Niobium alloying method for smelting niobium-containing stainless steel through VOD (Vacuum Oxygen Decarburization)
By using high temperature and deep vacuum conditions during VOD smelting, combining Al particles and FeSi alloy reduction materials, the Nb yield is improved, the problem of high cost of FeNb alloy is solved, and the efficiency of stainless steel Nb alloy is achieved is achieved Economic effect.
Patent Information
- Application Number
- CN202411213242.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-22
AI Technical Summary
During VOD smelting, when Nb alloying of niobium-containing stainless steel, high-cost FeNb alloys need to be added to improve the yield of Nb elements, resulting in lower economic benefits.
By using high temperature, deep vacuum and strong stirring thermal and kinetic conditions during VOD smelting, Al particles and FeSi alloys are used as reducing materials to effectively reduce niobium concentrate, improve the yield of Nb, and refine it in LF and The continuous casting stage is fine-tuned to realize Nb alloying of stainless steel.
The Nb yield rate is increased to more than 90%, the stainless steel production cost is reduced, and the economic benefits of the product are improved.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of stainless steel smelting, and in particular to a niobium alloying method for VOD smelting of niobium-containing stainless steel. Background Art
[0002] Niobium-containing stainless steel produced by the VOD process mainly includes ultra-pure ferritic stainless steels such as S43940 (J441), SUS443, SUS430J1L (J442D), and SUS445J2. They are easily oxidized after being added in the AOD and VOD oxygen blowing stages, and the Nb recovery rate is only 60-70%. The existing method is mainly to add a certain amount of FeNb alloy in the Lf refining furnace during the Nb alloying smelting of niobium-containing stainless steel. Although the recovery rate of Nb element has been improved, the cost of using FeNb alloy is relatively expensive, resulting in low economic benefits. Summary of the invention
[0003] In view of the above technical problems, the present invention provides a niobium alloying method for VOD smelting of niobium-containing stainless steel, which is used to solve the problem that during the Nb alloying smelting of niobium-containing stainless steel, FeNb alloy needs to be added to adjust the yield of Nb element, resulting in low economic benefits.
[0004] In order to achieve the above object, the technical solution of the present invention is as follows: A niobium alloying method for VOD smelting of niobium-containing stainless steel comprises the following steps: S1. VOD molten steel entering the tank: After the stainless steel mother liquor smelted by AOD is slag-stripped, it is placed in a ladle and hoisted to VOD. The ladle clearance is greater than 1000mm, the molten steel temperature is greater than 1600℃, and argon is blown from the bottom of the ladle to test whether the air brick is good. The argon flow rate is 100-300L / min, and samples are taken after the test; S2, VOD oxygen decarburization: Start shallow vacuum pumping, vacuum degree <150torr, start oxygen decarburization, the O2 flow rate of the oxygen gun is 1200-1500Nm 3 / h, oxygen lance position is 1000-1550mm, oxygen blowing volume is 500-1000Nm 3 , the vacuum degree at the end of dynamic oxygen blowing is less than 50torr; S3, VCD treatment: start deep vacuum pumping, vacuum degree <1.0torr, bottom blowing stirring gas argon flow rate is 800-1500L / min, enter VCD stage>5min after adding 400-1200kg niobium concentrate, VCD treatment time>15min; S4, VOD reduction and vacuum breaking: add 500-1500kg of reducing materials, and 3000-4000kg of auxiliary materials to make slag, vacuum degree 20-150torr, bottom blowing argon 600-1500L / min for full stirring; reduction time>15min, measure temperature and take samples after vacuum breaking; S5. LF refining and CCM: After the VOD treatment, the composition and temperature of the molten steel are fine-tuned in LF, and then the molten steel in the ladle is transported to the continuous casting platform for casting to obtain the niobium-containing stainless steel ingot product.
[0005] Furthermore, the reducing materials in step S4 are Al particles and FeSi alloy, and the auxiliary materials are lime and fluorite.
[0006] Compared with the prior art, the beneficial effects of the present invention are as follows: the present invention utilizes the thermal and dynamic conditions of high temperature, deep vacuum and strong stirring, and the carbon element in the molten steel effectively reduces the niobium pentoxide in the niobium concentrate to achieve Nb alloying in stainless steel smelting; at the same time, the reducing materials Al particles and FeSi alloy in the VOD smelting reduction stage can further increase the recovery rate of Nb in the niobium concentrate to more than 90%. The present invention provides a VOD process method for smelting niobium-containing stainless steel using niobium concentrate, which reduces the production cost of stainless steel and improves the economic benefits of stainless steel products. DETAILED DESCRIPTION
[0007] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with specific embodiments. It should be understood that these descriptions are exemplary only and are not intended to limit the scope of the present invention. In addition, in the following description, the description of known structures and technologies is omitted to avoid unnecessary confusion of the concept of the present invention.
