Preparation method of bainite steel rail and bainite steel rail
By controlling the cooling rate and heating process, combining universal rolling and stepping cold bed cooling, a fine bainite structure is formed, which solves the problem of uneven microstructure in the preparation of traditional bainite rails and improves the strength of the rails and resilience, meeting the high standards of modern railway transportation.
Patent Information
- Application Number
- CN202411207269.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-08-30
AI Technical Summary
The cooling rate in the traditional bainite rail preparation method is uncontrollable, resulting in uneven microstructure, affecting the strength, toughness and wear resistance of the rail, making it difficult to meet the high standards of modern railway transportation.
By using controlled cooling rate and heating technology, the universal rolling method and step-by-step cold bed cooling are used to form fine bainite structure, strengthen the strength and toughness of the rails, and promote the formation of nano-scale precipitation phases through the addition of Ti elements. Improve bainite transformation efficiency.
It achieves high strength, good toughness and wear resistance of bainite rails, meets the high standards of modern railway transportation, and extends the service life of the rails.
Smart Images

Figure CN118996080A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of rail manufacturing, and in particular relates to a method for preparing a bainite rail and a bainite rail obtained by using the method. Background Art
[0002] With the rapid development of the railway transportation industry, especially the continuous expansion of heavy-load transportation and high-speed railways, the performance requirements for rails are getting higher and higher. In the face of the growing transportation needs, traditional rail materials often cannot meet the high standards of modern railways due to problems such as insufficient strength, poor toughness, insufficient wear resistance or weak impact resistance. In order to improve the service performance and life of rails, the industry has been seeking to develop new rail materials with higher strength, better toughness, higher wear resistance and stronger impact resistance.
[0003] Bainitic steel has become a hot topic in rail material research due to its excellent combination of strength and toughness. The strength and toughness of bainitic rails are closely related to their microstructure. In actual production, the preparation of bainitic rails usually involves heating of continuous casting billets, heat treatment, multi-pass rolling and natural cooling. However, traditional preparation methods have many limitations, such as uncontrollable cooling rate, heterogeneous microstructure and unsatisfactory mechanical properties, which limit the further improvement of the performance of bainitic rails.
[0004] In the prior art, natural cooling is usually adopted after the rolling of bainitic rails. This process involves a wide temperature range, gradually decreasing from high temperature to room temperature. The rate of natural cooling varies throughout the cooling process, and the cooling rate changes from fast to slow as the temperature of the rail decreases. This cooling method may lead to insufficient transformation of bainite and the formation of non-bainite structures, such as proeutectoid ferrite, which affects the final performance of the rail. In addition, due to the change in cooling rate, bainite may present a variety of morphologies, such as needle-shaped, granular or block-shaped. These different morphologies have different effects on the performance of the rail.
[0005] In actual production, it is found that there are huge challenges in preparing bainitic rails with excellent comprehensive mechanical properties such as high strength, good toughness, wear resistance and impact resistance. Summary of the invention
[0006] In view of this, in order to solve the problems existing in the prior art, the present invention provides a method for preparing a bainitic rail and a bainitic rail obtained using the method, thereby providing technical support for obtaining a bainitic rail with excellent macroscopic properties (such as strength, toughness, wear resistance, corrosion resistance and impact resistance).
[0007] The technical solution adopted by the present invention is as follows: A first aspect of the present invention provides a method for preparing a bainite rail, comprising the following steps: Step S1: heating the continuous casting billet and performing a soaking treatment; Step S2: feeding the continuous casting billet into a rolling line for universal rolling, wherein the universal rolling includes billet opening, rough rolling, intermediate rolling and finish rolling, wherein the rough rolling has more than 3 passes, the intermediate rolling has more than 1 pass, the finish rolling has 1 pass, the rolling temperature of the last intermediate rolling pass is 930-960°C, the finish rolling temperature is controlled at 850-900°C, the rolling reduction ratio is ≥13:1, and the interval between the last two rolling passes is controlled within 30s; Step S3: performing controlled cooling on the rail, wherein the controlled cooling comprises cooling the rail to a first temperature at a first cooling rate, and then cooling the rail to a bainite transformation start temperature range at a second cooling rate, wherein the first cooling rate is greater than the second cooling rate; Step S4: Place the pre-bent rail on a step-type cooling bed to cool to room temperature.
[0008] According to one embodiment of the present invention, the continuous casting billet contains the following chemical components in mass percentage: C: 0.21%~0.25%; Si: 2.0%~2.5%; Mn: 0.60%~1.00%; Cr: 0.60%~0.80%; Mo: 0.40%~0.45%; N: 0.005%~0.008%; Ti: 0.08%~0.13%; the remainder is Fe and unavoidable impurities.
