Method for comprehensively extracting and utilizing multiple metals in platinum-palladium concentrate

Through the smelting and blowing of platinum-palladium concentrate, combined with atmospheric pressure and pressurized leaching technology, the problems of large slag volume and low recovery rate of precious metals in the existing process are solved, and the efficiency of nickel, copper, cobalt and various precious metals is achieved. Recycle and simplify process flow.

CN118996142APending Publication Date: 2024-11-22BEIJING MINING & METALLURGICAL TECH GRP CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411200341.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing platinum-palladium concentrate recycling process has problems such as large slag volume, low precious metal recovery rate or complex process, and it is difficult to effectively recover various precious metals such as nickel, copper, cobalt, gold, silver, platinum, and palladium.

Method used

The high-ice nickel is prepared by smelting and blowing of platinum-palladium concentrate, and the steps of extracting nickel, cobalt and precious metals are respectively obtained through the steps of normal pressure leaching, pressurized leaching, decomposition and pyrolysis to achieve effective recycling of nickel, copper and cobalt. It also improves the recovery rate of precious metals, while reducing the amount of slag and simplifying the process flow.

Benefits of technology

The efficient recycling of nickel, copper, cobalt and precious metals (such as gold, silver, platinum, palladium, osmium, ruthenium, rhodium, iridium) has been achieved, which significantly improves the recovery rate of precious metals, reduces the amount of slag, and simplifies the process flow.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118996142A_ABST
    Figure CN118996142A_ABST
Patent Text Reader

Abstract

The invention provides a method for comprehensively extracting and utilizing multiple metals in platinum-palladium concentrate, and relates to the field of metallurgy. The method for comprehensively extracting and utilizing the multiple metals in the platinum-palladium concentrate comprises the following steps: smelting and blowing the platinum-palladium concentrate to prepare high-grade matte nickel; the high-grade matte nickel and a first acid solution are subjected to normal-pressure leaching, a normal-pressure leaching solution and normal-pressure leaching residues are obtained, the normal-pressure leaching solution is subjected to purification, impurity removal and evaporative crystallization to obtain a nickel product and purified residues, and the purified residues are subjected to acid dissolution, extraction and pyrolysis to obtain a cobalt product; the atmospheric pressure leaching residues and a second acid solution are subjected to first-stage pressure leaching, and first-stage pressure leaching liquid and first-stage pressure leaching residues are obtained; and the first-stage pressure leaching residues and a third acid solution are subjected to second-stage pressure leaching, precious metal residues and second-stage pressure leaching liquid are obtained, and the second-stage pressure leaching liquid is purified, evaporated and crystallized to obtain a copper product. The method can realize comprehensive extraction and utilization of various metals in the platinum-palladium ore, and has the advantages of small slag amount, high precious metal recovery rate, simple process flow and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of metallurgy, and in particular to a method for comprehensive extraction and utilization of multiple metals in platinum-palladium concentrate. Background Art

[0002] Platinum-palladium concentrate is rich in nickel, copper, cobalt, gold, silver, platinum and palladium. Existing recycling processes, whether traditional roasting and leaching or full wet leaching, or pyrometallurgical processes focusing on base metal recovery, often have problems such as large slag volume, low precious metal recovery rate or complex recovery process.

[0003] Therefore, there is an urgent need to develop a new recycling method that can comprehensively recover nickel, copper, cobalt, as well as precious metals such as gold, silver, platinum, and palladium, while reducing the amount of slag, increasing the recovery rate of precious metals, and simplifying the process. Summary of the invention

[0004] The purpose of this application is to provide a method for comprehensive extraction and utilization of multiple metals in platinum-palladium concentrate to solve the above-mentioned problems.

[0005] To achieve the above objectives, this application adopts the following technical solutions: A method for comprehensive extraction and utilization of multiple metals in platinum-palladium concentrate, comprising: Smelting and blowing platinum-palladium concentrate to prepare high-grade nickel matte; The high-matte nickel is mixed with the first acid solution, and leached at normal pressure, wherein the endpoint pH of the normal pressure leaching is 4-7, to obtain a normal pressure leaching solution and a normal pressure leaching residue, wherein the normal pressure leaching solution is purified and impurities are removed, and then evaporated and crystallized to obtain a nickel product and a purified residue, and the purified residue is prepared by acid dissolution-extraction-pyrolysis to obtain a cobalt product; The atmospheric pressure leaching residue is mixed with the second acid solution, and the first stage pressure leaching is performed to obtain the first stage pressure leaching solution and the first stage pressure leaching residue, and the first stage pressure leaching solution is returned to perform the atmospheric pressure leaching; The first stage pressure leaching residue is mixed with the third acid solution, and the second stage pressure leaching is carried out to obtain precious metal slag and the second stage pressure leaching liquid. The second stage pressure leaching liquid is purified and evaporated and crystallized to obtain a copper product and a copper product crystallization liquid. The copper product crystallization liquid is returned to the normal pressure leaching. The precious metal slag is treated to obtain gold, silver, platinum, palladium, osmium, ruthenium, rhodium and iridium precious metals.

[0006] According to an embodiment of the present application, the smelting and blowing of platinum-palladium concentrate to prepare high-grade nickel matte comprises: smelting the platinum-palladium concentrate with a flux to obtain low-grade nickel matte containing copper and nickel; blowing the low-grade nickel matte and silicon dioxide to obtain high-grade nickel matte and blowing slag, and returning the blowing slag for the smelting; And / or, the flux includes one or more of silica, hematite, and lime; and / or, the mass of the flux is 20-40% of the mass of the platinum-palladium concentrate; And / or, the smelting temperature is 1350-1450°C; And / or, the smelting time is 20-60 min; And / or, the mass of the silicon dioxide is 20-40% of the mass of the low nickel matte; And / or, the blowing temperature is 1200-1400°C; And / or, the blowing time is 2-12 h; And / or, the blowing air flow rate of the blowing is 1-4 Nm 3 / h.

[0007] According to an embodiment of the present application, the first acid solution includes a sulfuric acid solution; And / or, the temperature of the atmospheric pressure leaching is 50-95°C; And / or, the normal pressure leaching time is 3-10 h; And / or, the liquid-to-solid ratio of the first acid solution and the high nickel matte is 2-12 L / kg.

[0008] According to an embodiment of the present application, the purification and impurity removal of the atmospheric pressure leachate includes: adding a barium compound to the atmospheric pressure leachate to remove lead, adding black nickel to remove cobalt, obtaining a filtrate and a purified slag, and the filtrate is evaporated and crystallized to obtain a nickel product.

[0009] According to an embodiment of the present application, the barium compound includes one or more of barium carbonate, barium chloride, barium sulfide, barium nitrate, and barium hydroxide.

[0010] According to an embodiment of the present application, the molar ratio of the barium compound to the lead in the atmospheric pressure leaching solution is 50-500.

[0011] According to an embodiment of the present application, the molar ratio of the black nickel to the cobalt in the atmospheric pressure leaching solution is 2-20.

[0012] According to an embodiment of the present application, the initial acidity of the first stage of pressure leaching is 10-30 g / L, and the initial acidity of the first stage of pressure leaching refers to: the concentration of the second acid solution in the feed solution obtained after the atmospheric pressure leaching residue is mixed with the second acid solution; and / or, the second acid solution comprises a sulfuric acid solution; and / or, the temperature of the first stage of pressure leaching is 140-170°C; And / or, the first stage of pressure leaching time is 1-3 h; and / or, the liquid-to-solid ratio of the second acid solution to the atmospheric pressure leaching residue is 4-10 L / kg; And / or, the oxygen partial pressure of the first stage of pressure leaching is 0.05-0.3 MPa.

[0013] According to an embodiment of the present application, the initial acidity of the second stage of pressure leaching is 20-40 g / L, and the initial acidity of the second stage of pressure leaching refers to: the concentration of the third acid solution in the feed solution obtained after the first stage of pressure leaching residue is mixed with the third acid solution; and / or, the third acid solution comprises a sulfuric acid solution; and / or, the temperature of the second stage of pressure leaching is 160-180°C; And / or, the second stage of pressure leaching time is 1-3 h; and / or, the liquid-to-solid ratio of the third acid solution to the first stage pressure leaching residue is 4-10 L / kg; And / or, the oxygen partial pressure of the second stage of pressure leaching is 0.05-0.5 MPa.

[0014] According to an embodiment of the present application, the purification of the second-stage pressurized leaching solution includes: adding one or more of alkali and alkaline solution to the second-stage pressurized leaching solution.

[0015] Compared with the prior art, the beneficial effects of this application include: The present application proposes a method for comprehensive extraction and utilization of multiple metals in platinum-palladium concentrate. The method smelts and blows the platinum-palladium concentrate, uses pyrometallurgical technology to obtain high-matte nickel, and then uses a hydrometallurgical process to perform atmospheric leaching, impurity removal, crystallization and pyrolysis to extract nickel products and cobalt products respectively. Then, the leachate and precious metal slag are obtained by the first stage of pressure leaching and the second stage of pressure leaching. The leachate is purified, evaporated and crystallized to obtain a copper product, and the precious metal slag is used to recover precious metals such as gold, silver, platinum, palladium, osmium, ruthenium, rhodium, and iridium. This method solves the problem that the traditional pyrometallurgical process focuses on the recovery of nickel and copper while ignoring precious metals, and also overcomes the problem of large slag volume and high processing difficulty when the traditional hydrometallurgical process recovers precious metals. After pyrometallurgy, nickel, copper, cobalt and precious metals are effectively enriched, while iron and gangue enter the slag and are separated. The high-grade nickel matte obtained by pyrometallurgy is then subjected to hydrometallurgy, which not only realizes the effective recovery of nickel, copper and cobalt, but also greatly improves the recovery rate of precious metals, while significantly reducing the amount of slag and simplifying the process. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope of the present application.

