Processing method and processing device of catalytic cracking light cycle oil, and application of heavy component prepared by processing method

Through the first distillation and cutting, heat condensation reaction and second distillation and cutting technology of catalytic cracking light cycle oil, heavy components rich in tricyclic aromatic hydrocarbons are prepared, and the problem of insufficient utilization of aromatic components in catalytic cracking diesel is solved, and the problem of the supply of insufficient utilization of aromatic components in catalytic cracking diesel is provided. High-quality needle-shaped coke raw materials meet the needs of carbon materials and lithium-ion battery anode materials.

CN118995263AActive Publication Date: 2024-11-22CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202310565221.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-18
Publication Date
2024-11-22
Estimated Expiration
2043-05-18

AI Technical Summary

Technical Problem

The prior art is difficult to effectively utilize the aromatic components in catalytic cracked light cycle oil (LCO), resulting in excess of two- and three-cyclic aromatic hydrocarbons and a shortage of needle-shaped coke raw materials, affecting the production of carbon materials and the efficient utilization of diesel.

Method used

Catalytic cracking light cycle oil is used to perform the first distillation and cutting, heat condensation reaction and second distillation to prepare heavy components rich in three to six rings of aromatic hydrocarbons, as needle-shaped coke raw materials, and improve the cutting temperature and heat condensation conditions. Yield and mass of recombinant components.

Benefits of technology

It enriches the source of carbon material raw materials and improves the resource utilization of catalytic cracking cycle oil. The needle-shaped coke produced has low sulfur nitrogen content, low ash content, high true density, and meets the "GB/T 37308-2019" standard, and Improves the electrochemical performance of lithium-ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118995263A_ABST
    Figure CN118995263A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of petroleum processing, in particular to a processing method and a processing device of catalytic cracking light cycle oil and application of heavy components prepared by the processing method. The processing method comprises the following steps: (1) carrying out first distillation cutting on catalytic cracking light cycle oil to obtain distillate oil rich in polycyclic aromatic hydrocarbon; (2) carrying out a thermal polycondensation reaction on the distillate oil to obtain a thermal polycondensation product; (3) carrying out second distillation cutting on the thermal polycondensation product to obtain a light component and a heavy component; in the distillate oil, the saturated hydrocarbon content is less than or equal to 20wt%, the monocyclic aromatic hydrocarbon content is less than or equal to 10wt%, and the polycyclic aromatic hydrocarbon content is more than or equal to 70wt%. The heavy component prepared by the processing method is used as a needle coke raw material for producing needle coke, and the prepared needle coke has the advantages of low sulfur and nitrogen content, low ash content, high true density and low thermal expansion coefficient, and meets the standard of GB / T 37308-2019 oil-based needle coke.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of petroleum processing, and in particular to a processing method for catalytic cracking light cycle oil, a processing device for catalytic cracking light cycle oil, an application of a heavy component obtained by the processing method, a needle coke and an application thereof. Background Art

[0002] Catalytic cracking light cycle oil (catalytic cracking light diesel, referred to as LCO), is usually used as a poor quality diesel blending component mixed with straight-run diesel. From the composition of LCO, the sulfur and nitrogen content is high, the total aromatic content is high, and the cetane number is low, which is a relatively inferior diesel component.

[0003] At present, the main outlets for LCO include blending components of commercial diesel, production of light aromatics (BTX) or high-octane gasoline, and marine fuel oil. Hydrogenation refining technology can achieve substantial modification of catalytic cracking diesel, and catalytic diesel modified by hydrogenation can be used as a blending component of commercial diesel and a low-sulfur marine fuel. At present, catalytic cracking diesel in my country accounts for about 30% of the total diesel product. In recent years, with the development of my country's economy, the growth rate of diesel demand in the domestic market for refined oil consumption is significantly lower than that of gasoline demand. my country's apparent consumption of diesel and gasoline ratio has dropped from 2.31 in 2005 to 1.25 in 2018, and the consumption of diesel and gasoline ratio will further show a downward trend in the long term in the next few years. LCO can be converted into light aromatics or high-octane gasoline by hydrogenation saturation and catalytic cracking. Domestic and foreign scholars have carried out a lot of basic research and industrial practice on this technical route.

[0004] CN201210410162.3, CN201310516588.1, CN201310517650.9, CN201310517666.X and CN201310010219.5 etc. disclose a series of processes or methods for catalytic conversion and upgrading of catalytic cracking diesel, and the technology of converting inferior LCO into high-octane catalytic cracking gasoline or light aromatics (BTX), mainly through the combination of hydrogenation and catalytic cracking, the aromatics in the LCO fraction are first selectively hydrogenated and saturated and then selectively catalytic cracked, and by setting a hydrogenation LCO conversion zone, the process parameters of hydrogenation and catalytic cracking are optimized and matched to achieve the maximum production of high-octane gasoline or light aromatics.