[0009] According to one embodiment of the present invention, Ti, C and N in the continuous casting billet satisfy the following chemical equivalent ratio: Ti / C is 3.95-4.00, and Ti / N≤3.42.
[0010] According to one embodiment of the present invention, the original austenite grain size of the continuous casting billet is 50-90 μm.
[0011] According to one embodiment of the present invention, in step S1, the heating rate is ≤400°C / h, the heating time is ≥180min, and after heating to 1150-1250°C, a soaking treatment is performed, the soaking temperature is 1100-1200°C, and the soaking time is ≥40min.
[0012] According to one embodiment of the present invention, in step S2, the starting rolling temperature of the universal rolling is 990-1000°C, and the rolling reduction ratio is ≥10:1.
[0013] According to one embodiment of the present invention, in step S3, the bainite transformation starting temperature range is 390-480°C.
[0014] According to one embodiment of the present invention, in step S3, the first temperature is 480°C, the first cooling rate is 3-5°C / s, and the second cooling rate is 0.3-0.5°C / s.
[0015] According to an embodiment of the present invention, the cooling rate of the rail in step S4 is 0.1-0.3° C. / s.
[0016] According to another aspect of the present invention, there is provided a bainite rail, wherein the bainite rail is prepared by the method described in any one of the above embodiments.
[0017] According to one embodiment of the present invention, the yield strength of the bainite rail is ≥1400 MPa, the tensile strength is ≥1450 MPa, the elongation at break is ≥15%, and the room temperature impact energy is ≥100 J.
[0018] The beneficial effects of the method for preparing bainite rails of the present invention compared with the prior art include at least one of the following: The present invention controls the hot rolling process so that the strain and deformation defects accumulated during rolling are retained, and deformed austenite grains are generated by rolling. The deformed austenite is ellipsoidal. During the bainite transformation, atoms diffuse to defects such as grain boundaries or dislocations in a short time, which are used as nucleation points to accelerate the bainite transformation. The first formed bainite subunits can promote the formation of new bainite subunits at the austenite / bainite interface, and the self-catalytic mechanism is accelerated. Since the density of defects accumulated during rolling is large, more bainite nucleation points are provided, which is conducive to the formation of fine bainite. In the present invention, during the rolling process, more strain-induced precipitation phase nucleation sites are introduced by rolling, so that nano-scale precipitation phases are precipitated in the matrix. The precipitation phases can be used as nucleation particles for bainite transformation to promote bainite transformation. The strain-induced precipitation phases enhance the autocatalytic effect by promoting the formation of bainite subunits, and at the same time, the carbon concentration of the remaining austenite is reduced by consuming carbon atoms, thereby reducing the thermal stability of the austenite and accelerating the formation of bainite. In addition, during the bainite transformation process, there is a competition mechanism between the precipitation of carbides and the bainite transformation. After the bainite transformation, a smaller precipitation phase is precipitated, which can pin dislocations in the bainite and the surrounding residual austenite, further enhancing the strength of the rail.
[0019] The present invention can obtain finer lath bainite structure by controlling the cooling path and accurately controlling the bainite transformation temperature range. Such fine bainite structure not only improves the strength of the rail, but also maintains good toughness and wear resistance. The method of the present invention achieves fine control of bainite microstructure by precisely controlling the heating, rolling and cooling processes and optimizing the design of chemical composition, thereby obtaining a bainite rail with excellent macroscopic properties. The present invention can not only improve the mechanical properties of the rail, but also extend its service life, meeting the high standard requirements of modern railway transportation for rails. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings in the following description are only some embodiments of the present invention. For ordinary technicians in this field, other embodiments can be obtained based on these drawings without paying creative work.
[0021] Figure 1 A flow chart of a method for preparing a bainite rail provided in some embodiments of the present invention; Figure 2 The microstructure diagram of the bainite rail prepared by the method of Example 2 is shown in FIG. DETAILED DESCRIPTION
[0022] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the embodiments of the present invention are further described in detail below in combination with specific embodiments and with reference to the accompanying drawings.
[0023] like Figure 1 As shown, the first aspect of the present invention provides a method for preparing a bainite rail, which generally comprises the following steps: Step S1: heating the continuous casting billet and performing a soaking treatment; Step S2: feeding the continuous casting billet into a rolling line for universal rolling, wherein the universal rolling includes billet opening, rough rolling, intermediate rolling and finishing rolling, wherein the number of rough rolling passes is more than 3, the number of intermediate rolling passes is more than 1, the number of finishing rolling passes is 1, the rolling temperature of the last intermediate rolling pass is 930-960°C, the temperature of finishing rolling is controlled at 850-900°C, the rolling reduction ratio is ≥13:1, and the interval time between the last two rolling passes is controlled within 30s; Step S3: performing controlled cooling on the rail, wherein the controlled cooling includes cooling the rail to a first temperature at a first cooling rate, and then cooling the rail to a bainite transformation start temperature range at a second cooling rate, wherein the first cooling rate is greater than the second cooling rate; Step S4: Place the pre-bent rail on a step-type cooling bed to cool to room temperature.