[0008] Embodiment 1, S43940 (J441) ultrapure ferritic stainless steel is selected. Its chemical composition is C: 0.0080%, Si: 0.30%, Mn: 0.30%, P: 0.025%, S: 0.0010%, Cr: 17.50%, Nb: 0.40%, N: 0.0080%, and the balance is Fe. The following steps are included: S1. VOD molten steel entering the tank: J441 ultra-pure ferritic stainless steel molten steel smelted by AOD is hoisted to VOD after slagging, the ladle clearance is 1200mm, the molten steel temperature is 1630℃, the argon flow rate of the ladle bottom blowing is 100L / min, and the test of the air-permeable brick is good; the chemical composition of the molten steel after sampling is C: 0.32%, Si: 0.11%, Mn: 0.20%, P: 0.025%, S: 0.013%, Cr: 17.82%, Ni: 0.23%, Nb: 0.0035%, N: 0.0098%, and the balance is Fe; S2, VOD oxygen decarburization: Start shallow vacuum pumping, vacuum degree 140torr, start oxygen decarburization, oxygen gun flow rate 1200Nm 3 / h, oxygen lance initial position 1000mm, oxygen blowing volume 500Nm 3 , the vacuum degree at the end of dynamic oxygen blowing is 35torr; S3, VCD treatment: start deep vacuum pumping, vacuum degree 0.6torr, bottom blowing stirring gas argon flow 800Nm 3 / h, 400kg of niobium concentrate was added 8min after entering the VCD stage, and the processing time continued for 10min; S4, VOD reduction and vacuum breaking: adding reducing materials Al particles 400kg, FeSi alloy 100kg, auxiliary materials lime 2700kg, fluorite 300kg slag making, vacuum degree 20torr, bottom blowing argon 600L / min, reduction time 17min, temperature measured after vacuum breaking 1610℃; chemical composition of molten steel after sampling is C: 0.0065%, Si: 0.21%, Mn: 0.22%, P: 0.024%, S: 0.0008%, Cr: 17.68%, Ni: 0.23%, Nb: 0.36%, N: 0.0078%, and the balance is Fe; S5. LF refining and CCM: After the VOD treatment of the J441 stainless steel liquid is completed, the ladle is hoisted to the LF furnace for refining, the composition is fine-tuned and the temperature is adjusted. After the outlet temperature reaches 1588°C, weak blowing is performed for 15 minutes. The ladle is then transported to the continuous casting platform for casting to obtain the niobium-containing stainless steel S43940 (J441) ingot product.
[0009] This pouring process produces 5 furnaces of continuous pouring according to the above steps S1-S5.
[0010] Embodiment 2, SUS445J2 ultrapure hot metal stainless steel is selected. Its chemical composition is C: 0.010%, Si: 0.33%, Mn: 0.21%, P: 0.019%, S: 0.0010%, Ni: 0.28%, Cr: 22.17%, Mo: 1.60%, Nb: 0.26%, Ti: 0.17%, N: 0.0088%, and the balance is Fe. The following steps are included: S1. VOD molten steel entering the tank: SUS445J2 ultra-pure ferritic stainless steel molten steel smelted by AOD is hoisted to VOD after slagging, the ladle clearance is 1350mm, the molten steel temperature is 1655℃, the argon flow rate of the ladle bottom blowing is 200L / min, and the air-permeable brick effect is good; the chemical composition of the molten steel after sampling is C: 0.24%, Si: 0.08%, Mn: 0.21%, P: 0.019%, S: 0.0093%, Cr: 22.27%, Ni: 0.28%, Mo: 1.55%, Nb: 0.0042%, N: 0.0116%, and the balance is mainly Fe; S2, VOD oxygen blowing decarburization: Start shallow vacuum pumping, vacuum degree 130torr, start oxygen blowing decarburization, oxygen flow rate 1350Nm 3 / h, oxygen lance initial position 1300mm, oxygen blowing volume 750Nm 3 ,,The vacuum degree at the end of dynamic oxygen blowing is 37.2torr; S3, VCD treatment: start deep vacuum pumping, vacuum degree 0.1torr, bottom blowing stirring gas argon flow rate 800L / min, add 800kg niobium concentrate 10min into VCD stage, and continue treatment time 8min; S4, VOD reduction and breaking: adding reducing materials of aluminum particles 776kg, FeSi alloy 224kg, auxiliary materials of lime 2800kg, fluorite 700kg, vacuum degree 85torr, bottom blowing argon 1050L / min, reduction time 20min, temperature measured after breaking vacuum 1617℃; chemical composition of molten steel after sampling is C: 0.0087%, Si: 0.19%, Mn: 0.21%, P: 0.019%, S: 0.0009%, Cr: 22.14%, Ni: 0.28%, Mo: 1.53%, Nb: 0.23%, N: 0.0081%, and the balance is Fe; S5. LF refining and CCM: After the SUS445J2 stainless steel liquid is subjected to VOD treatment, the ladle is hoisted to the LF furnace for refining treatment, the composition is fine-tuned and the temperature is adjusted. After the outlet temperature reaches 1584°C, weak blowing is performed for 15 minutes. The ladle is then transported to the continuous casting platform for casting to obtain the SUS445J2 niobium-containing stainless steel ingot product.