[0017] Figure 1This is a flow chart of the method for comprehensive extraction and utilization of multiple metals in platinum-palladium concentrate in Example 1 of the present application. DETAILED DESCRIPTION

[0018] As used herein: When an amount, concentration, or other value or parameter is expressed as a range, a preferred range, or a range defined by a series of upper preferred values ​​and lower preferred values, this should be understood as specifically disclosing all ranges formed by any pairing of any range upper limit or preferred value with any range lower limit or preferred value, regardless of whether the range is disclosed separately. For example, when a range of "1 to 5" is disclosed, the described range should be interpreted as including ranges "1 to 4", "1 to 3", "1 to 2", "1 to 2 and 4 to 5", "1 to 3 and 5", etc. When a numerical range is described in this article, unless otherwise stated, the range is intended to include its end values ​​and all integers and fractions within the range.

[0019] "And / or" is used to indicate that one or both of the stated situations may occur, for example, A and / or B includes (A and B) and (A or B).

[0020] The terms "first", "second" and "third" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the quantity of the indicated technical features.

[0021] The present application provides a method for comprehensive extraction and utilization of multiple metals in platinum-palladium concentrate, comprising: Smelting and blowing platinum-palladium concentrate to prepare high-grade nickel matte; The high-matte nickel is mixed with the first acid solution, and leached at normal pressure, wherein the endpoint pH of the normal pressure leaching is 4-7, to obtain a normal pressure leaching solution and a normal pressure leaching residue, wherein the normal pressure leaching solution is purified and impurities are removed, and then evaporated and crystallized to obtain a nickel product and a purified residue, and the purified residue is prepared by acid dissolution-extraction-pyrolysis to obtain a cobalt product; The atmospheric pressure leaching residue is mixed with the second acid solution, and the first stage pressure leaching is performed to obtain the first stage pressure leaching solution and the first stage pressure leaching residue, and the first stage pressure leaching solution is returned to perform the atmospheric pressure leaching; The first stage pressure leaching residue is mixed with the third acid solution, and the second stage pressure leaching is carried out to obtain precious metal slag and the second stage pressure leaching liquid. The second stage pressure leaching liquid is purified and evaporated and crystallized to obtain a copper product and a copper product crystallization liquid. The copper product crystallization liquid is returned to the normal pressure leaching. The precious metal slag is treated to obtain gold, silver, platinum, palladium, osmium, ruthenium, rhodium and iridium precious metals.

[0022] The method of the present application can separate and refine nickel, cobalt, copper, gold, silver, platinum, palladium, osmium, ruthenium, rhodium and iridium in platinum-palladium ore, and realize the comprehensive utilization of platinum-palladium concentrate. Moreover, the method of the present application also significantly reduces the amount of slag, greatly improves the recovery rate of precious metals, and simplifies the process flow.

[0023] The endpoint pH of atmospheric pressure leaching in this application is 4-7; For example, the endpoint pH of atmospheric pressure leaching can be 4, 5, 6, 7 or any value between 4 and 7.

[0024] Furthermore, the polymetallic elements in the platinum-palladium concentrate refer to nickel, cobalt, copper, gold, silver, platinum, palladium, osmium, ruthenium, rhodium and iridium in the platinum-palladium concentrate.

[0025] According to an embodiment of the present application, the smelting and blowing of platinum-palladium concentrate to prepare high-grade nickel matte comprises: smelting the platinum-palladium concentrate with a flux to obtain low-grade nickel matte containing copper and nickel; blowing the low-grade nickel matte and silicon dioxide to obtain high-grade nickel matte and blowing slag, and returning the blowing slag for the smelting; And / or, the flux includes one or more of silica, hematite, and lime; and / or, the mass of the flux is 20-40% of the mass of the platinum-palladium concentrate; Exemplarily, the mass of the flux is 20%, 25%, 30%, 35%, 40% or any value between 20-40% of the mass of the platinum-palladium concentrate.

[0026] And / or, the smelting temperature is 1350-1450°C; Illustratively, the smelting temperature may be 1350°C, 1360°C, 1370°C, 1380°C, 1390°C, 1400°C, 1410°C, 1420°C, 1430°C, 1440°C, 1450°C, or any value between 1350-1450°C.

[0027] And / or, the smelting time is 20-60 min; Exemplarily, the smelting time may be 20 min, 30 min, 40 min, 50 min, 60 min or any value between 20-60 min.

[0028] And / or, the mass of the silicon dioxide is 20-40% of the mass of the low nickel matte; Exemplarily, the mass of the silicon dioxide is 20%, 30%, 40% or any value between 20-40% of the mass of the nickel matte.

[0029] And / or, the blowing temperature is 1200-1400°C; Illustratively, the blowing temperature may be 1200°C, 1250°C, 1300°C, 1350°C, 1400°C or any value between 1200-1400°C.

[0030] And / or, the blowing time is 2-12 h; Exemplarily, the blowing time may be 2 h, 4 h, 6 h, 8 h, 10 h, 12 h or any value between 2 and 12 h.

[0031] And / or, the blowing air flow rate of the blowing is 1-4 Nm 3 / h; For example, the blowing flow rate of the blowing air can be 1 Nm 3 / h, 2 Nm 3 / h, 3 Nm 3 / h, 4 Nm 3 / h or 1-4 Nm 3 Any value between / h.

[0032] According to an embodiment of the present application, the first acid solution includes a sulfuric acid solution; And / or, the temperature of the atmospheric pressure leaching is 50-95°C; Illustratively, the temperature of the atmospheric pressure leaching can be 50°C, 55°C, 60°C, 65°C, 70°C, 75°C, 80°C, 85°C, 90°C, 95°C or any value between 50-95°C.

[0033] And / or, the normal pressure leaching time is 3-10 h; Exemplarily, the normal pressure leaching time can be 3 h, 4 h, 5 h, 6 h, 7 h, 8 h, 9 h, 10 h or any value between 3-10 h.

[0034] and / or, the liquid-to-solid ratio of the first acid solution to the high nickel matte is 2-12 L / kg; Exemplarily, the liquid-to-solid ratio of the first acid solution to the nickel matte can be 2 L / kg, 4 L / kg, 6 L / kg, 8 L / kg, 10 L / kg, 12 L / kg or any value between 2-12 L / kg.

[0035] Through atmospheric pressure leaching, nickel, cobalt, copper, iron and precious metals can be selectively separated. The metal phases of nickel, iron, cobalt, etc. in high-grade nickel matte are leached to prevent the metal phases from entering the subsequent pressurization process to react and produce hydrogen and cause explosion. The endpoint pH of atmospheric pressure leaching is controlled, and the copper and iron in the leachate enter the atmospheric pressure leaching slag through precipitation. The precious metals are retained in the atmospheric pressure leaching slag because they do not participate in the reaction and enter the subsequent first stage of pressure leaching process.

[0036] According to an embodiment of the present application, the purification and impurity removal of the atmospheric pressure leachate includes: adding a barium compound to the atmospheric pressure leachate to remove lead, adding black nickel to remove cobalt, obtaining a filtrate and a purified slag, and the filtrate is evaporated and crystallized to obtain a nickel product.

[0037] According to an embodiment of the present application, the barium compound includes one or more of barium carbonate, barium chloride, barium sulfide, barium nitrate, and barium hydroxide.

[0038] According to an embodiment of the present application, the molar ratio of the barium compound to the lead in the atmospheric pressure leaching solution is 50-500; Illustratively, the molar ratio of the barium compound to the lead in the atmospheric pressure leachate may be 50, 100, 150, 200, 250, 300, 350, 400, 450, 500 or any value between 50-500.

[0039] According to an embodiment of the present application, the molar ratio of the black nickel to the cobalt in the atmospheric pressure leaching solution is 2-20; For example, the molar ratio of the black nickel to the cobalt in the atmospheric pressure leaching solution may be 2, 4, 6, 8, 10, 12, 14, 16, 18, 20 or 2-20 (Ni 3+ / Co molar ratio).

[0040] According to an embodiment of the present application, the initial acidity of the first stage of pressure leaching is 10-30 g / L, and the initial acidity of the first stage of pressure leaching refers to: the concentration of the second acid solution in the feed solution obtained after the atmospheric pressure leaching residue is mixed with the second acid solution; Illustratively, the initial acidity of the first stage of pressure leaching can be 10 g / L, 15 g / L, 20 g / L, 25 g / L, 30 g / L or any value between 10-30 g / L.

[0041] and / or, the second acid solution comprises a sulfuric acid solution; and / or, the temperature of the first stage of pressure leaching is 140-170°C; Illustratively, the temperature of a stage of the pressure leaching may be 140°C, 145°C, 150°C, 155°C, 160°C, 165°C, 170°C or any value between 140-170°C.

[0042] And / or, the first stage of pressure leaching time is 1-3 h; Exemplarily, the time of the first stage of pressure leaching can be 1 h, 2 h, 3 h or any value between 1-3 h.

[0043] and / or, the liquid-to-solid ratio of the second acid solution to the atmospheric pressure leaching residue is 4-10 L / kg; Exemplarily, the liquid-to-solid ratio of the second acid solution to the atmospheric pressure leaching residue can be 4 L / kg, 5 L / kg, 6 L / kg, 7 L / kg, 8 L / kg, 9 L / kg, 10 L / kg or any value between 4-10 L / kg.

[0044] and / or, the oxygen partial pressure of the first stage of pressure leaching is 0.05-0.3 MPa; Illustratively, the oxygen partial pressure in the first stage of pressure leaching may be 0.05 MPa, 0.1 MPa, 0.15 MPa, 0.2 MPa, 0.25 MPa, 0.3 MPa or any value between 0.05-0.3 MPa.