[0024] The preparation method of the present invention controls the hot rolling process so that the strain and deformation defects accumulated during rolling are retained, and the deformed austenite grains are generated by rolling. The deformed austenite is ellipsoidal. During the bainite transformation, atoms diffuse to defects such as grain boundaries or dislocations in a relatively short time, which are used as nucleation points to accelerate the bainite transformation. The first formed bainite subunit can promote the formation of new bainite subunits at the austenite / bainite interface, and the autocatalytic mechanism is accelerated. Since the defect density accumulated during rolling is large, it provides more bainite nucleation points, which is conducive to the formation of fine bainite. On the other hand, during the rolling process, more strain-induced precipitation phase nucleation sites are introduced by rolling, so that nano-scale precipitation phases are precipitated from the matrix. The precipitation phases can be used as nucleation points for bainite transformation to promote bainite transformation. The strain-induced precipitation phases enhance the autocatalytic effect by promoting the formation of bainite subunits, and at the same time reduce the carbon concentration of the remaining austenite by consuming carbon atoms, thereby reducing the thermal stability of the austenite and accelerating the formation of bainite. In addition, during the bainite transformation process, there is a competition mechanism between the precipitation of carbides and the transformation of bainite. After the bainite transformation, a smaller precipitate phase is precipitated, which can pin dislocations in the bainite and the surrounding residual austenite, further enhancing the strength of the rail. The bainite rail obtained by the method according to the present invention has excellent mechanical properties and a long service life, meeting the high standard requirements of modern railway transportation for rails.
[0025] In some embodiments, the continuous casting billet in step S1 contains the following chemical components in mass percentage: C: 0.21%~0.25%; Si: 2.0%~2.5%; Mn: 0.60%~1.00%; Cr: 0.60%~0.80%; Mo: 0.40%~0.45%; N: 0.005%~0.008%; Ti: 0.08%~0.13%; the remainder is Fe and unavoidable impurities.
[0026] Titanium (Ti), as an important microalloying element, plays a key role in bainitic rails. Ti forms titanium carbide (TiC) and titanium nitride (TiN) in steel. These fine dispersed precipitates are formed at grain boundaries and dislocations, which hinder the migration of grain boundaries through the pinning effect, significantly improving the strength and toughness of the rails. During the rolling stage, the strain-induced precipitation phenomenon significantly affects the recrystallization behavior of austenite. The addition of Ti can increase the recrystallization temperature of austenite, inhibit the recrystallization of austenite at lower rolling temperatures, maintain the deformation accumulation during rolling, and thus promote the formation of a higher number of dislocations after rolling. This accumulated deformation provides more nucleation points for the subsequent bainite transformation and reduces the energy barrier of bainite transformation, accelerating the bainite transformation process.
[0027] Ti is usually added to steel in trace amounts, and the content generally does not exceed 0.08wt%, which helps to form a large number of fine dispersed precipitates during the cooling process. The precipitates of Ti in steel are TiN and TiC. Ti exists in the form of carbides and nitrides in steel. Nanoscale fine dispersed precipitates can be formed at grain boundaries and dislocations, hindering the migration of grain boundaries through the pinning effect. Affecting the recrystallization behavior of austenite. During hot rolling, the Ti element can affect the recrystallization behavior of austenite. The precipitation of TiN or Ti (C, N) can inhibit the growth of austenite grains at high temperatures, thereby forming finer grains during the phase transformation process. Moreover, the Ti element can form heterogeneous precipitation at the phase interface between austenite and ferrite. This precipitation can hinder the movement of the phase interface, thereby affecting the grain size and distribution. Further, the addition of Ti can increase the recrystallization temperature of cold-rolled steel, which means that a higher temperature is required to start the recrystallization process, which helps to maintain a fine grain structure and defects such as dislocations in the crystal at a lower temperature. The ratio of Ti to C and Ti to N is crucial for the formation of nano-scale fine TiC and TiN precipitation phases, which have an important influence on the original austenite grain size. To this end, in some embodiments, the Ti, C, and N in the continuous casting billet are controlled to meet the following chemical equivalent ratio: Ti / C is 3.95-4.00, and Ti / N≤3.42.