[0005] Needle coke is a carbon material with a silver-grey appearance and needle-like texture on the surface. It has the advantages of high crystallinity, small thermal expansion coefficient, good orientation, good electrical and thermal conductivity, etc. It is the raw material for preparing high-end carbon material products such as high-power graphite electrodes and high-performance lithium battery negative electrodes. Needle coke can be divided into two types: oil-based needle coke and coal-based needle coke. Oil-based needle coke has fewer pores, high volume density, high mechanical strength, low nitrogen content, low gas expansion rate during graphitization, and can be graphitized quickly; it has good adsorption properties for binders and is easy to shape. Although the raw materials of coal-based needle coke and oil-based needle coke come from different sources, the existing needle coke preparation or production-related technologies are all based on polycyclic aromatic hydrocarbons with three to six rings as raw materials, and are prepared through processes such as thermal polycondensation, intermediate phase cultivation, and coke pulling and solidification.

[0006] In the past two years, affected by the strong market demand for needle coke, the number of new needle coke companies has increased significantly. From 2018 to 2021, in just four years, the production capacity has increased from 510,000 tons to 2.1 million tons, and the market competition is fierce; however, the supply of catalytic oil slurry, the raw material for oil-based needle coke, has not increased, resulting in an increase in the price of catalytic oil slurry. At the same time, some companies have low operating rates and poor product quality due to insufficient raw material supply and poor raw material quality. In other words, the domestic refining industry is facing the problems of excess LCO two- and three-ring aromatics and shortage of three- to six-ring aromatic raw materials for needle coke. If the aromatic components of LCO can be effectively utilized, the two- and three-ring aromatics can be converted into three- to six-ring aromatics, and high-end carbon materials such as needle coke can be produced, it will find a new way to efficiently utilize catalytic cracking diesel. Summary of the invention

[0007] The purpose of the present invention is to overcome the problems that the existing LCO is aimed at producing clean diesel, low-sulfur marine fuel, increasing the production of light aromatics or high-octane gasoline, etc., while the technology for preparing three to six-ring aromatics from catalytic diesel as a raw material and finally preparing carbon materials is still lacking. Provided are a processing method for catalytic cracking light cycle oil, a processing device for catalytic cracking light cycle oil, an application of a heavy component obtained by the processing method, a needle coke and its application. The method uses catalytic cracking light cycle oil as a raw material, and the obtained heavy component can be used as a carbon material raw material, especially a needle coke raw material.

[0008] In order to achieve the above object, the first aspect of the present invention provides a method for processing catalytic cracking light cycle oil, the processing method comprising the following steps:

[0009] (1) performing a first distillation cut on the catalytic cracking light cycle oil to obtain a distillate oil rich in polycyclic aromatic hydrocarbons;

[0010] (2) subjecting the distillate oil to a thermal polycondensation reaction to obtain a thermal polycondensation product;

[0011] (3) subjecting the thermal polycondensation product to a second distillation cut to obtain a light component and a heavy component;

[0012] Among them, in the distillate oil, the content of saturated hydrocarbons is ≤20wt%, the content of monocyclic aromatic hydrocarbons is ≤10wt%, and the content of polycyclic aromatic hydrocarbons is ≥70wt%.

[0013] A second aspect of the present invention provides a processing device for catalytic cracking light cycle oil, the processing device comprising: a first fractionation tower, a thermal polycondensation reactor and a second fractionation tower connected in sequence;

[0014] Wherein, the first fractionation tower is used to perform a first distillation cut on the catalytic cracking light cycle oil, and obtain a fraction oil rich in polycyclic aromatic hydrocarbons at the bottom of the tower;

[0015] The thermal polycondensation reactor is used to carry out a thermal polycondensation reaction on the distillate oil, and a thermal polycondensation product is obtained at the bottom of the tower;

[0016] The second fractionation tower is used to perform a second distillation cut on the thermal polycondensation product, and a light component is obtained at the top of the tower, and a heavy component is obtained at the bottom of the tower.

[0017] The third aspect of the present invention provides an application of the heavy component obtained by the processing method provided in the first aspect in a carbon material raw material, preferably in a needle coke raw material.

[0018] A fourth aspect of the present invention provides a needle coke, wherein the needle coke is obtained by sequentially calcining and graphitizing the heavy component obtained by the processing method provided by the first aspect as the needle coke raw material.

[0019] The fifth aspect of the present invention provides an application of the needle coke provided in the fourth aspect in negative electrode materials and graphite electrodes of lithium-ion batteries.