[0011] This pouring process produces 3 furnaces of continuous pouring according to the above steps S1-S5.
[0012] Embodiment 3, SUS430J1L (J442D) ultrapure ferritic stainless steel is selected. Its chemical composition is C: 0.011%, Si: 0.55%, Mn: 0.18%, P: 0.018%, S: 0.0013%, Ni: 0.35%, Cr: 19.17%, Cu: 0.45%, Nb: 0.54%, N: 0.00108%, and the balance is Fe. The following steps are included: S1. VOD molten steel entering the tank: J442D ultra-pure ferritic stainless steel molten steel smelted by AOD is hoisted to VOD after slagging, the ladle clearance is 1150mm, the molten steel temperature is 1633℃, the argon flow rate of the ladle bottom blowing is 300L / min, and the air-permeable brick effect is good; the chemical composition of the molten steel after sampling is C: 0.21%, Si: 0.073%, Mn: 0.16%, P: 0.018%, S: 0.0077%, Cr: 19.28%, Ni: 0.32%, Cu: 0.39%, Nb: 0.0046%, N: 0.0099%, and the balance is Fe; S2, VOD oxygen decarburization: Start shallow vacuum pumping, vacuum degree 135L / min, start oxygen decarburization, oxygen flow rate 1500Nm 3 / h, oxygen lance initial position 1550mm, oxygen blowing volume 1000Nm 3 , the vacuum degree at the end of dynamic oxygen blowing is 33.2torr; S3, VCD treatment: start deep vacuum pumping, vacuum degree 0.3torr, bottom blowing stirring gas argon flow rate 1500L / min, enter the VCD stage 8min after adding 1200kg niobium concentrate, continue processing time 10min; S4, VOD reduction: add 1500kg of FeSi alloy as reducing material, 3000kg of lime and 1000kg of fluorite as auxiliary materials, vacuum degree 150torr, bottom blowing argon 1500Nm 3 / h, reduction time 18min, temperature after breaking vacuum 1608℃; chemical composition of molten steel after sampling is C: 0.0078%, Si: 0.49%, Mn: 0.18%, P: 0.018%, S: 0.0012%, Cr: 19.19%, Ni: 0.32%, Cu: 0.39%, Nb: 0.51%, N: 0.0090%, balance Fe; S5. LF refining and CCM: After the VOD treatment of J442D ultrapure ferritic stainless steel is completed, the ladle is hoisted to the LF furnace for refining treatment, the composition is fine-tuned and the temperature is adjusted. After the outlet temperature is 1580°C and weak blowing is performed for 18 minutes, the ladle is transported to the continuous casting platform for casting to obtain the J442D niobium-containing stainless steel ingot product.
[0013] This pouring process produces 3 furnaces of continuous pouring according to the above steps S1-S5.
[0014] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A niobium alloying method for smelting niobium-containing stainless steel by VOD, characterized in that: The following steps are involved: S1. VOD molten steel entering the tank: After the stainless steel mother liquor smelted by AOD is slag-stripped, it is placed in a ladle and hoisted to VOD. The ladle clearance is greater than 1000mm, the molten steel temperature is greater than 1600℃, and argon is blown from the bottom of the ladle to test whether the air brick is good. The argon flow rate is 100-300L / min, and samples are taken after the test; S2, VOD oxygen decarburization: Start shallow vacuum pumping, vacuum degree <150torr, start oxygen decarburization, the O2 flow rate of the oxygen gun is 1200-1500Nm 3 / h, oxygen lance position is 1000-1550mm, oxygen blowing volume is 500-1000Nm 3 , the vacuum degree at the end of dynamic oxygen blowing is less than 50torr; S3, VCD treatment: start deep vacuum pumping, vacuum degree <1.0torr, bottom blowing stirring gas argon flow rate is 800-1500L / min, enter VCD stage>5min after adding 400-1200kg niobium concentrate, VCD treatment time>15min; S4, VOD reduction and vacuum breaking: add 500-1500kg of reducing materials, and 3000-4000kg of auxiliary materials to make slag, vacuum degree 20-150torr, bottom blowing argon 600-1500L / min for full stirring; reduction time>15min, measure temperature and take samples after vacuum breaking; S5. LF refining and CCM: After the VOD treatment, the composition and temperature of the molten steel are fine-tuned in LF, and then the molten steel in the ladle is transported to the continuous casting platform for casting to obtain the niobium-containing stainless steel ingot product.
2. The niobium alloying method for VOD smelting niobium-containing stainless steel according to claim 1, characterized in that: The reducing materials in step S4 are Al particles and FeSi alloy, and the auxiliary materials are lime and fluorite.