[0028] Furthermore, the original austenite grain size of the continuous casting billet is 50~90μm. The original austenite grain size of the continuous casting billet is small, and grain refinement means more grain boundary area, providing more potential nucleation sites. The smaller original austenite grain size may promote the formation of finer bainite subunits. The already formed bainite subunits can promote the formation of new bainite subunits at the austenite / bainite interface. The smaller austenite grain size can increase the chance of autocatalytic nucleation, that is, the difference between the activation energy of grain boundary nucleation and the activation energy of autocatalytic nucleation is greater, which is conducive to the formation of fine bainite. The microstructure refinement of bainite can improve its strength, toughness, impact resistance, etc.
[0029] In some embodiments, in step S1, the heating rate is ≤400°C / h, the heating time is ≥180min, and after heating to 1150~1250°C, a soaking treatment is performed, the soaking temperature is 1100~1200°C, and the soaking time is ≥40min. Controlling the heating rate and time can avoid stress concentration and micro defects inside the material, help to obtain a uniform microstructure, thereby improving the uniformity and overall performance of the material. During the homogenization process, a portion of the titanium carbon and nitrides are redissolved into the matrix, and the Ti dissolved in the austenite can increase the recrystallization temperature, which is beneficial for rolling in the non-recrystallized austenite area. High-pressure water descaling can be performed after the soaking treatment.
[0030] In some embodiments, in step S2, the rolling is performed by universal rolling, and the universal rolling includes cogging, rough rolling, intermediate rolling and finishing rolling. For example, the mill layout adopts a seven-stand mode of 1-1-2-2-1, and the main mill area is composed of two reversible cogging mills (BD1, BD2), a universal rough rolling mill group (U1-E1), a universal and intermediate rolling mill group (U2-E2) and a universal finishing mill (UF).
[0031] The continuous cast rectangular billet is rolled through BD1 and BD2 and rolled into an H-shaped billet for rolling in the universal rolling mill in the pilot hole. In the universal rolling mill unit, the heavy rail is reversibly rolled in the tandem mill U1-E1 for multiple passes, for example, 3 passes in the universal roughing mill U1 and 2 passes in the edge rolling mill E1. The heavy rail is then rolled in the tandem mill U2-E2 for at least 1 pass, for example, 1 pass in both the universal roughing mill U2 and the edge rolling mill E2, and finally 1 pass in the universal finishing mill UF.
[0032] In some embodiments, the rolling start temperature is 990-1000°C, and the rolling reduction ratio is ≥10:1. The rough rolling passes are more than 3 passes, the intermediate rolling passes are more than 1 pass, the finishing rolling pass is 1 pass, the rolling temperature of the last intermediate rolling pass is 930-960°C, the finishing rolling temperature is controlled at 850-900°C, the interval time between the last two rolling passes is controlled within 30s, and the overall rolling reduction ratio is ≥13:1.
[0033] Starting rolling at less than 1000℃ and finishing rolling at 850~900℃, the rolling process introduces more nucleation sites for strain-induced precipitation phases, which ultimately leads to a higher nucleation rate and a shorter incubation time, accelerating the formation of precipitation phases. During hot rolling, the nano-precipitation phase of Ti consumes about 30%~40% of the total Ti content. The size of the nano-precipitation phase of Ti is about 30~80nm. Since Ti dissolved in austenite increases the recrystallization temperature, when the finishing rolling temperature is controlled at 850~900℃, rolling is carried out in the non-recrystallized austenite region. There is no recrystallization during rolling, so that the accumulated strain and deformation defects are retained, and deformed austenite grains are generated by rolling. Based on the original austenite grain size of 50~90μm in the continuous casting billet, the deformed austenite is ellipsoidal, with a short axis to long axis ratio of 1:3~1:5, and the nano-scale precipitation phases preferentially nucleate on dislocations and subgrains in the deformed austenite.
[0034] The deformation temperature of the last two rolling passes is controlled so that the rolling is carried out in the non-recrystallized austenite region, dynamic recrystallization during rolling is suppressed, the accumulated strain and deformation defects are retained, and deformed austenite grains are generated by rolling to facilitate the refinement of bainite structure. The interval time between the last two rolling passes is controlled within 30s to suppress static recrystallization, so that the accumulated strain and deformation defects are retained, which is conducive to the refinement of bainite structure.
[0035] In step S3, after the hot rolling is completed, the rail is subjected to controlled cooling, wherein the controlled cooling includes cooling the rail to a first temperature at a first cooling rate, and then cooling the rail to a bainite transformation start temperature range at a second cooling rate, wherein the first cooling rate is greater than the second cooling rate.