[0020] Compared with the prior art, the present invention has the following advantages:

[0021] (1) The processing method provided by the present invention uses catalytic cracking light cycle oil as a raw material, adopts the technical means of first distillation cutting, thermal polycondensation reaction and second distillation cutting to prepare a heavy component rich in three- to six-ring condensed aromatic hydrocarbons, especially by regulating the cutting temperature of the first distillation cutting, the temperature and time of the thermal polycondensation reaction, and the cutting temperature of the second distillation cutting, the yield of the heavy component can be effectively improved, and the content of three- to six-ring condensed aromatic hydrocarbons in the heavy component can be increased;

[0022] (2) The processing method provided by the present invention not only enriches the source of carbon material raw materials, especially the source of needle coke raw materials, but also broadens the resource utilization of catalytic cracking cycle oil and increases the added value of the product;

[0023] (3) The heavy component obtained by the processing method provided by the present invention is used as a needle coke raw material to produce needle coke. The obtained needle coke has the advantages of low sulfur and nitrogen content, low ash content, high true density, and low thermal expansion coefficient, and meets the standard of "GB / T 37308-2019 Oil-based Needle Coke". At the same time, the needle coke is used in lithium-ion batteries to effectively improve the electrochemical performance of lithium-ion batteries. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 It is a schematic structural diagram of a processing device for catalytic cracking light cycle oil provided by the present invention;

[0025] Figure 2a and Figure 2b The polarized light micrographs of the needle coke P2 prepared from the heavy component of Example 2 at 200 times and 500 times magnification respectively.

[0026] Description of Reference Numerals

[0027] I, first fractionation tower II, thermal polycondensation reactor III, second fractionation tower 01, catalytic cracking light cycle oil 02, distillate oil 03, light fraction

[0028] 04. Thermal polycondensation products 05. Cracking gas 06. Heavy components 07. Light components DETAILED DESCRIPTION

[0029] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0030] In the present invention, unless otherwise specified, "first" and "second" do not indicate a sequence or limit to each material or step, but are only used to distinguish or indicate that they are not the same material or step. For example, "first" and "second" in "first distillation cut" and "second distillation cut" are only used to indicate that they are not the same distillation cut.

[0031] A first aspect of the present invention provides a method for processing catalytic cracking light cycle oil, the method comprising the following steps:

[0032] (1) performing a first distillation cut on the catalytic cracking light cycle oil to obtain a distillate oil rich in polycyclic aromatic hydrocarbons;

[0033] (2) subjecting the distillate oil to a thermal polycondensation reaction to obtain a thermal polycondensation product;

[0034] (3) subjecting the thermal polycondensation product to a second distillation cut to obtain a light component and a heavy component;

[0035] Among them, in the distillate oil, the content of saturated hydrocarbons is ≤20wt%, the content of monocyclic aromatic hydrocarbons is ≤10wt%, and the content of polycyclic aromatic hydrocarbons is ≥75wt%.

[0036] The inventors of the present invention have found that: by using catalytic cracking light cycle oil as raw material, adopting the technical means of first distillation cutting, thermal polycondensation reaction and second distillation cutting, the heavy component obtained can be used as needle coke raw material; in particular, by regulating the parameters of the raw material, the initial distillation point of the distillate oil, and the temperature of the thermal polycondensation reaction, the content of each component in the thermal polycondensation product can be regulated, thereby regulating the yield of the heavy component.

[0037] In the present invention, unless otherwise specified, the catalytic cracking light cycle oil refers to the diesel fraction produced by catalytic cracking, and the distillation range is 180-380°C.

[0038] In the present invention, unless otherwise specified, in the distillate oil, the saturated hydrocarbon content refers to the sum of the contents of paraffins and cycloalkanes; the polycyclic aromatic hydrocarbon content refers to the sum of the contents of dicyclic aromatic hydrocarbons and tricyclic aromatic hydrocarbons.

[0039] In some embodiments of the present invention, preferably, in step (1), the distillate oil has a saturated hydrocarbon content of 0.1-15 wt%, a monocyclic aromatic hydrocarbon content of 0.1-10 wt%, and a polycyclic aromatic hydrocarbon content of 75-99.8 wt%.

[0040] In some embodiments of the present invention, preferably, in the distillate oil, the content of dicyclic aromatics accounts for ≥75% of the content of polycyclic aromatics, preferably 79-99%; the content of tricyclic aromatics accounts for ≤25% of the content of polycyclic aromatics, preferably 1-21%. The use of the preferred conditions is more conducive to improving the yield of the heavy component and the content of three to six ring aromatics in the heavy component.

[0041] In some embodiments of the present invention, preferably, in step (1), the physical properties of the catalytic cracking light cycle oil meet the following requirements: sulfur content of 0.1-4wt%; nitrogen content of 1-1000mg / kg; oxygen content of 1-1000mg / kg; total aromatic content of 50-90wt%. In the present invention, unless otherwise specified, the total aromatic content in the catalytic cracking light cycle oil refers to the sum of the contents of monocyclic aromatics, dicyclic aromatics and tricyclic aromatics.

[0042] In the present invention, unless otherwise specified, the hydrocarbon composition in the feed oil is determined according to the "Determination of Hydrocarbons in Saturated Hydrocarbon Fractions in Gas Oil (Mass Spectrometry) (SH / T 0659-1998)".

[0043] In the present invention, unless otherwise specified, the hydrocarbon composition in the distillate oil is determined according to the "Determination of Hydrocarbon Composition of Mesophase Fraction (Mass Spectrometry) (SH / T 0606-2019)".