[0045] Through the first stage of pressure leaching, the atmospheric pressure leaching slag realizes the selective separation of nickel and copper, maximizes the leaching of the soluble nickel and cobalt in the alloy phase and sulfide phase in the atmospheric pressure leaching slag, and at the same time, a small amount of copper is leached back to the atmospheric pressure leaching system. The first stage of pressure leaching slag mainly contains copper, a small amount of nickel, iron and precious metals, etc., which are enriched and enter the second stage of pressure leaching process, thereby achieving the purpose of selective leaching. Through the first stage of pressure leaching, the remaining nickel minerals are dissolved in large quantities, and the copper minerals react to form copper sulfate under the action of sulfuric acid, and interact with the nickel sulfide in the slag, so that a large amount of nickel is leached and copper sulfide precipitation is generated.

[0046] According to an embodiment of the present application, the initial acidity of the second stage of pressure leaching is 20-40 g / L, and the initial acidity of the second stage of pressure leaching refers to: the concentration of the third acid solution in the feed solution obtained after the first stage of pressure leaching residue is mixed with the third acid solution; Exemplarily, the initial acidity of the second stage pressure leaching can be 20 g / L, 25 g / L, 30 g / L, 35 g / L, 40 g / L or any value between 20-40 g / L.

[0047] and / or, the third acid solution comprises a sulfuric acid solution; and / or, the temperature of the second stage of pressure leaching is 160-180°C; Illustratively, the temperature of the second stage pressure leaching may be 160°C, 165°C, 170°C, 175°C, 180°C or any value between 160-180°C.

[0048] And / or, the second stage of pressure leaching time is 1-3 h; Exemplarily, the time of the second stage of pressure leaching can be 1 h, 2 h, 3 h or any value between 1-3 h.

[0049] and / or, the liquid-to-solid ratio of the third acid solution to the first stage pressure leaching residue is 4-10 L / kg; Exemplarily, the liquid-to-solid ratio of the third acid solution to the first-stage pressure leaching residue can be 4 L / kg, 5 L / kg, 6 L / kg, 7 L / kg, 8 L / kg, 9 L / kg, 10 L / kg or any value between 4-10 L / kg.

[0050] and / or, the oxygen partial pressure of the second stage of pressure leaching is 0.05-0.5 MPa; Illustratively, the oxygen partial pressure of the second stage of pressure leaching can be 0.05 MPa, 0.1 MPa, 0.15 MPa, 0.2 MPa, 0.25 MPa, 0.3 MPa, 0.35 MPa, 0.4 MPa, 0.45 MPa, 0.5 MPa or any value between 0.05-0.5 MPa.

[0051] According to an embodiment of the present application, the purification of the second-stage pressurized leaching solution includes: adding one or more of alkali and alkaline solution to the second-stage pressurized leaching solution.

[0052] Through the second stage of pressure leaching, almost all nickel, cobalt and copper in the first stage of pressure leaching residue can be leached into the second stage of pressure leaching solution, while iron and precious metals are retained in the precious metal slag, thereby achieving the effect of precious metal enrichment.

[0053] After the pyrometallurgical smelting and blowing process, the platinum-palladium concentrate can effectively remove a large amount of gangue, iron and a part of sulfur in the concentrate to produce high-grade nickel matte, in which the iron content can be controlled below 3%, laying a good foundation for the subsequent wet separation and extraction; after the atmospheric pressure leaching process, the atmospheric pressure leaching slag is produced, which can effectively remove the alloy phase. In the leaching process, the first stage pressurized leaching solution and the mixed solution of the copper product crystallization liquid are used as the leaching solution, which can greatly reduce the sulfuric acid consumption in the process and can be used for atmospheric pressure leaching. The concentrations of copper and iron in the leaching solution can be effectively reduced, which can reduce the difficulty of removing impurities in the subsequent open-circuit preparation of battery-grade nickel sulfate from the atmospheric pressure leaching solution; the atmospheric pressure leaching slag undergoes two pressure leaching processes, namely the first pressure leaching and the second pressure leaching, to produce precious metal-enriched slag. During the leaching process, good selective separation and recovery of nickel and copper can be achieved, thereby maximizing the comprehensive resource recovery efficiency. The precious metal elements are retained in the slag during the leaching process, which can effectively improve the enrichment degree of the precious metals, and the actual precious metal enrichment ratio is more than hundreds of times.

[0054] The embodiments of the present application will be described in detail below in conjunction with specific examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. If specific conditions are not specified in the examples, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0055] First, the composition range of the platinum-palladium concentrate that can be processed by the method provided in this application is described: The specific composition of the platinum-palladium concentrate used in the examples of the present application is: Ni 2.5%, copper 2.2%, cobalt 0.2%, iron 18.8%, sulfur 13.7%, silicon dioxide 22.6%, calcium oxide 3.4%, magnesium oxide 14.5%, aluminum oxide 1.0%; gold 3.0 g / t, silver 11.5 g / t, platinum 18.7 g / t, palladium 25.8 g / t, osmium 0.1 g / t, ruthenium 0.3 g / t, rhodium 0.5 g / t, iridium 0.8 g / t.

[0056] Example 1 This embodiment provides a method for comprehensive extraction and utilization of multiple metals in platinum-palladium concentrate. Figure 1 , the method specifically comprises the following steps: Take 30.0 kg of platinum-palladium concentrate, add 2.40 kg of lime, 6.50 kg of silica, and 2.10 kg of hematite, and smelt at 1389 °C for 28 min. Smelting obtains 7.19 kg of low-grade nickel matte, adds 2.16 kg of silicon dioxide, and blows at 1350 °C with a blowing airflow of 2.0 Nm 3 / h, blowing time 10 h, 1.60 kg of high-grade nickel matte was obtained, containing 42.26% nickel, 33.65% copper, 2.30% iron, 43.93 g / t gold, 148.83 g / t silver, 306.07 g / t platinum, and 439.57 g / t palladium. The concentration enrichment ratio of nickel, copper, gold, silver, platinum, and palladium in high-grade nickel matte is greater than 15.5.

[0057] 1.60 kg of high-matte nickel was leached at normal pressure in sulfuric acid solution, with a leaching temperature of 70 °C, a leaching time of 8 h, a leaching liquid-solid ratio of 6 L / kg, and a leaching end point pH of 6. A normal pressure leaching solution and 1.36 kg of normal pressure leaching residue were obtained, with metal leaching rates of 43.13% nickel, 48.63% cobalt, 0.41% copper, and 1.31% iron. The normal pressure leaching solution was subjected to a process of removing lead with barium hydroxide, with the amount of barium hydroxide added being 200 (the molar ratio of barium hydroxide to lead in the normal pressure leaching solution), and the lead concentration of the solution after lead removal was 0.0005 g / L; after a process of removing cobalt with black nickel, the amount of black nickel added being 18 (the molar ratio of black nickel to cobalt in the normal pressure leaching solution), and the cobalt concentration of the solution after cobalt removal was 0.007 g / L; the solution after cobalt removal was concentrated and crystallized, with a crystallization rate of 45.71%, to obtain a nickel sulfate product with a lead content of 0.0002% and a cobalt content of 0.02%. The nickel sulfate product met the nickel sulfate standard for type I batteries. The cobalt tetroxide product is prepared from the cobalt slag through acid dissolution-extraction-pyrolysis.

[0058] 1.36 kg of atmospheric leaching residue was subjected to the first stage of pressure leaching in sulfuric acid solution. After the atmospheric leaching residue was mixed with the sulfuric acid solution, the concentration of sulfuric acid in the obtained liquid was 10 g / L, the leaching temperature was 150 °C, the leaching time was 1 h, the leaching liquid-solid ratio was 10 L / kg, the oxygen partial pressure was 0.2 MPa, and the first stage of pressure leaching liquid and 1.11 kg of the first stage of pressure leaching residue were obtained. The metal leaching rates were 73.99% for nickel, 62.40% for cobalt, 8.68% for copper, and 4.35% for iron.

[0059] 1.11 kg of the first-stage pressure leaching residue was subjected to the second-stage pressure leaching in sulfuric acid solution. After the first-stage pressure leaching residue was mixed with the sulfuric acid solution, the concentration of sulfuric acid in the obtained liquid was 40 g / L, the leaching temperature was 180 ℃, the leaching time was 2h, the leaching liquid-solid ratio was 10 L / kg, and the oxygen partial pressure was 0.1 MPa. The second-stage pressure leaching solution and 22.9 g of precious metal slag were obtained, and the metal leaching rates were 99.84% for nickel, 99.68% for cobalt, 99.64% for copper, and 16.98% for iron. The second-stage pressure leaching solution was concentrated and cooled for crystallization, with a crystallization temperature of 30 ℃, a crystallization time of 3 h, an initial pH of crystallization of 1, and a crystallization rate of 56.74%. Copper sulfate product was obtained, with a copper sulfate content of 99.3%, and the copper sulfate product met the first-grade standard of copper sulfate (smelting by-product).

[0060] Test results: comprehensive recovery rate of nickel is 99.19%, comprehensive recovery rate of copper is 98.14%, comprehensive recovery rate of cobalt is 94.41%, comprehensive recovery rate of gold is 98.11%, comprehensive recovery rate of silver is 97.98%, comprehensive recovery rate of platinum is 98.31%, and comprehensive recovery rate of palladium is 99.50%; the enrichment ratio of precious metals is 1540 times for gold, 1440 times for silver, 1247 times for platinum, 1305 times for palladium, 1271 times for osmium, 1090 times for ruthenium, 1302 times for rhodium, and 1013 times for iridium.