[0036] In some embodiments, the first cooling rate is 3-5°C / s, and the rail is cooled to 500°C at this cooling rate, and the cooling is accelerated to the bainite start transformation temperature. The Ti element can improve the stability of the supercooled austenite by delaying the formation of carbides in the eutectoid decomposition, thereby inhibiting the pearlite transformation. At the same time, the compressed air is used to accelerate the cooling to avoid the pearlite transformation before the bainite transformation. Below 480°C, the cooling rate is controlled at 0.3-0.5°C / s to enter the bainite transformation range from a suitable temperature point. The cooling path is controlled to obtain fine and uniform lath-shaped bainite and a small amount of film-shaped residual austenite.
[0037] In some embodiments, the bainite transformation start temperature range is 390-480° C. When the temperature is reduced to this temperature, the bainite structure begins to form.
[0038] In step S4, the pre-bent rail is placed on a step-type cooling bed to cool to room temperature. For example, the rail can be moved to the cooling bed for natural cooling, and the cooling rate can be controlled at 0.1-0.3°C / s. During the slow cooling process, the bainite transformation is completed.
[0039] After completing the above processing, the rail can be further sent to a horizontal and vertical composite straightening machine for straightening.
[0040] Through the grain size refinement of the continuous casting billet and the control of rolling without recrystallization, the austenite grains do not grow and generate deformed austenite grains, which achieves the effect of refining the austenite grain size before the bainite transformation. Grain refinement means that there are more grain boundary areas before the bainite transformation occurs, providing more potential nucleation sites, thereby refining the ferrite sheet. In addition, the smaller original austenite grain size will promote the formation of finer bainite subunits. The already formed bainite subunits can promote the formation of new bainite subunits at the austenite / bainite interface, accelerating the autocatalytic mechanism. The smaller austenite grain size can increase the chance of autocatalytic nucleation, that is, the difference between the activation energy of grain boundary nucleation and the activation energy of autocatalytic nucleation is greater. Since there is no recrystallization in the hot rolling process, the accumulated deformation leads to a higher dislocation density. Dislocations can serve as effective sites for bainite nucleation. The presence of dislocations reduces the energy barrier required for bainite nucleation, thereby accelerating the formation of bainite.
[0041] In addition, the strain-induced precipitation phase generated during hot rolling can act as nucleation points for bainite transformation, and the dislocation- and strain-induced precipitation phases promote the formation of bainite subunits to enhance the autocatalytic effect. At the same time, the carbon concentration of the remaining austenite is reduced by consuming carbon atoms, thereby reducing the thermal stability of austenite and accelerating the formation of bainite.
[0042] Bainite generated from the transformation of deformed austenite can effectively fix the defects of deformed austenite. Atoms diffuse to nucleation points such as grain boundaries or dislocations in a short time to accelerate the transformation of bainite. There is a competitive mechanism between the precipitation of carbides and the transformation of bainite. Carbides precipitate after the transformation of bainite, so that smaller precipitates are pinned on the dislocations of bainite and the surrounding residual austenite, further enhancing the strength of the rail.
[0043] Another aspect of the present invention provides a bainite rail, which is prepared by the method described in the above embodiment.
[0044] In some embodiments, the yield strength of the bainitic rail is ≥1400 MPa, the tensile strength is ≥1450 MPa, the elongation at break is ≥15%, and the room temperature impact energy is ≥100 J.
[0045] In order to further illustrate the technical solution and beneficial effects of the present invention, the present invention also provides the following specific embodiments.
[0046] Example 1 In this embodiment, the bainite rail contains the following chemical components by mass percentage: C: 0.21%; Si: 2.0%; Mn: 0.60%; Cr: 0.60%; Mo: 0.40%; N: 0.005%; Ti: 0.08%; the remainder is Fe and inevitable impurities. The original austenite grain size of the continuous casting slab is 50 μm.
[0047] The continuous casting billet meeting the above components is heated to 1150℃ at a heating rate of 400℃ / h, and is soaked for 60min. After soaking treatment, high-pressure water descaling is performed. The square continuous casting billet is sent to the rolling line for rolling, and the seven-stand mode is used for universal rolling. The starting rolling temperature is 990℃, the rolling reduction ratio is 10:1, and the H-shaped rail billet is rolled into a rail-shaped billet. The rail-shaped billet is reversibly rolled for 3 passes in the universal edge rolling rough rolling unit, rolled for 2 passes in the universal edge rolling medium rolling unit, and finally rolled for 1 pass in the universal finishing mill. The temperature of the last intermediate rolling is controlled at 930℃, and the temperature of the finishing rolling is controlled at 850℃. The interval time between the last two rolling passes is controlled within 30s, and the rolling reduction ratio is 14:1. The rail is then sprayed with compressed air to cool it to 480℃ at a cooling rate of 3℃ / s, and then cooled to 390℃ at a cooling rate of 0.3℃ / s. The pre-bent rails are then placed on a step-type cooling bed and cooled to room temperature of 20-30°C at a cooling rate of 0.1°C / s, and then placed in a horizontal and vertical composite straightening machine for straightening.