[0044] In the present invention, unless otherwise specified, the carbon and hydrogen content parameters are determined in accordance with the "Elemental Analyzer Method for the Determination of Carbon, Hydrogen and Nitrogen in Petroleum Products and Lubricants (SH / T 0656-2017)".

[0045] In the present invention, unless otherwise specified, the oxygen content parameter is determined according to the "Determination of total oxygen content in gasoline, diesel and methanol fuels - Reduction cracking method (SH / T 0986-2019)".

[0046] In the present invention, unless otherwise specified, the nitrogen content parameter is determined in accordance with the "Determination of Nitrogen Content in Petroleum and Petroleum Products - Boat Injection Chemiluminescence Method (SH / T 0704-2010)".

[0047] In the present invention, unless otherwise specified, the sulfur content parameter is determined in accordance with "Determination of sulfur content of petroleum and petroleum products - Energy dispersive X-ray fluorescence (GB / T 17040-2008)".

[0048] In some embodiments of the present invention, preferably, the content of monocyclic aromatic hydrocarbons in the catalytic cracking light cycle oil is ≥5wt%, preferably 5-15wt%; the content of dicyclic aromatic hydrocarbons is ≥50wt%, preferably 50-80wt%; the content of tricyclic aromatic hydrocarbons is ≥5wt%, preferably 5-10wt%.

[0049] In the present invention, the type of the catalytic cracking light cycle oil has a wide selection range, as long as the catalytic cracking light cycle oil meets the above definition. Preferably, the catalytic cracking light cycle oil is selected from catalytic cracking middle distillate oil and / or catalytic cracking refined diesel.

[0050] In a specific embodiment of the present invention, preferably, the catalytic cracking middle distillate is selected from at least one of residual catalytic cracking distillate, wax catalytic cracking distillate and heavy oil catalytic cracking distillate. That is to say, the catalytic cracking middle distillate is a middle distillate produced by a catalytic cracking unit, wherein the catalytic cracking unit can be a residual catalytic cracking unit, a wax catalytic cracking unit, a heavy oil catalytic cracking unit and a mixed feed catalytic cracking unit.

[0051] In the present invention, unless otherwise specified, the catalytic cracking refined diesel refers to the refined catalytic diesel with low sulfur content and low nitrogen content obtained by hydrotreating and hydrofining the catalytic cracking middle distillate oil.

[0052] In the present invention, the first distillation cut is intended to obtain a distillate oil of a specific fraction. Preferably, the cutting temperature of the first distillation cut is 220-300°C, such as 220°C, 230°C, 240°C, 250°C, 260°C, 280°C, 300°C, and any value in the range of any two values, preferably 230-280°C. The use of the preferred conditions is more conducive to regulating the content of saturated hydrocarbons, monocyclic aromatic hydrocarbons and polycyclic aromatic hydrocarbons in the distillate oil, and then regulating the yield of the heavy component and the content of three to six ring aromatic hydrocarbons in the heavy component.

[0053] In some embodiments of the present invention, preferably, in step (1), the initial distillation point of the distillate oil is 220-300° C., such as 220° C., 230° C., 240° C., 250° C., 260° C., 280° C., 300° C., and any value in the range of any two values, preferably 230-280° C. In the present invention, the final distillation point of the distillate oil is not limited, and the final distillation point of the distillate oil is the final distillation point of the feed oil.

[0054] In the present invention, the thermal polycondensation reaction is intended to polycondense the polycyclic aromatic hydrocarbons (i.e., dicyclic aromatic hydrocarbons and tricyclic aromatic hydrocarbons) of the distillate oil into three to six-cyclic aromatic hydrocarbons. Preferably, in step (2), the conditions of the thermal polycondensation reaction include: a temperature of 400-510°C, for example, 400°C, 410°C, 420°C, 430°C, 440°C, 450°C, 460°C, 480°C, 510°C, and any value in the range of any two values, preferably 410-460°C; a time of 0.1-5h, for example, 0.1h, 0.5h, 1h, 2h, 3h, 5h, and any value in the range of any two values, preferably 0.5-3h.

[0055] In some embodiments of the present invention, preferably, the toluene insoluble matter content in the thermal condensation product is ≤5wt%, for example, 0.1wt%, 0.5wt%, 1wt%, 2wt%, 3wt%, 4wt%, 5wt%, and any value in the range consisting of any two values, preferably ≤2wt%.

[0056] In some embodiments of the present invention, preferably, the total aromatic content in the thermal polycondensation product is 90-99wt%, and the content of dicyclic aromatics is ≤5wt%. In the present invention, the total aromatics in the thermal polycondensation product refers to the sum of the contents of monocyclic aromatics, dicyclic aromatics, tricyclic aromatics, tetracyclic aromatics, pentacyclic aromatics and hexacyclic aromatics.

[0057] In the present invention, the second distillation cutting is intended to separate the thermal polycondensation product into light components and heavy components. Preferably, the cutting temperature of the second distillation cutting is 330-400°C, for example, 300°C, 340°C, 350°C, 360°C, 380°C, 400°C, and any value in the range of any two values, preferably 340-360°C.

