15-20 parts of toluene diisocyanate, 8-12 parts of tetramethyl meta-xylylene diisocyanate, 15-25 parts of dehydroabietic acid, 5-12 parts of epichlorohydrin, 0.1-0.5 parts of dibutyltin oxide, and 30-40 parts of solvent.
6. The acrylic pressure-sensitive adhesive tape for battery fixing according to claim 5, characterized in that: The tackifying resin comprises the following raw materials in specific weight parts: 22 parts of melamine, 18 parts of toluene diisocyanate, 10 parts of tetramethyl meta-xylylene diisocyanate, 20 parts of dehydroabietic acid, 8 parts of epichlorohydrin, 0.3 parts of dibutyltin oxide, and 35 parts of solvent.
7. The acrylic pressure-sensitive adhesive tape for battery fixing according to claim 1, characterized in that: The active diluent comprises o-cresyl glycidyl ether and triethylene glycol divinyl ether in a mass ratio of 7-9:1-2.
8. The acrylic pressure-sensitive adhesive tape for battery fixing according to claim 1, characterized in that: The filler is at least one of nano-scale silicon dioxide, nano-scale talcum powder, nano-scale mica powder and nano-scale quartz powder.
9. The acrylic pressure-sensitive adhesive tape for battery fixing according to claim 1, characterized in that: The photoinitiator includes photoinitiator 907 and photoinitiator UVI-6976 in a mass ratio of 3-5:
1.
10. A method for preparing the acrylic pressure-sensitive adhesive tape for battery fixing according to any one of claims 1 to 9, characterized in that: The following steps are involved: S1. Weigh the raw materials of UV adhesive layer, methyl methacrylate, 2-hydroxyethyl acrylate, epoxy acrylate, styrene, tackifying resin, reactive diluent, filler, and photoinitiator, and mix them evenly to obtain a mixed adhesive; S2, firstly coating the mixed adhesive on the substrate to form a UV adhesive layer, and then attaching a release film to the other side of the UV adhesive layer to obtain a semi-finished product; S3. Bake the semi-finished product at 80-90° C. for 5-10 minutes to form the required acrylic pressure-sensitive tape for battery fixing.
Citation Information
Patent Citations
Polyurethane synthetic resin for preparing traceless glue sticker and traceless glue sticker prepared by applying polyurethane synthetic resin
CN103937197A
Preparation method of radiation curing polyacrylate adhesive tape and application thereof
CN107760222A
Ultraviolet-curing flame-retardant acrylic filling adhesive, light-curing adhesive film and preparation method thereof
CN118791998A
Resin composition for coating composition
JP1991231926A
Cited By
UV semi-structural adhesive, preparation method of UV semi-structural adhesive, UV semi-structural adhesive film and preparation method of UV semi-structural adhesive film
CN121271458A
Curable electrical insulation tape
EP4578921A1