[0048] After testing, the yield strength of the bainitic rail is about 1420MPa, the tensile strength is about 1460MPa, the elongation at break is about 15%, and the impact energy at room temperature is about 105J.
[0049] Example 2 In this embodiment, the bainite rail contains the following chemical components by mass percentage: C: 0.23%; Si: 2.3%; Mn: 0.80%; Cr: 0.70%; Mo: 0.42%; N: 0.006%; Ti: 0.11%; the remainder is Fe and inevitable impurities. The original austenite grain size of the continuous casting slab is 70 μm.
[0050] The continuous casting billet meeting the above components is heated to 1200℃ at a heating rate of 390℃ / h, and is soaked for 50min. After soaking treatment, high-pressure water descaling is performed. The square continuous casting billet is sent to the rolling line for rolling, and the seven-stand mode is used for universal rolling. The starting rolling temperature is 995℃, the rolling reduction ratio is 11:1, and the H-shaped rail billet is rolled into a rail-shaped billet. The rail-shaped billet is reversibly rolled for 3 passes in the universal edge rolling rough rolling unit, rolled for 1 pass in the universal edge rolling medium rolling unit, and finally rolled for 1 pass in the universal finishing mill. The intermediate rolling temperature is controlled at 940℃, the finishing rolling temperature is controlled at 880℃, and the interval time between the last two rolling passes is controlled within 30s, and the rolling reduction ratio is 13:1. The rail is then sprayed with compressed air to cool to 480℃ at a cooling rate of 4℃ / s, and then cooled to 430℃ at a cooling rate of 0.4℃ / s. The pre-bent rails are then placed on a step-type cooling bed and cooled to room temperature of 20-30°C at a cooling rate of 0.2°C / s, and then placed in a horizontal and vertical composite straightening machine for straightening.
[0051] After testing, the yield strength of the bainitic rail is 1450MPa, the tensile strength is 1470MPa, the elongation at break is 18%, and the impact energy at room temperature is 130J. Figure 2 The microstructure of the bainite rail prepared by the method is shown. In the figure, the green is a film-like retained austenite, and the rest is thin lath-like bainite. The bainite structure is fine and uniform.
[0052] Example 3 In this embodiment, the bainite rail contains the following chemical components by mass percentage: C: 0.25%; Si: 2.5%; Mn: 1.00%; Cr: 0.80%; Mo: 0.45%; N: 0.008%; Ti: 0.13%; the remainder is Fe and inevitable impurities. The original austenite grain size of the continuous casting slab is 90 μm.
[0053] The continuous casting billet meeting the above components is heated to 1250℃ at a heating rate of 380℃ / h, soaked for 40min, and descaled with high-pressure water after soaking treatment. The square continuous casting billet is sent to the rolling line for rolling, and the seven-stand mode is used for universal rolling. The starting rolling temperature is 1000℃, the rolling reduction ratio is 12:1, and the H-shaped rail billet is rolled into a rail-shaped billet. The rail-shaped billet is reversibly rolled for 3 passes in the universal edge rolling rough rolling unit, rolled for 2 passes in the universal edge rolling medium rolling unit, and finally rolled for 1 pass in the universal finishing mill. The temperature of the last intermediate rolling is controlled at 960℃, and the temperature of the finishing rolling is controlled at 900℃. The interval time between the last two rolling passes is controlled within 30s, and the rolling reduction ratio is 13:1. The rail is then sprayed with compressed air to cool it to 480℃ at a cooling rate of 5℃ / s, and then cooled to 480℃ at a cooling rate of 0.5℃ / s. The pre-bent rails are then placed on a step-type cooling bed and cooled to room temperature of 20-30°C at a cooling rate of 0.3°C / s, and then placed in a horizontal and vertical composite straightening machine for straightening.
[0054] After testing, the yield strength of the bainitic rail was 1460MPa, the tensile strength was 1480MPa, the elongation at break was 16%, and the impact energy at room temperature was 125J.
[0055] Comparative Example 1 In this comparative example, the bainite rail contains the following chemical components by mass percentage: C: 0.23%; Si: 2.3%; Mn: 0.80%; Cr: 0.70%; Mo: 0.42%; N: 0.006%; Ti: 0.11%; the remainder is Fe and unavoidable impurities. The original austenite grain size of the continuous casting slab is 70 μm.