[0058] In some embodiments of the present invention, preferably, the initial distillation point of the heavy component is 330-400°C, for example, 300°C, 340°C, 350°C, 360°C, 380°C, 400°C, and any value in the range consisting of any two numerical values, preferably 340-360°C; the final distillation point is 500-600°C, for example, 500°C, 550°C, 560°C, 570°C, 580°C, 590°C, 600°C, and any value in the range consisting of any two numerical values, preferably 550-600°C.

[0059] In some embodiments of the present invention, preferably, the total content of three to six ring aromatics in the heavy component is 80-95 wt%.

[0060] In some embodiments of the present invention, preferably, before the thermal polycondensation reaction, the distillate oil is heated to 400-510° C., for example, 400° C., 410° C., 420° C., 430° C., 440° C., 450° C., 460° C., 480° C., 510° C., and any value in a range consisting of any two values, preferably 410-460° C. In the present invention, the heating method has a wide range of selections, as long as the distillate oil is heated to the temperature of the thermal polycondensation reaction, and the heating method includes but is not limited to tubular heating furnace heating, heat exchanger heating, tubular furnace heating, etc.

[0061] In some embodiments of the present invention, preferably, the processing method further comprises: recycling the light component back to the catalytic cracking light cycle oil.

[0062] The second aspect of the present invention provides a schematic diagram of the structure of a catalytic cracking light cycle oil processing device. Figure 1 As shown by Figure 1 It can be seen that the processing device includes: a first fractionation tower I, a thermal polycondensation reactor II and a second fractionation tower III connected in sequence;

[0063] Wherein, the first fractionation tower I is used to perform a first distillation cut on the catalytic cracking light cycle oil 01, and obtain a distillate oil 02 rich in polycyclic aromatic hydrocarbons at the bottom of the tower;

[0064] The thermal polycondensation reactor II is used to perform a thermal polycondensation reaction on the distillate oil 02, and obtain a thermal polycondensation product 04 at the bottom of the tower;

[0065] The second fractionation tower III is used to perform a second distillation cut on the thermal polycondensation product 04, and obtain a light component 07 at the top of the tower and a heavy component 06 at the bottom of the tower.

[0066] In the present invention, the types of the first fractionator and the second fractionator have a wide range of choices, as long as the catalytic cracking light cycle oil and the thermal polycondensation product are respectively cut into the above fractions. In the present invention, the first fractionator and the second fractionator include but are not limited to vacuum fractionators, etc.

[0067] According to the present invention, Figure 1 As shown, the top of the first fractionation tower I also obtains a light fraction 03, and the top of the thermal polycondensation reactor II also obtains a cracking gas 05.

[0068] According to the present invention, preferably, Figure 1 As shown, the top of the second fractionation tower III is also connected to the raw material inlet of the first fractionation tower I, so as to return the light component 07 and mix it into the catalytic cracking light cycle oil 01 for the first distillation cutting.

[0069] The third aspect of the present invention provides an application of the heavy component obtained by the processing method provided in the first aspect in a carbon material raw material, preferably in a needle coke raw material.

[0070] A fourth aspect of the present invention provides a needle coke, wherein the needle coke is obtained by sequentially calcining and graphitizing the heavy component obtained by the processing method provided by the first aspect as the needle coke raw material.

[0071] In some embodiments of the present invention, preferably, the calcination conditions include: temperature of 1300-1450° C., preferably 1350-1400° C.; time of 10-20 h, preferably 12-14 h.

[0072] In some embodiments of the present invention, preferably, the conditions of the graphitization treatment include: a temperature of 2700-3000° C., preferably 2800-2900° C.; and a time of 2-5 h, preferably 3-4 h.

[0073] In some embodiments of the present invention, preferably, the sulfur content of the needle coke is ≤0.5wt%, the nitrogen content is ≤0.5wt%, the ash content is ≤0.1wt%, and the true density (before calcination) is ≥1.35g / cm 3 , true density (before calcination) ≥2.12g / cm 3 , thermal expansion coefficient (25-600℃) ≤1.3×10 -6 / ℃, and its polarized light microstructure is wide-area streamlined.

[0074] The fifth aspect of the present invention provides an application of the needle coke provided in the fourth aspect in negative electrode materials and graphite electrodes of lithium-ion batteries.