[0061] Example 2 This embodiment provides a method for comprehensive extraction and utilization of multiple metals in platinum-palladium concentrate, which specifically comprises the following steps: Take 30.0 kg of platinum-palladium concentrate, add 3.0 kg of lime and 3.0 kg of hematite, and smelt at 1395 °C for 35 min. Smelting obtains 6.82 kg of low-grade nickel matte, adds 2.25 kg of silicon dioxide and blows at 1350 °C, with a blowing airflow of 2.0 Nm 3 / h, blowing time 10 h, 1.52 kg of high-grade nickel matte was obtained.

[0062] High matte nickel was leached at normal pressure in sulfuric acid solution, with a leaching temperature of 70 °C, a leaching time of 8 h, a leaching liquid-solid ratio of 6 L / kg, and a leaching end point pH of 6, to obtain a normal pressure leaching solution and a normal pressure leaching residue. The normal pressure leaching solution was subjected to a process of removing lead with barium hydroxide, with the amount of barium hydroxide added being 200 (the molar ratio of barium hydroxide to lead in the normal pressure leaching solution), and the lead concentration of the lead-removed solution being 0.0005 g / L; the process of removing cobalt with black nickel, with the amount of black nickel added being 18 (the molar ratio of black nickel to cobalt in the normal pressure leaching solution), and the cobalt concentration of the cobalt-removed solution being 0.007 g / L; the cobalt-removed solution was concentrated and crystallized to obtain a nickel sulfate product, which met the nickel sulfate standard for type I batteries. The cobalt slag was prepared by acid dissolution-extraction-pyrolysis to obtain a cobalt tetroxide product.

[0063] The atmospheric leaching residue was subjected to the first stage of pressure leaching in a sulfuric acid solution. After the atmospheric leaching residue was mixed with the sulfuric acid solution, the concentration of sulfuric acid in the obtained liquid was 10 g / L, the leaching temperature was 150 °C, the leaching time was 1 h, the leaching liquid-solid ratio was 10 L / kg, and the oxygen partial pressure was 0.2 MPa, thereby obtaining the first stage of pressure leaching liquid and the first stage of pressure leaching residue.

[0064] The first-stage pressure leaching residue was subjected to the second-stage pressure leaching in the sulfuric acid solution. After the first-stage pressure leaching residue was mixed with the sulfuric acid solution, the concentration of sulfuric acid in the obtained liquid was 40 g / L, the leaching temperature was 180 °C, the leaching time was 2 h, the leaching liquid-solid ratio was 10 L / kg, and the oxygen partial pressure was 0.1 MPa, and the second-stage pressure leaching solution and precious metal slag were obtained. The second-stage pressure leaching solution was concentrated and cooled for crystallization, the crystallization temperature was 30 °C, the crystallization time was 3 h, and the initial pH of the crystallization was 1, and the copper sulfate product was obtained. The copper sulfate product met the first-grade standard of copper sulfate (smelting by-product).

[0065] Test results: comprehensive recovery rate of nickel is 98.56%, comprehensive recovery rate of copper is 95.99%, comprehensive recovery rate of cobalt is 87.94%, comprehensive recovery rate of gold is 95.92%, comprehensive recovery rate of silver is 95.64%, comprehensive recovery rate of platinum is 96.35%, and comprehensive recovery rate of palladium is 98.92%; the enrichment ratio of precious metals is 710 times for gold, 677 times for silver, 588 times for platinum, 605 times for palladium, 562 times for osmium, 492 times for ruthenium, 535 times for rhodium, and 476 times for iridium.

[0066] Example 3 This embodiment provides a method for comprehensive extraction and utilization of multiple metals in platinum-palladium concentrate, which specifically comprises the following steps: Take 30.0 kg of platinum-palladium concentrate, add 2.25 kg of lime, 6.00 kg of silica, and 3.75 kg of hematite, and smelt at 1400 °C for 40 min. Smelting obtains 6.98 kg of low-grade nickel matte, adds 2.10 kg of silicon dioxide, and blows at 1350 °C with a blowing airflow of 2.0 Nm 3 / h, blowing time is 10 h, and 1.65 kg of high-grade nickel matte is obtained.

[0067] High matte nickel was leached at normal pressure in sulfuric acid solution, with a leaching temperature of 70 °C, a leaching time of 8 h, a leaching liquid-solid ratio of 6 L / kg, and a leaching end point pH of 6, to obtain a normal pressure leaching solution and a normal pressure leaching residue. The normal pressure leaching solution was subjected to a process of removing lead with barium hydroxide, with the amount of barium hydroxide added being 200 (the molar ratio of barium hydroxide to lead in the normal pressure leaching solution), and the lead concentration of the lead-removed solution being 0.0005 g / L; the process of removing cobalt with black nickel, with the amount of black nickel added being 18 (the molar ratio of black nickel to cobalt in the normal pressure leaching solution), and the cobalt concentration of the cobalt-removed solution being 0.007 g / L; the cobalt-removed solution was concentrated and crystallized to obtain a nickel sulfate product, which met the nickel sulfate standard for type I batteries. The cobalt slag was prepared by acid dissolution-extraction-pyrolysis to obtain a cobalt tetroxide product.

[0068] The atmospheric leaching residue was subjected to the first stage of pressure leaching in a sulfuric acid solution. After the atmospheric leaching residue was mixed with the sulfuric acid solution, the concentration of sulfuric acid in the obtained liquid was 10 g / L, the leaching temperature was 150 °C, the leaching time was 1 h, the leaching liquid-solid ratio was 10 L / kg, and the oxygen partial pressure was 0.2 MPa, thereby obtaining the first stage of pressure leaching liquid and the first stage of pressure leaching residue.

[0069] The first-stage pressure leaching residue was subjected to the second-stage pressure leaching in the sulfuric acid solution. After the first-stage pressure leaching residue was mixed with the sulfuric acid solution, the concentration of sulfuric acid in the obtained liquid was 40 g / L, the leaching temperature was 180 °C, the leaching time was 2 h, the leaching liquid-solid ratio was 10 L / kg, and the oxygen partial pressure was 0.1 MPa, and the second-stage pressure leaching solution and precious metal slag were obtained. The second-stage pressure leaching solution was concentrated and cooled for crystallization, the crystallization temperature was 30 °C, the crystallization time was 3 h, and the initial pH of the crystallization was 1, and the copper sulfate product was obtained. The copper sulfate product met the first-grade standard of copper sulfate (smelting by-product).

[0070] Test results: comprehensive recovery rate of nickel is 98.58%, comprehensive recovery rate of copper is 97.01%, comprehensive recovery rate of cobalt is 89.11%, comprehensive recovery rate of gold is 96.32%, comprehensive recovery rate of silver is 96.07%, comprehensive recovery rate of platinum is 96.71%, and comprehensive recovery rate of palladium is 99.03%; the enrichment ratio of precious metals is 788 times for gold, 750 times for silver, 652 times for platinum, 670 times for palladium, 580 times for osmium, 503 times for ruthenium, 602 times for rhodium, and 491 times for iridium.

[0071] Example 4 This embodiment provides a method for comprehensive extraction and utilization of multiple metals in platinum-palladium concentrate, which specifically comprises the following steps: Take 30.0 kg of platinum-palladium concentrate, add 2.18 kg of lime, 6.48 kg of silica, and 1.88 kg of hematite, and smelt at 1350 °C for 60 min. Smelting obtains 8.92 kg of low-grade nickel matte, adds 2.68 kg of silicon dioxide, and blows at 1350 °C with a blowing airflow of 2.0 Nm 3 / h, blowing time 10 h, 1.73 kg of high-matte nickel was obtained.

[0072] High matte nickel was leached at normal pressure in sulfuric acid solution, with a leaching temperature of 70 °C, a leaching time of 8 h, a leaching liquid-solid ratio of 6 L / kg, and a leaching end point pH of 6, to obtain a normal pressure leaching solution and a normal pressure leaching residue. The normal pressure leaching solution was subjected to a process of removing lead with barium hydroxide, with the amount of barium hydroxide added being 200 (the molar ratio of barium hydroxide to lead in the normal pressure leaching solution), and the lead concentration of the lead-removed solution being 0.0005 g / L; the process of removing cobalt with black nickel, with the amount of black nickel added being 18 (the molar ratio of black nickel to cobalt in the normal pressure leaching solution), and the cobalt concentration of the cobalt-removed solution being 0.007 g / L; the cobalt-removed solution was concentrated and crystallized to obtain a nickel sulfate product, which met the nickel sulfate standard for type I batteries. The cobalt slag was prepared by acid dissolution-extraction-pyrolysis to obtain a cobalt tetroxide product.

[0073] The atmospheric leaching residue was subjected to the first stage of pressure leaching in a sulfuric acid solution. After the atmospheric leaching residue was mixed with the sulfuric acid solution, the concentration of sulfuric acid in the obtained liquid was 10 g / L, the leaching temperature was 150 °C, the leaching time was 1 h, the leaching liquid-solid ratio was 10 L / kg, and the oxygen partial pressure was 0.2 MPa, thereby obtaining the first stage of pressure leaching liquid and the first stage of pressure leaching residue.

[0074] The first-stage pressure leaching residue was subjected to the second-stage pressure leaching in the sulfuric acid solution. After the first-stage pressure leaching residue was mixed with the sulfuric acid solution, the concentration of sulfuric acid in the obtained liquid was 40 g / L, the leaching temperature was 180 °C, the leaching time was 2 h, the leaching liquid-solid ratio was 10 L / kg, and the oxygen partial pressure was 0.1 MPa, and the second-stage pressure leaching solution and precious metal slag were obtained. The second-stage pressure leaching solution was concentrated and cooled for crystallization, the crystallization temperature was 30 °C, the crystallization time was 3 h, and the initial pH of the crystallization was 1, and the copper sulfate product was obtained. The copper sulfate product met the first-grade standard of copper sulfate (smelting by-product).