[0056] The continuous casting billet meeting the above components is heated to 1200℃ at a heating rate of 390℃ / h, and is soaked for 50min. After soaking treatment, high-pressure water descaling is performed. The square continuous casting billet is sent to the rolling line for rolling, and the seven-stand mode is used for universal rolling. The starting rolling temperature is 1050℃, the rolling reduction ratio is 11:1, and it is rolled into an H-shaped rail billet. The rail billet is reversibly rolled for 3 times in the universal edge rolling rough rolling unit, rolled for 1 time in the universal edge rolling medium rolling unit, and finally rolled for 1 time in the universal finishing mill. The final rolling temperature is controlled at 980℃, and the rolling reduction ratio is 13:1. Compressed air is sprayed on the rail to cool it to 480℃ at a cooling rate of 4℃ / s, and then cooled to 430℃ at a cooling rate of 0.4℃ / s. The pre-bent rails are then placed on a step-type cooling bed and cooled to room temperature of 20-30°C at a cooling rate of 0.2°C / s, and then placed in a horizontal and vertical composite straightening machine for straightening.
[0057] After testing, the yield strength of the bainite rail is 1150 MPa, the tensile strength is 1070 MPa, the elongation at break is 12%, and the room temperature impact energy is 85 J. In this comparative example, due to the high final rolling temperature, dynamic recrystallization occurs during rolling, and the rolling defects disappear during the recrystallization process, which cannot provide more nucleation points for the subsequent bainite transformation, and thus cannot use the accumulation of rolling defects to refine the bainite structure.
[0058] Comparative Example 2 In this comparative example, the bainite rail contains the following chemical components by mass percentage: C: 0.23%; Si: 2.3%; Mn: 0.80%; Cr: 0.70%; Mo: 0.42%; N: 0.006%; the remainder is Fe and inevitable impurities. The original austenite grain size of the continuous casting slab is 70 μm.
[0059] The continuous casting billet meeting the above components is heated to 1200℃ at a heating rate of 390℃ / h, and is soaked for 50min. After soaking treatment, high-pressure water descaling is performed. The square continuous casting billet is sent to the rolling line for rolling, and the seven-stand mode is used for universal rolling. The starting rolling temperature is 995℃, the rolling reduction ratio is 11:1, and the H-shaped rail billet is rolled into a rail-shaped billet. The rail-shaped billet is reversibly rolled for 3 passes in the universal edge rolling rough rolling unit, rolled for 1 pass in the universal edge rolling medium rolling unit, and finally rolled for 1 pass in the universal finishing mill. The intermediate rolling temperature is controlled at 940℃, the finishing rolling temperature is controlled at 880℃, and the interval time between the last two rolling passes is controlled within 30s, and the rolling reduction ratio is 13:1. The rail is then sprayed with compressed air to cool to 480℃ at a cooling rate of 4℃ / s, and then cooled to 430℃ at a cooling rate of 0.4℃ / s. The pre-bent rails are then placed on a step-type cooling bed and cooled to room temperature of 20-30°C at a cooling rate of 0.2°C / s, and then placed in a horizontal and vertical composite straightening machine for straightening.
[0060] After testing, the yield strength of the bainitic rail is 1320MPa, the tensile strength is 1350MPa, the elongation at break is 16%, and the impact energy at room temperature is 120J. In this comparative example, since the chemical composition of the continuous casting billet does not contain Ti, the recrystallization temperature during hot rolling is lower than that of the Ti-containing rail. Therefore, the rolling defects of the last few passes will decrease with the recovery of recrystallization, and it is impossible to provide more nucleation points for the subsequent bainite transformation, and thus it is impossible to use the accumulation of rolling defects to refine the bainite structure. In addition, the lack of Ti also leads to the lack of titanium carbonitrides in the matrix, the reduction of precipitation phases, and the reduction of the mechanical properties of the rail.
[0061] Comparative Example 3 In this comparative example, the bainite rail contains the following chemical components in mass percentage: C: 0.23%, Si: 2.3%, Mn: 0.80%, Cr: 0.70%, Mo: 0.42%, N: 0.006%, Ti: 0.11%, and the balance is Fe and inevitable impurities.