[0075] According to a particularly preferred embodiment of the present invention, a method for processing catalytic cracking light cycle oil comprises the following steps:

[0076] (1) performing a first distillation cut on the catalytic cracking light cycle oil to obtain a distillate oil rich in polycyclic aromatic hydrocarbons;

[0077] (2) subjecting the distillate oil to a thermal polycondensation reaction to obtain a thermal polycondensation product;

[0078] (3) heating the thermal polycondensation product to 410-460° C. and performing a second distillation cutting to obtain a light component and a heavy component;

[0079] The content of monocyclic aromatic hydrocarbons in the catalytic cracking light cycle oil is 5-15wt%; the content of dicyclic aromatic hydrocarbons is 50-80wt%; the content of tricyclic aromatic hydrocarbons is 5-10wt%;

[0080] The distillate oil contains 0.1-15 wt% saturated hydrocarbons, 0.1-10 wt% monocyclic aromatic hydrocarbons and 75-99.8 wt% polycyclic aromatic hydrocarbons;

[0081] Among them, the cutting temperature of the first distillation cutting is 230-280℃; the conditions of the thermal polycondensation reaction include: temperature of 410-460℃; time of 0.5-3h; the content of toluene insoluble matter in the thermal polycondensation product is ≤2wt%; the cutting temperature of the second distillation cutting is 340-360℃; the total content of three to six ring aromatics in the heavy component is 80-95wt%.

[0082] The present invention will be described in detail below through examples.

[0083] The hydrocarbon composition in the feedstock oil is determined in accordance with the "Determination of Hydrocarbons in Saturated Hydrocarbon Fractions in Gas Oil (Mass Spectrometry) (SH / T0659-1998)";

[0084] The hydrocarbon composition in the distillate oil is determined according to the "Determination of Hydrocarbon Composition of Mesophase Fraction (Mass Spectrometry) (SH / T0606-2019)";

[0085] The carbon and hydrogen content parameters are determined in accordance with the "Elemental Analyzer Method for the Determination of Carbon, Hydrogen and Nitrogen in Petroleum Products and Lubricants (SH / T 0656-2017)";

[0086] The oxygen content parameters are determined according to the "Determination of total oxygen content in gasoline, diesel and methanol fuels - Reduction cracking method (SH / T0986-2019)";

[0087] The nitrogen content parameters are determined in accordance with the "Determination of Nitrogen Content in Petroleum and Petroleum Products - Boat Injection Chemiluminescence Method (SH / T0704-2010)";

[0088] The sulfur content parameters are determined in accordance with the "Determination of sulfur content of petroleum and petroleum products - Energy dispersive X-ray fluorescence (GB / T 17040-2008)".

[0089] The yield is calculated as follows: The components are selected from light components or heavy components.

[0090] Example 1

[0091] (1) Using YS catalytic diesel (each component and its content are shown in Table 1) as a raw material, a first distillation cut (cutting temperature is 250° C.) is performed to obtain a distillate oil A1 with a distillation range of more than 250° C. (each component and its content are shown in Table 2);

[0092] (2) The distillate oil A1 was heated to 410° C. and subjected to a thermal polycondensation reaction (temperature: 410° C., time: 1.2 h) to obtain a thermal polycondensation product S1 (components and their contents are shown in Table 3);

[0093] (3) The above-mentioned thermal polycondensation product S1 was subjected to a second distillation cutting (cutting temperature was 400° C.), and the yields of the light component and the heavy component were listed in Table 4.

[0094] Example 2

[0095] (1) YS catalytic diesel (each component and its content are shown in Table 1) is used as a raw material for the first distillation cutting (cutting temperature is 280° C.) to obtain a distillate oil A2 with a distillation range of more than 280° C. (each component and its content are shown in Table 2);

[0096] (2) The distillate oil A2 was heated to 440° C. and subjected to a thermal polycondensation reaction (temperature: 440° C., time: 1.2 h) to obtain a thermal polycondensation product S2 (components and their contents are shown in Table 3);

[0097] (3) The above-mentioned thermal polycondensation product S2 was subjected to a second distillation cutting (cutting temperature was 400° C.), and the yields of the light component and the heavy component were listed in Table 4.

[0098] Example 3

[0099] (1) YS catalytic diesel (each component and its content are shown in Table 1) is used as a raw material for the first distillation cutting (cutting temperature is 280° C.) to obtain a distillate oil A2 with a distillation range of more than 280° C. (each component and its content are shown in Table 2);

[0100] (2) The distillate oil A2 was heated to 410° C. and subjected to a thermal polycondensation reaction (temperature: 410° C., time: 1.2 h) to obtain a thermal polycondensation product S3 (components and their contents are shown in Table 3);

[0101] (3) The above-mentioned thermal polycondensation product S3 was subjected to a second distillation cutting (cutting temperature was 400° C.), and the yields of the light component and the heavy component were listed in Table 4.

[0102] Example 4

[0103] According to the method of Example 1, the difference is that

[0104] In step (1), YS catalytic diesel is replaced by MM catalytic diesel, the temperature of the first distillation cut is replaced by 280° C., and the other conditions are the same, to obtain a distillate oil A3 with a distillation range of more than 280° C. (refer to Table 2 for each component and its content);

[0105] In step (2), a thermal polycondensation product S4 is obtained (the components and their contents are shown in Table 3);

[0106] In step (3), the yields of light components and heavy components are listed in Table 4.