[0075] Test results: comprehensive recovery rate of nickel is 95.74%, comprehensive recovery rate of copper is 95.26%, comprehensive recovery rate of cobalt is 81.63%, comprehensive recovery rate of gold is 94.23%, comprehensive recovery rate of silver is 94.70%, comprehensive recovery rate of platinum is 94.13%, and comprehensive recovery rate of palladium is 98.23%; the enrichment ratio of precious metals is 316 times for gold, 300 times for silver, 265 times for platinum, 268 times for palladium, 259 times for osmium, 208 times for ruthenium, 269 times for rhodium, and 202 times for iridium.

[0076] Example 5 This embodiment provides a method for comprehensive extraction and utilization of multiple metals in platinum-palladium concentrate, which specifically comprises the following steps: Take 10.0 kg of platinum-palladium concentrate, add 0.85 kg of lime, 2.10 kg of silica, and 0.70 kg of hematite, and smelt at 1450 °C for 20 min. Smelting obtains 5.73 kg of low-grade nickel matte, adds 1.72 kg of silicon dioxide, and blows at 1350 °C with a blowing airflow of 2.0 Nm 3 / h, blowing time 10 h, 1.44 kg of high-grade nickel matte was obtained.

[0077] High matte nickel was leached at normal pressure in sulfuric acid solution, with a leaching temperature of 70 °C, a leaching time of 8 h, a leaching liquid-solid ratio of 6 L / kg, and a leaching end point pH of 6, to obtain a normal pressure leaching solution and a normal pressure leaching residue. The normal pressure leaching solution was subjected to a process of removing lead with barium hydroxide, with the amount of barium hydroxide added being 200 (the molar ratio of barium hydroxide to lead in the normal pressure leaching solution), and the lead concentration of the lead-removed solution being 0.0005 g / L; the process of removing cobalt with black nickel, with the amount of black nickel added being 18 (the molar ratio of black nickel to cobalt in the normal pressure leaching solution), and the cobalt concentration of the cobalt-removed solution being 0.007 g / L; the cobalt-removed solution was concentrated and crystallized to obtain a nickel sulfate product, which met the nickel sulfate standard for type I batteries. The cobalt slag was prepared by acid dissolution-extraction-pyrolysis to obtain a cobalt tetroxide product.

[0078] The atmospheric leaching residue was subjected to the first stage of pressure leaching in a sulfuric acid solution. After the atmospheric leaching residue was mixed with the sulfuric acid solution, the concentration of sulfuric acid in the obtained liquid was 10 g / L, the leaching temperature was 150 °C, the leaching time was 1 h, the leaching liquid-solid ratio was 10 L / kg, and the oxygen partial pressure was 0.2 MPa, thereby obtaining the first stage of pressure leaching liquid and the first stage of pressure leaching residue.

[0079] The first-stage pressure leaching residue was subjected to the second-stage pressure leaching in the sulfuric acid solution. After the first-stage pressure leaching residue was mixed with the sulfuric acid solution, the concentration of sulfuric acid in the obtained liquid was 40 g / L, the leaching temperature was 180 °C, the leaching time was 2 h, the leaching liquid-solid ratio was 10 L / kg, and the oxygen partial pressure was 0.1 MPa, and the second-stage pressure leaching solution and precious metal slag were obtained. The second-stage pressure leaching solution was concentrated and cooled for crystallization, the crystallization temperature was 30 °C, the crystallization time was 3 h, and the initial pH of the crystallization was 1, and the copper sulfate product was obtained. The copper sulfate product met the first-grade standard of copper sulfate (smelting by-product).

[0080] Test results: comprehensive recovery rate of nickel is 92.46%, comprehensive recovery rate of copper is 93.07%, comprehensive recovery rate of cobalt is 78.30%, comprehensive recovery rate of gold is 92.70%, comprehensive recovery rate of silver is 91.55%, comprehensive recovery rate of platinum is 92.53%, and comprehensive recovery rate of palladium is 97.46%; the enrichment ratio of precious metals is 370 times for gold, 355 times for silver, 306 times for platinum, 341 times for palladium, 308 times for osmium, 256 times for ruthenium, 314 times for rhodium, and 246 times for iridium.

[0081] Example 6 This embodiment provides a method for comprehensive extraction and utilization of multiple metals in platinum-palladium concentrate, which specifically comprises the following steps: Take 30.0 kg of platinum-palladium concentrate, add 2.3 kg of lime, 6.4 kg of silica, and 2.4 kg of hematite, and smelt at 1400 °C for 40 min. Smelting obtains 7.03 kg of low-grade nickel matte, adds 1.41 kg of silicon dioxide, and blows at 1400 °C with a blowing airflow of 4.0 Nm 3 / h, blowing time is 2 h, and 1.36 kg of high-matte nickel is obtained.

[0082] High matte nickel was leached at normal pressure in sulfuric acid solution, with a leaching temperature of 70 °C, a leaching time of 8 h, a leaching liquid-solid ratio of 6 L / kg, and a leaching end point pH of 6, to obtain a normal pressure leaching solution and a normal pressure leaching residue. The normal pressure leaching solution was subjected to a process of removing lead with barium hydroxide, with the amount of barium hydroxide added being 200 (the molar ratio of barium hydroxide to lead in the normal pressure leaching solution), and the lead concentration of the lead-removed solution being 0.0005 g / L; the process of removing cobalt with black nickel, with the amount of black nickel added being 18 (the molar ratio of black nickel to cobalt in the normal pressure leaching solution), and the cobalt concentration of the cobalt-removed solution being 0.007 g / L; the cobalt-removed solution was concentrated and crystallized to obtain a nickel sulfate product, which met the nickel sulfate standard for type I batteries. The cobalt slag was prepared by acid dissolution-extraction-pyrolysis to obtain a cobalt tetroxide product.

[0083] The atmospheric leaching residue was subjected to the first stage of pressure leaching in a sulfuric acid solution. After the atmospheric leaching residue was mixed with the sulfuric acid solution, the concentration of sulfuric acid in the obtained liquid was 10 g / L, the leaching temperature was 150 °C, the leaching time was 1 h, the leaching liquid-solid ratio was 10 L / kg, and the oxygen partial pressure was 0.2 MPa, thereby obtaining the first stage of pressure leaching liquid and the first stage of pressure leaching residue.

[0084] The first-stage pressure leaching residue was subjected to the second-stage pressure leaching in the sulfuric acid solution. After the first-stage pressure leaching residue was mixed with the sulfuric acid solution, the concentration of sulfuric acid in the obtained liquid was 40 g / L, the leaching temperature was 180 °C, the leaching time was 2 h, the leaching liquid-solid ratio was 10 L / kg, and the oxygen partial pressure was 0.1 MPa, and the second-stage pressure leaching solution and precious metal slag were obtained. The second-stage pressure leaching solution was concentrated and cooled for crystallization, the crystallization temperature was 30 °C, the crystallization time was 3 h, and the initial pH of the crystallization was 1, and the copper sulfate product was obtained. The copper sulfate product met the first-grade standard of copper sulfate (smelting by-product).

[0085] Test results: The comprehensive recovery rate of nickel is 94.94%, the comprehensive recovery rate of copper is 72.53%, the comprehensive recovery rate of cobalt is 90.53%, the comprehensive recovery rate of gold is 72.52%, the comprehensive recovery rate of silver is 72.42%, the comprehensive recovery rate of platinum is 72.66%, and the comprehensive recovery rate of palladium is 73.54%; the enrichment ratio of precious metals is 156 times for gold, 141 times for silver, 127 times for platinum, 132 times for palladium, 130 times for osmium, 106 times for ruthenium, 132 times for rhodium, and 109 times for iridium.

[0086] Example 7 This embodiment provides a method for comprehensive extraction and utilization of multiple metals in platinum-palladium concentrate, which specifically comprises the following steps: Take 30.0 kg of platinum-palladium concentrate, add 2.4 kg of lime, 6.0 kg of silica, and 2.6 kg of hematite, and smelt at 1400 °C for 40 min. Smelting obtains 6.96 kg of low-grade nickel matte, adds 2.78 kg of silicon dioxide, and blows at 1200 °C with a blowing airflow of 1.0 Nm 3 / h, blowing time 12 h, and 1.32 kg of high-matte nickel was obtained.

[0087] High matte nickel was leached at normal pressure in sulfuric acid solution, with a leaching temperature of 70 °C, a leaching time of 8 h, a leaching liquid-solid ratio of 6 L / kg, and a leaching end point pH of 6, to obtain a normal pressure leaching solution and a normal pressure leaching residue. The normal pressure leaching solution was subjected to a process of removing lead with barium hydroxide, with the amount of barium hydroxide added being 200 (the molar ratio of barium hydroxide to lead in the normal pressure leaching solution), and the lead concentration of the lead-removed solution being 0.0005 g / L; the process of removing cobalt with black nickel, with the amount of black nickel added being 18 (the molar ratio of black nickel to cobalt in the normal pressure leaching solution), and the cobalt concentration of the cobalt-removed solution being 0.007 g / L; the cobalt-removed solution was concentrated and crystallized to obtain a nickel sulfate product, which met the nickel sulfate standard for type I batteries. The cobalt slag was prepared by acid dissolution-extraction-pyrolysis to obtain a cobalt tetroxide product.

[0088] The atmospheric leaching residue was subjected to the first stage of pressure leaching in a sulfuric acid solution. After the atmospheric leaching residue was mixed with the sulfuric acid solution, the concentration of sulfuric acid in the obtained liquid was 10 g / L, the leaching temperature was 150 °C, the leaching time was 1 h, the leaching liquid-solid ratio was 10 L / kg, and the oxygen partial pressure was 0.2 MPa, thereby obtaining the first stage of pressure leaching liquid and the first stage of pressure leaching residue.