[0062] The continuous casting billet meeting the above components is heated to 1200℃ at a heating rate of 390℃ / h, and is soaked for 50min. After soaking treatment, high-pressure water descaling is performed. The square continuous casting billet is sent to the rolling line for rolling, and the seven-stand mode is used for universal rolling. The starting rolling temperature is 995℃, the rolling reduction ratio is 11:1, and it is rolled into an H-shaped rail billet. The rail billet is reversibly rolled for 3 passes in the universal edge rolling rough rolling unit, rolled for 1 pass in the universal edge rolling medium rolling unit, and finally rolled for 1 pass in the universal finishing mill. The medium rolling temperature is controlled at 940℃, the finishing temperature is controlled at 880℃, and the interval time between the last two rolling passes is controlled within 30s, and the rolling reduction ratio is 13:1. Compressed air is then sprayed on the rail to cool it to 430℃ at a cooling rate of 0.8℃ / s. The pre-bent rails are then placed on a step-type cooling bed and cooled to room temperature of 20-30°C at a cooling rate of 0.2°C / s, and then placed in a horizontal and vertical composite straightening machine for straightening.
[0063] After testing, the yield strength of the bainite rail is 880MPa, the tensile strength is 892MPa, the elongation at break is 12%, and the impact energy at room temperature is 45J. In this comparative example, due to the low cooling rate after final rolling, the rail forms ferrite and pearlite structures before the bainite transformation, and the temperature is too high when entering the bainite transformation zone, resulting in granular bainite. These undesirable structures reduce the mechanical properties of the rail.
[0064] The technical features of the above embodiments may be combined arbitrarily. To make the description concise, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0065] The above-mentioned embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the patent of the present application shall be subject to the attached claims.
Claims
1. A method for preparing a bainite rail, It is characterized in that The steps include: Step S1: heating the continuous casting billet and performing a soaking treatment; Step S2: feeding the continuous casting billet into a rolling line for universal rolling, wherein the universal rolling includes billet opening, rough rolling, intermediate rolling and finish rolling, wherein the rough rolling has more than 3 passes, the intermediate rolling has more than 1 pass, the finish rolling has 1 pass, the rolling temperature of the last intermediate rolling pass is 930-960°C, the finish rolling temperature is controlled at 850-900°C, the rolling reduction ratio is ≥13:1, and the interval between the last two rolling passes is controlled within 30s; Step S3: performing controlled cooling on the rail, wherein the controlled cooling comprises cooling the rail to a first temperature at a first cooling rate, and then cooling the rail to a bainite transformation start temperature range at a second cooling rate, wherein the first cooling rate is greater than the second cooling rate; Step S4: Place the pre-bent rail on a step-type cooling bed to cool to room temperature.
2. The method for preparing a bainite rail according to claim 1, It is characterized in that The continuous casting slab comprises the following chemical components by mass percentage: C: 0.21%-0.25%; Si: 2.0%-2.5%; Mn: 0.60%-1.00%; Cr: 0.60%-0.80%; Mo: 0.40%-0.45%; N: 0.005%-0.008%; Ti: 0.08%-0.13%; the remainder is Fe and unavoidable impurities.
3. The method for preparing a bainite rail according to claim 2, It is characterized in that The Ti, C and N in the continuous casting billet satisfy the following chemical equivalent ratio: Ti / C is 3.95-4.00, and Ti / N≤3.
42.
4. The method for preparing a bainite rail according to claim 2, It is characterized in that The original austenite grain size of the continuous casting billet is 50-90 μm.
5. The method for preparing a bainite rail according to claim 1, It is characterized in that In step S1, the heating rate is ≤400°C / h, the heating time is ≥180min, and after heating to 1150-1250°C, a soaking treatment is performed, the soaking temperature is 1100-1200°C, and the soaking time is ≥40min.
6. The method for preparing a bainite rail according to claim 1, It is characterized in that In step S2, the starting rolling temperature of the universal rolling is 990-1000°C, and the rolling reduction ratio is ≥10:
1.
7. The method for preparing a bainite rail according to claim 2, It is characterized in that In step S3, the bainite transformation starting temperature range is 390-480°C.
8. The method for preparing a bainite rail according to claim 1, It is characterized in that In step S3, the first temperature is 480°C, the first cooling rate is 3-5°C / s, and the second cooling rate is 0.3-0.5°C / s.
9. The method for preparing a bainite rail according to claim 1, It is characterized in that The cooling rate of the rail in step S4 is 0.1-0.3°C / s.
10. A bainitic rail, It is characterized in that The bainite rail is prepared by the method according to any one of claims 1 to 8.
Citation Information
Patent Citations
High strength bainitic steel rail and heat treatment process thereof
CN103160736A
Hot-rolled ultrahigh-strength steel plate with tensile strength of 1000MPa and preparation method thereof
CN115354237A
B and Ti microalloyed hot-rolled bainite steel rail and manufacturing method thereof
CN117327985A
Bainite steel rail with excellent anti-fatigue performance and its production method
CN1978690A
Production of high-strength and high-toughness bainite rail having excellent surface damage resistance
JP1995034132A