[0107] Example 5

[0108] According to the method of Example 1, the difference is that

[0109] In step (1), the cutting temperature of the first distillation cutting is adjusted to 300° C. to obtain a distillate oil A4 having a distillation range of more than 300° C.;

[0110] In step (2), a thermal polycondensation product S5 is obtained (the components and their contents are shown in Table 3);

[0111] In step (3), the yields of light components and heavy components are listed in Table 4.

[0112] Example 6

[0113] According to the method of Example 1, the difference is that

[0114] In step (1), the cutting temperature of the first distillation cutting is adjusted, and the other conditions are the same, to obtain a distillate oil A5 with a distillation range of 200° C. (refer to Table 2 for each component and its content);

[0115] In step (2), a thermal polycondensation product S6 is obtained (the components and their contents are shown in Table 3);

[0116] In step (3), the yields of light components and heavy components are listed in Table 4.

[0117] Example 7

[0118] According to the method of Example 1, the difference is that

[0119] In step (2), the distillate oil is heated to 520° C. and subjected to a thermal polycondensation reaction (temperature is 520° C., time is 1.2 h), and other conditions are the same to obtain a thermal polycondensation product S7 (refer to Table 3 for each component and its content);

[0120] In step (3), the yields of light components and heavy components are listed in Table 4.

[0121] Example 8

[0122] According to the method of Example 1, the difference is that

[0123] In step (3), the cutting temperature of the second distillation cutting was replaced with 450°C, and the other conditions were the same. The yields of the light components and the heavy components were listed in Table 4.

[0124] Comparative Example 1

[0125] The method of Example 1 is followed, except that step (1) is omitted, i.e.,

[0126] The YS catalytic diesel was directly heated to 440°C for a thermal polycondensation reaction (temperature: 440°C, time: 1 h) to obtain a thermal polycondensation product DS1 (components and their contents are shown in Table 3);

[0127] The above-mentioned thermal polycondensation product DS1 was subjected to a second distillation cutting (cutting temperature was 400° C.), and the yields of the light component and the heavy component were listed in Table 4.

[0128] Comparative Example 2

[0129] According to the method of Example 1, the difference is that

[0130] In step (1), YS catalytic diesel is replaced by YS straight-run diesel (refer to Table 1 for each component and its content), and other conditions are the same, to obtain distillate oil DA1 with a distillation range of 280° C. (refer to Table 2 for each component and its content);

[0131] In step (2), a thermal polycondensation product DS2 is obtained (the components and their contents are shown in Table 3);

[0132] In step (3), the yields of light components and heavy components are listed in Table 4.

[0133] Table 1

[0134]

[0135]

[0136] Table 2

[0137]

[0138] Table 3

[0139]

[0140]

[0141] Table 3

[0142]

[0143] Table 4

[0144]

[0145]

[0146] Table 4

[0147] Yield, wt% Example 6 Example 7 Example 8 Comparative Example 1 Comparative Example 2 Light component yield 80 76 78 95 98 Heavy component yield 20 24 22 5 2 Total yield 100 100 100 100 100

[0148] It can be seen from the results in Table 1-4 that, compared with Comparative Example 1-2, Example 1-8 uses catalytic cracking light cycle oil as feedstock oil, and adopts the technical means of first distillation cutting, thermal polycondensation reaction and second distillation cutting to obtain a heavy component rich in three to six-ring condensed aromatic hydrocarbons, and effectively improves the yield of the heavy component.

[0149] Test Case

[0150] The heavy components obtained in Examples 1-8 and Comparative Examples 1-2 were used as needle coke raw materials (P1-P8 and DP1-DP2) and were calcined (temperature: 1350°C, time: 4h) and graphitized (temperature: 2800°C, time: 2h) in sequence to obtain needle cokes (W1-W7 and DW1-DW3). The physical properties of the obtained needle cokes are listed in Table 5.

[0151] The polarized light micrographs of the needle coke P2 prepared from the heavy component of Example 2 at 200 times and 500 times are as follows: Figure 2a and Figure 2b As shown by Figure 2a and Figure 2b As shown in FIG. 1 , the polarized light microstructure of needle coke P2 is a wide-area streamlined structure.

[0152] Table 5

[0153]

[0154]

[0155] Table 5

[0156]

[0157] It can be seen from the results in Table 5 that, compared with Comparative Examples 1-2, the needle coke prepared by the processing method provided by the present invention in Examples 1-8 has the advantages of low sulfur and nitrogen content, low ash content, high true density, and low thermal expansion coefficient, and meets the standard of "GB / T37308-2019 Oil-based Needle Coke".

[0158] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A method for processing catalytic cracking light cycle oil, characterized in that: The processing method comprises the following steps: (1) performing a first distillation cut on the catalytic cracking light cycle oil to obtain a distillate oil rich in polycyclic aromatic hydrocarbons; (2) subjecting the distillate oil to a thermal polycondensation reaction to obtain a thermal polycondensation product; (3) subjecting the thermal polycondensation product to a second distillation cut to obtain a light component and a heavy component; Among them, in the distillate oil, the content of saturated hydrocarbons is ≤20wt%, the content of monocyclic aromatic hydrocarbons is ≤10wt%, and the content of polycyclic aromatic hydrocarbons is ≥70wt%.