[0089] The first-stage pressure leaching residue was subjected to the second-stage pressure leaching in the sulfuric acid solution. After the first-stage pressure leaching residue was mixed with the sulfuric acid solution, the concentration of sulfuric acid in the obtained liquid was 40 g / L, the leaching temperature was 180 °C, the leaching time was 2 h, the leaching liquid-solid ratio was 10 L / kg, and the oxygen partial pressure was 0.1 MPa, and the second-stage pressure leaching solution and precious metal slag were obtained. The second-stage pressure leaching solution was concentrated and cooled for crystallization, the crystallization temperature was 30 °C, the crystallization time was 3 h, and the initial pH of the crystallization was 1, and the copper sulfate product was obtained. The copper sulfate product met the first-grade standard of copper sulfate (smelting by-product).

[0090] Test results: comprehensive recovery rate of nickel is 87.13%, comprehensive recovery rate of copper is 83.33%, comprehensive recovery rate of cobalt is 83.09%, comprehensive recovery rate of gold is 83.31%, comprehensive recovery rate of silver is 83.20%, comprehensive recovery rate of platinum is 83.48%, and comprehensive recovery rate of palladium is 84.59%; the enrichment ratio of precious metals is 145 times that of gold, 134 times that of silver, 117 times that of platinum, 120 times that of palladium, 118 times that of osmium, 104 times that of ruthenium, 116 times that of rhodium, and 98 times that of iridium.

[0091] Example 8 This embodiment provides a method for comprehensive extraction and utilization of multiple metals in platinum-palladium concentrate, which specifically comprises the following steps: Take 30.0 kg of platinum-palladium concentrate, add 2.40 kg of lime, 6.50 kg of silica, and 2.10 kg of hematite, and smelt at 1400 °C for 40 min. Smelting obtains 7.08 kg of low-grade nickel matte, adds 2.12 kg of silicon dioxide, and blows at 1350 °C with a blowing airflow of 2.0 Nm 3 / h, blowing time is 10 h, and 1.56 kg of high-grade nickel matte is obtained.

[0092] High matte nickel was leached at normal pressure in sulfuric acid solution, with leaching temperature of 50 ℃, leaching time of 10 h, leaching liquid-solid ratio of 12 L / kg, leaching end point pH of 7, and obtained normal pressure leaching solution and normal pressure leaching residue. The normal pressure leaching solution was subjected to the process of removing lead with barium hydroxide, with the amount of barium hydroxide added being 50 (the molar ratio of barium hydroxide to lead in the normal pressure leaching solution), and the lead concentration of the lead-removed solution was 0.0008 g / L; the process of removing cobalt with black nickel, with the amount of black nickel added being 2 (the molar ratio of black nickel to cobalt in the normal pressure leaching solution), and the cobalt concentration of the cobalt-removed solution was 0.012 g / L; the cobalt-removed solution was concentrated and crystallized to obtain a nickel sulfate product, which met the nickel sulfate standard for type I batteries. The cobalt slag was prepared by acid dissolution-extraction-pyrolysis to obtain a cobalt tetroxide product.

[0093] The atmospheric leaching residue was subjected to the first stage of pressure leaching in a sulfuric acid solution. After the atmospheric leaching residue was mixed with the sulfuric acid solution, the concentration of sulfuric acid in the obtained liquid was 10 g / L, the leaching temperature was 150 °C, the leaching time was 1 h, the leaching liquid-solid ratio was 10 L / kg, and the oxygen partial pressure was 0.2 MPa, thereby obtaining the first stage of pressure leaching liquid and the first stage of pressure leaching residue.

[0094] The first-stage pressure leaching residue was subjected to the second-stage pressure leaching in the sulfuric acid solution. After the first-stage pressure leaching residue was mixed with the sulfuric acid solution, the concentration of sulfuric acid in the obtained liquid was 40 g / L, the leaching temperature was 180 °C, the leaching time was 2 h, the leaching liquid-solid ratio was 10 L / kg, and the oxygen partial pressure was 0.1 MPa, and the second-stage pressure leaching solution and precious metal slag were obtained. The second-stage pressure leaching solution was concentrated and cooled for crystallization, the crystallization temperature was 30 °C, the crystallization time was 3 h, and the initial pH of the crystallization was 1, and the copper sulfate product was obtained. The copper sulfate product met the first-grade standard of copper sulfate (smelting by-product).

[0095] Test results: comprehensive recovery rate of nickel is 97.35%, comprehensive recovery rate of copper is 92.15%, comprehensive recovery rate of cobalt is 94.90%, comprehensive recovery rate of gold is 94.20%, comprehensive recovery rate of silver is 93.75%, comprehensive recovery rate of platinum is 92.95%, and comprehensive recovery rate of palladium is 92.40%; the enrichment ratio of precious metals is 114 times for gold, 102 times for silver, 110 times for platinum, 122 times for palladium, 119 times for osmium, 100 times for ruthenium, 123 times for rhodium, and 91 times for iridium.

[0096] Example 9 This embodiment provides a method for comprehensive extraction and utilization of multiple metals in platinum-palladium concentrate, which specifically comprises the following steps: Take 30.0 kg of platinum-palladium concentrate, add 2.40 kg of lime, 6.50 kg of silica, and 2.10 kg of hematite, and smelt at 1400 °C for 40 min. Smelting obtains 7.08 kg of low-grade nickel matte, adds 2.12 kg of silicon dioxide, and blows at 1350 °C with a blowing airflow of 2.0 Nm 3 / h, blowing time is 10 h, and 1.56 kg of high-grade nickel matte is obtained.

[0097] High matte nickel was leached at normal pressure in sulfuric acid solution, with leaching temperature of 95 ℃, leaching time of 3 h, leaching liquid-solid ratio of 2 L / kg, leaching end point pH of 4, and obtained normal pressure leaching solution and normal pressure leaching residue. The normal pressure leaching solution was subjected to the process of removing lead with barium hydroxide, with the amount of barium hydroxide added being 500 (the molar ratio of barium hydroxide to lead in the normal pressure leaching solution), and the lead concentration of the liquid after lead removal was 0.0004 g / L; the process of removing cobalt with black nickel, with the amount of black nickel added being 20 (the molar ratio of black nickel to cobalt in the normal pressure leaching solution), and the cobalt concentration of the liquid after cobalt removal was 0.009 g / L; the liquid after cobalt removal was concentrated and crystallized to obtain nickel sulfate product, which met the nickel sulfate standard for type I batteries. The cobalt slag was prepared by acid dissolution-extraction-pyrolysis to obtain cobalt tetroxide product.

[0098] The atmospheric leaching residue was subjected to the first stage of pressure leaching in a sulfuric acid solution. After the atmospheric leaching residue was mixed with the sulfuric acid solution, the concentration of sulfuric acid in the obtained liquid was 10 g / L, the leaching temperature was 150 °C, the leaching time was 1 h, the leaching liquid-solid ratio was 10 L / kg, and the oxygen partial pressure was 0.2 MPa, thereby obtaining the first stage of pressure leaching liquid and the first stage of pressure leaching residue.

[0099] The first-stage pressure leaching residue was subjected to the second-stage pressure leaching in the sulfuric acid solution. After the first-stage pressure leaching residue was mixed with the sulfuric acid solution, the concentration of sulfuric acid in the obtained liquid was 40 g / L, the leaching temperature was 180 °C, the leaching time was 2 h, the leaching liquid-solid ratio was 10 L / kg, and the oxygen partial pressure was 0.1 MPa, and the second-stage pressure leaching solution and precious metal slag were obtained. The second-stage pressure leaching solution was concentrated and cooled for crystallization, the crystallization temperature was 30 °C, the crystallization time was 3 h, and the initial pH of the crystallization was 1, and the copper sulfate product was obtained. The copper sulfate product met the first-grade standard of copper sulfate (smelting by-product).

[0100] Test results: comprehensive recovery rate of nickel is 82.70%, comprehensive recovery rate of copper is 82.75%, comprehensive recovery rate of cobalt is 82.95%, comprehensive recovery rate of gold is 93.90%, comprehensive recovery rate of silver is 94.60%, comprehensive recovery rate of platinum is 93.90%, and comprehensive recovery rate of palladium is 93.70%; the enrichment ratio of precious metals is 2215 times for gold, 2048 times for silver, 2066 times for platinum, 2171 times for palladium, 2138 times for osmium, 1822 times for ruthenium, 2169 times for rhodium, and 1637 times for iridium.

[0101] Example 10 This embodiment provides a method for comprehensive extraction and utilization of multiple metals in platinum-palladium concentrate, which specifically comprises the following steps: Take 30.0 kg of platinum-palladium concentrate, add 2.40 kg of lime, 6.50 kg of silica, and 2.10 kg of hematite, and smelt at 1400 °C for 40 min. Smelting obtains 7.08 kg of low-grade nickel matte, adds 2.12 kg of silicon dioxide, and blows at 1350 °C with a blowing airflow of 2.0 Nm 3 / h, blowing time is 10 h, and 1.56 kg of high-grade nickel matte is obtained.

[0102] High matte nickel was leached at normal pressure in sulfuric acid solution, with leaching temperature of 70 ℃, leaching time of 8 h, leaching liquid-solid ratio of 6 L / kg, leaching end point pH of 6, and obtained normal pressure leaching solution and 1.33 kg normal pressure leaching residue, with metal leaching rates of 40.40% nickel, 52.43% cobalt, 0.43% copper, and 0.99% iron. The normal pressure leaching solution was subjected to the process of removing lead with barium hydroxide, with the amount of barium hydroxide added being 200 (the molar ratio of barium hydroxide to lead in the normal pressure leaching solution), and the lead concentration of the solution after lead removal was 0.0005 g / L; after the process of removing cobalt with black nickel, with the amount of black nickel added being 18 (the molar ratio of black nickel to cobalt in the normal pressure leaching solution), and the cobalt concentration of the solution after cobalt removal was 0.007 g / L; the solution after cobalt removal was concentrated and crystallized, with a crystallization rate of 45.71%, to obtain a nickel sulfate product with a lead content of 0.0002% and a cobalt content of 0.02%, and the nickel sulfate product met the nickel sulfate standard for type I batteries. The cobalt tetroxide product is prepared from the cobalt slag through acid dissolution-extraction-pyrolysis.

[0103] The atmospheric leaching residue was subjected to the first stage of pressure leaching in a sulfuric acid solution. After the atmospheric leaching residue was mixed with the sulfuric acid solution, the concentration of sulfuric acid in the obtained liquid was 30 g / L, the leaching temperature was 170 °C, the leaching time was 3 h, the leaching liquid-solid ratio was 10 L / kg, and the oxygen partial pressure was 0.05 MPa, thereby obtaining the first stage of pressure leaching liquid and the first stage of pressure leaching residue.

[0104] The first-stage pressure leaching residue was subjected to the second-stage pressure leaching in the sulfuric acid solution. After the first-stage pressure leaching residue was mixed with the sulfuric acid solution, the concentration of sulfuric acid in the obtained liquid was 40 g / L, the leaching temperature was 180 °C, the leaching time was 2 h, the leaching liquid-solid ratio was 10 L / kg, and the oxygen partial pressure was 0.1 MPa, and the second-stage pressure leaching solution and precious metal slag were obtained. The second-stage pressure leaching solution was concentrated and cooled for crystallization, the crystallization temperature was 30 °C, the crystallization time was 3 h, and the initial pH of the crystallization was 1, and the copper sulfate product was obtained. The copper sulfate product met the first-grade standard of copper sulfate (smelting by-product).

[0105] Test results: comprehensive recovery rate of nickel is 87.45%, comprehensive recovery rate of copper is 86.49%, comprehensive recovery rate of cobalt is 81.88%, comprehensive recovery rate of gold is 95.03%, comprehensive recovery rate of silver is 94.58%, comprehensive recovery rate of platinum is 93.11%, and comprehensive recovery rate of palladium is 93.45%; the enrichment ratio of precious metals is 234 times for gold, 217 times for silver, 197 times for platinum, 202 times for palladium, 224 times for osmium, 193 times for ruthenium, 226 times for rhodium, and 178 times for iridium.

[0106] Embodiment 11 This embodiment provides a method for comprehensive extraction and utilization of multiple metals in platinum-palladium concentrate, which specifically comprises the following steps: Take 30.0 kg of platinum-palladium concentrate, add 2.40 kg of lime, 6.50 kg of silica, and 2.10 kg of hematite, and smelt at 1400 °C for 40 min. Smelting obtains 7.08 kg of low-grade nickel matte, adds 2.12 kg of silicon dioxide, and blows at 1350 °C with a blowing airflow of 2.0 Nm 3 / h, blowing time is 10 h, and 1.56 kg of high-grade nickel matte is obtained.

[0107] High matte nickel was leached at normal pressure in sulfuric acid solution, with leaching temperature of 70 ℃, leaching time of 8 h, leaching liquid-solid ratio of 6 L / kg, leaching end point pH of 6, and obtained normal pressure leaching solution and 1.33 kg normal pressure leaching residue, with metal leaching rates of 40.40% nickel, 52.43% cobalt, 0.43% copper, and 0.99% iron. The normal pressure leaching solution was subjected to the process of removing lead with barium hydroxide, with the amount of barium hydroxide added being 200 (the molar ratio of barium hydroxide to lead in the normal pressure leaching solution), and the lead concentration of the solution after lead removal was 0.0005 g / L; after the process of removing cobalt with black nickel, with the amount of black nickel added being 18 (the molar ratio of black nickel to cobalt in the normal pressure leaching solution), and the cobalt concentration of the solution after cobalt removal was 0.007 g / L; the solution after cobalt removal was concentrated and crystallized, with a crystallization rate of 45.71%, to obtain a nickel sulfate product with a lead content of 0.0002% and a cobalt content of 0.02%, and the nickel sulfate product met the nickel sulfate standard for type I batteries. The cobalt tetroxide product is prepared from the cobalt slag through acid dissolution-extraction-pyrolysis.

[0108] The atmospheric leaching residue was subjected to the first stage of pressure leaching in a sulfuric acid solution. After the atmospheric leaching residue was mixed with the sulfuric acid solution, the concentration of sulfuric acid in the obtained liquid was 10 g / L, the leaching temperature was 140 °C, the leaching time was 1 h, the leaching liquid-solid ratio was 4 L / kg, and the oxygen partial pressure was 0.3 MPa, thereby obtaining the first stage of pressure leaching liquid and the first stage of pressure leaching residue.

[0109] The first-stage pressure leaching residue was subjected to the second-stage pressure leaching in the sulfuric acid solution. After the first-stage pressure leaching residue was mixed with the sulfuric acid solution, the concentration of sulfuric acid in the obtained liquid was 40 g / L, the leaching temperature was 180 °C, the leaching time was 2 h, the leaching liquid-solid ratio was 10 L / kg, and the oxygen partial pressure was 0.1 MPa, and the second-stage pressure leaching solution and precious metal slag were obtained. The second-stage pressure leaching solution was concentrated and cooled for crystallization, the crystallization temperature was 30 °C, the crystallization time was 3 h, and the initial pH of the crystallization was 1, and the copper sulfate product was obtained. The copper sulfate product met the first-grade standard of copper sulfate (smelting by-product).

[0110] Test results: comprehensive recovery rate of nickel is 87.85%, comprehensive recovery rate of copper is 81.91%, comprehensive recovery rate of cobalt is 82.01%, comprehensive recovery rate of gold is 97.22%, comprehensive recovery rate of silver is 96.12%, comprehensive recovery rate of platinum is 98.83%, and comprehensive recovery rate of palladium is 96.75%; the enrichment ratio of precious metals is 363 times for gold, 290 times for silver, 233 times for platinum, 315 times for palladium, 336 times for osmium, 231 times for ruthenium, 339 times for rhodium, and 202 times for iridium.

[0111] Example 12 This embodiment provides a method for comprehensive extraction and utilization of multiple metals in platinum-palladium concentrate, which specifically comprises the following steps: Take 30.0 kg of platinum-palladium concentrate, add 2.40 kg of lime, 6.50 kg of silica, and 2.10 kg of hematite, and smelt at 1400 °C for 40 min. Smelting obtains 7.08 kg of low-grade nickel matte, adds 2.12 kg of silicon dioxide, and blows at 1350 °C with a blowing airflow of 2.0 Nm 3 / h, blowing time is 10 h, and 1.56 kg of high-grade nickel matte is obtained.

[0112] High matte nickel was leached at normal pressure in sulfuric acid solution, with leaching temperature of 70 ℃, leaching time of 8 h, leaching liquid-solid ratio of 6 L / kg, leaching end point pH of 6, and obtained normal pressure leaching solution and 1.33 kg normal pressure leaching residue, with metal leaching rates of 40.40% nickel, 52.43% cobalt, 0.43% copper, and 0.99% iron. The normal pressure leaching solution was subjected to the process of removing lead with barium hydroxide, with the amount of barium hydroxide added being 200 (the molar ratio of barium hydroxide to lead in the normal pressure leaching solution), and the lead concentration of the solution after lead removal was 0.0005 g / L; after the process of removing cobalt with black nickel, with the amount of black nickel added being 18 (the molar ratio of black nickel to cobalt in the normal pressure leaching solution), and the cobalt concentration of the solution after cobalt removal was 0.007 g / L; the solution after cobalt removal was concentrated and crystallized, with a crystallization rate of 45.71%, to obtain a nickel sulfate product with a lead content of 0.0002% and a cobalt content of 0.02%, and the nickel sulfate product met the nickel sulfate standard for type I batteries. The cobalt tetroxide product is prepared from the cobalt slag through acid dissolution-extraction-pyrolysis.

[0113] The atmospheric leaching residue was subjected to the first stage of pressure leaching in a sulfuric acid solution. The concentration of sulfuric acid in the obtained solution after the atmospheric leaching residue was mixed with the sulfuric acid solution was 10 g / L, the leaching temperature was 150 °C, the leaching time was 1 h, the leaching liquid-solid ratio was 10 L / kg, the oxygen partial pressure was 0.2 MPa, and the first stage of pressure leaching solution and 1.09 kg of the first stage of pressure leaching residue were obtained. The metal leaching rates were 75.03% for nickel, 68.06% for cobalt, 11.03% for copper, and 4.40% for iron.

[0114] The first-stage pressure leaching residue was subjected to the second-stage pressure leaching in the sulfuric acid solution. The concentration of sulfuric acid in the obtained liquid after the first-stage pressure leaching residue was mixed with the sulfuric acid solution was 20 g / L, the leaching temperature was 160 °C, the leaching time was 1 h, the leaching liquid-solid ratio was 4 L / kg, and the oxygen partial pressure was 0.5 MPa, and the second-stage pressure leaching solution and precious metal slag were obtained. The second-stage pressure leaching solution was concentrated and cooled for crystallization, the crystallization temperature was 30 °C, the crystallization time was 3 h, and the initial pH of the crystallization was 1, and the copper sulfate product was obtained. The copper sulfate product met the first-grade standard of copper sulfate (smelting by-product).

[0115] Test results: comprehensive recovery rate of nickel is 98.69%, comprehensive recovery rate of copper is 98.82%, comprehensive recovery rate of cobalt is 94.70%, comprehensive recovery rate of gold is 96.99%, comprehensive recovery rate of silver is 90.95%, comprehensive recovery rate of platinum is 93.68%, and comprehensive recovery rate of palladium is 98.49%; the enrichment ratio of precious metals is 1926 times for gold, 1835 times for silver, 1559 times for platinum, 1630 times for palladium, 1635 times for osmium, 1397 times for ruthenium, 1672 times for rhodium, and 1203 times for iridium.