2. The processing method according to claim 1, wherein: In step (1), the distillate oil has a saturated hydrocarbon content of 0.1-15wt%, a monocyclic aromatic hydrocarbon content of 0.1-10wt%, and a polycyclic aromatic hydrocarbon content of 75-99.8wt%; And / or, in the distillate oil, the content of dicyclic aromatic hydrocarbons accounts for ≥75% of the content of polycyclic aromatic hydrocarbons, preferably 79-99%; the content of tricyclic aromatic hydrocarbons accounts for ≤25% of the content of polycyclic aromatic hydrocarbons, preferably 1-21%.

3. The processing method according to claim 1 or 2, wherein: In step (1), the physical properties of the catalytic cracking light cycle oil meet the following requirements: sulfur content of 0.1-4 wt%; nitrogen content of 1-1000 mg / kg; oxygen content of 1-1000 mg / kg; total aromatic content of 50-90 wt%; And / or, the content of monocyclic aromatic hydrocarbons in the catalytic cracking light cycle oil is ≥5wt%, preferably 5-15wt%; the content of dicyclic aromatic hydrocarbons is ≥50wt%, preferably 50-80wt%; the content of tricyclic aromatic hydrocarbons is ≥5wt%, preferably 5-10wt%; And / or, the catalytic cracking light cycle oil is selected from catalytic cracking middle distillate oil and / or catalytic cracking refined diesel oil; preferably, the catalytic cracking middle distillate oil is selected from at least one of residual oil catalytic cracking distillate oil, wax oil catalytic cracking distillate oil and heavy oil catalytic cracking distillate oil.

4. The processing method according to any one of claims 1 to 3, wherein: In step (1), the cutting temperature of the first distillation cutting is 220-300° C., preferably 230-280° C.; And / or, the initial boiling point of the distillate oil is 220-300°C, preferably 230-280°C.

5. The processing method according to any one of claims 1 to 4, wherein: In step (2), the conditions of the thermal polycondensation reaction include: temperature of 400-510° C., preferably 410-460° C.; time of 0.1-5 h, preferably 0.5-3 h; and / or, the content of toluene insoluble matter in the thermal polycondensation product is ≤5wt%, preferably ≤2wt%; And / or, the total aromatic content in the thermal polycondensation product is 90-99wt%, and the dicyclic aromatic content is ≤5wt%.

6. The processing method according to any one of claims 1 to 5, wherein: In step (3), the cutting temperature of the second distillation cutting is 330-400°C, preferably 340-360°C; And / or, the initial distillation point of the heavy component is 330-400°C, preferably 340-360°C; the final distillation point is 500-600°C, preferably 550-600°C; and / or, the total content of three to six ring aromatics in the heavy component is 80-95wt%; And / or, the processing method further comprises: before the thermal condensation reaction, heating the distillate oil to 400-510°C, preferably 410-460°C.

7. A processing device for catalytic cracking light cycle oil, characterized in that: The processing device comprises: a first fractionation tower, a thermal polycondensation reactor and a second fractionation tower connected in sequence; Wherein, the first fractionation tower is used to perform a first distillation cut on the catalytic cracking light cycle oil, and obtain a fraction oil rich in polycyclic aromatic hydrocarbons at the bottom of the tower; The thermal polycondensation reactor is used to carry out a thermal polycondensation reaction on the distillate oil, and a thermal polycondensation product is obtained at the bottom of the tower; The second fractionation tower is used to perform a second distillation cut on the thermal polycondensation product, and a light component is obtained at the top of the tower, and a heavy component is obtained at the bottom of the tower.

8. Use of the heavy component obtained by the processing method according to any one of claims 1 to 6 in carbon material raw materials, preferably in needle coke raw materials.

9. A needle coke, characterized in that: The needle coke is obtained by calcining and graphitizing the heavy component obtained by the processing method according to any one of claims 1 to 6 as the needle coke raw material; And / or, the polarized light microstructure of the needle coke is a wide-area streamlined structure; And / or, the sulfur content of the needle coke is ≤0.5wt%, the nitrogen content is ≤0.5wt%, the ash content is ≤0.1wt%, and the true density (before calcination) is ≥1.35g / cm 3 , true density (before calcination) ≥2.12g / cm 3 , thermal expansion coefficient (25-600℃) ≤1.3×10 -6 / ℃.

10. Use of the needle coke according to claim 9 in negative electrode materials and graphite electrodes of lithium-ion batteries.

Citation Information

Patent Citations

  • Novel coke tower and needle coke production method

    CN105733650A

  • Method of utilizing catalytic cracking diesel oil, and high-octane gasoline or high-octane gasoline blend component

    CN107880934A

  • Method and equipment for preparing needle coke crude materials

    CN107987875A

  • Method and equipment for preparing needle coke raw material

    CN112745916A

  • Method for preparing high-quality petroleum coke

    CN114479906A