[0116] Embodiment 13 This embodiment provides a method for comprehensive extraction and utilization of multiple metals in platinum-palladium concentrate, which specifically comprises the following steps: Take 30.0 kg of platinum-palladium concentrate, add 2.40 kg of lime, 6.50 kg of silica, and 2.10 kg of hematite, and smelt at 1400 °C for 40 min. Smelting obtains 7.08 kg of low-grade nickel matte, adds 2.12 kg of silicon dioxide, and blows at 1350 °C with a blowing airflow of 2.0 Nm 3 / h, blowing time is 10 h, and 1.56 kg of high-grade nickel matte is obtained.

[0117] High matte nickel was leached at normal pressure in sulfuric acid solution, with leaching temperature of 70 ℃, leaching time of 8 h, leaching liquid-solid ratio of 6 L / kg, leaching end point pH of 6, and obtained normal pressure leaching solution and 1.33 kg normal pressure leaching residue, with metal leaching rates of 40.40% nickel, 52.43% cobalt, 0.43% copper, and 0.99% iron. The normal pressure leaching solution was subjected to the process of removing lead with barium hydroxide, with the amount of barium hydroxide added being 200 (the molar ratio of barium hydroxide to lead in the normal pressure leaching solution), and the lead concentration of the solution after lead removal was 0.0005 g / L; after the process of removing cobalt with black nickel, with the amount of black nickel added being 18 (the molar ratio of black nickel to cobalt in the normal pressure leaching solution), and the cobalt concentration of the solution after cobalt removal was 0.007 g / L; the solution after cobalt removal was concentrated and crystallized, with a crystallization rate of 45.71%, to obtain a nickel sulfate product with a lead content of 0.0002% and a cobalt content of 0.02%, and the nickel sulfate product met the nickel sulfate standard for type I batteries. The cobalt tetroxide product is prepared from the cobalt slag through acid dissolution-extraction-pyrolysis.

[0118] The atmospheric leaching residue was subjected to the first stage of pressure leaching in a sulfuric acid solution. The concentration of sulfuric acid in the obtained solution after the atmospheric leaching residue was mixed with the sulfuric acid solution was 10 g / L, the leaching temperature was 150 °C, the leaching time was 1 h, the leaching liquid-solid ratio was 10 L / kg, the oxygen partial pressure was 0.2 MPa, and the first stage of pressure leaching solution and 1.09 kg of the first stage of pressure leaching residue were obtained. The metal leaching rates were 75.03% for nickel, 68.06% for cobalt, 11.03% for copper, and 4.40% for iron.

[0119] The first-stage pressure leaching residue was subjected to the second-stage pressure leaching in the sulfuric acid solution. The concentration of sulfuric acid in the obtained liquid after the first-stage pressure leaching residue was mixed with the sulfuric acid solution was 40 g / L, the leaching temperature was 180 °C, the leaching time was 3 h, the leaching liquid-solid ratio was 10 L / kg, and the oxygen partial pressure was 0.05 MPa, and the second-stage pressure leaching solution and precious metal slag were obtained. The second-stage pressure leaching solution was concentrated and cooled for crystallization, the crystallization temperature was 30 °C, the crystallization time was 3 h, and the initial pH of the crystallization was 1, and the copper sulfate product was obtained. The copper sulfate product met the first-grade standard of copper sulfate (smelting by-product).

[0120] Test results: comprehensive recovery rate of nickel is 97.75%, comprehensive recovery rate of copper is 95.95%, comprehensive recovery rate of cobalt is 96.24%, comprehensive recovery rate of gold is 98.80%, comprehensive recovery rate of silver is 96.70%, comprehensive recovery rate of platinum is 96.95%, and comprehensive recovery rate of palladium is 99.45%; the enrichment ratio of precious metals is 384 times for gold, 364 times for silver, 317 times for platinum, 325 times for palladium, 311 times for osmium, 261 times for ruthenium, 318 times for rhodium, and 256 times for iridium.

[0121] Comparative Example 1 Take 30.0 kg of platinum-palladium concentrate, add 2.40 kg of lime, 6.50 kg of silica, and 2.10 kg of hematite, and smelt at 1400 °C for 40 min. Smelting obtains 7.08 kg of low-grade nickel matte, adds 2.12 kg of silicon dioxide, and blows at 1350 °C with a blowing airflow of 2.0 Nm 3 / h, blowing time is 10 h, and 1.56 kg of high-grade nickel matte is obtained.

[0122] The high-matte nickel was leached at normal pressure in sulfuric acid solution, with a leaching temperature of 40 °C, a leaching time of 2 h, a leaching liquid-solid ratio of 15 L / kg, and a leaching end point pH of 6. Normal pressure leaching solution and 1.49 kg of normal pressure leaching slag were obtained, with metal leaching rates of nickel 12.72%, cobalt 13.11%, copper 0.04%, and iron 6.05%. The normal pressure leaching effect was not good, with low leaching rates of nickel and cobalt and high leaching rate of iron.

[0123] Comparative Example 2 Take 30.0 kg of platinum-palladium concentrate, add 2.40 kg of lime, 6.50 kg of silica, and 2.10 kg of hematite, and smelt at 1400 °C for 40 min. Smelting obtains 7.08 kg of low-grade nickel matte, adds 2.12 kg of silicon dioxide, and blows at 1350 °C with a blowing airflow of 2.0 Nm 3 / h, blowing time is 10 h, and 1.56 kg of high-grade nickel matte is obtained.

[0124] The high-matte nickel was leached at normal pressure in a sulfuric acid solution, with a leaching temperature of 100 °C, a leaching time of 12 h, a leaching liquid-solid ratio of 1 L / kg, and a leaching end point pH of 6. A normal pressure leaching solution and 1.12 kg of normal pressure leaching slag were obtained, with metal leaching rates of 31.17% nickel, 55.62% cobalt, 0.84% ​​copper, and 82.37% iron. The normal pressure leaching effect was not good, with a low nickel leaching rate, a high iron leaching rate, and a small amount of copper being leached.

[0125] Comparative Example 3 Take 30.0 kg of platinum-palladium concentrate, add 2.40 kg of lime, 6.50 kg of silica, and 2.10 kg of hematite, and smelt at 1400 °C for 40 min. Smelting obtains 7.08 kg of low-grade nickel matte, adds 2.12 kg of silicon dioxide, and blows at 1350 °C with a blowing airflow of 2.0 Nm 3 / h, blowing time is 10 h, and 1.56 kg of high-grade nickel matte is obtained.

[0126] The high-matte nickel was leached at normal pressure in sulfuric acid solution, with a leaching temperature of 70 °C, a leaching time of 8 h, a leaching liquid-solid ratio of 6 L / kg, and a leaching end point pH of 2. Normal pressure leaching solution and 1.08 kg of normal pressure leaching residue were obtained, and the metal leaching rates were 51.45% nickel, 56.16% cobalt, 0.52% copper, and 80.99% iron. The normal pressure leaching effect was not good, and the iron leaching rate was high.

[0127] Comparative Example 4 Take 30.0 kg of platinum-palladium concentrate, add 2.40 kg of lime, 6.50 kg of silica, and 2.10 kg of hematite, and smelt at 1400 °C for 40 min. Smelting obtains 7.08 kg of low-grade nickel matte, adds 2.12 kg of silicon dioxide, and blows at 1350 °C with a blowing airflow of 2.0 Nm 3 / h, blowing time is 10 h, and 1.56 kg of high-grade nickel matte is obtained.

[0128] The high-matte nickel was leached at normal pressure in a sulfuric acid solution, with a leaching temperature of 70 °C, a leaching time of 8 h, a leaching liquid-solid ratio of 6 L / kg, and a leaching end point pH of 8. A normal pressure leaching solution and 1.55 kg of normal pressure leaching slag were obtained, with metal leaching rates of 1.23% nickel, 0.98% cobalt, 0.01% copper, and 0.61% iron. The normal pressure leaching effect was not good, and the leaching rates of nickel and cobalt were low.

[0129] Comparative Example 5 Take 30.0 kg of platinum-palladium concentrate, add 2.40 kg of lime, 6.50 kg of silica, and 2.10 kg of hematite, and smelt at 1400 °C for 40 min. Smelting obtains 7.08 kg of low-grade nickel matte, adds 2.12 kg of silicon dioxide, and blows at 1350 °C with a blowing airflow of 2.0 Nm 3 / h, blowing time is 10 h, and 1.56 kg of high-grade nickel matte is obtained.

[0130] The high-matte nickel was leached at normal pressure in a sulfuric acid solution, with a leaching temperature of 70 °C, a leaching time of 8 h, a leaching liquid-solid ratio of 6 L / kg, and a leaching end point pH of 6. The normal pressure leaching solution and 1.33 kg of normal pressure leaching slag were obtained, with metal leaching rates of 40.40% nickel, 52.43% cobalt, 0.43% copper, and 0.99% iron. The normal pressure leaching solution was concentrated and crystallized with a crystallization rate of 26.07%, and a nickel sulfate product was obtained with a lead content of 0.0023% and a cobalt content of 0.24%. The nickel sulfate crystallization effect was not good, and the nickel sulfate product contained high impurities such as cobalt and lead, which could not meet the nickel sulfate standard for batteries.

[0131] Comparative Example 6 Take 30.0 kg of platinum-palladium concentrate, add 2.40 kg of lime, 6.50 kg of silica, and 2.10 kg of hematite, and smelt at 1400 °C for 40 min. Smelting obtains 7.08 kg of low-grade nickel matte, adds 2.12 kg of silicon dioxide, and blows at 1350 °C with a blowing airflow of 2.0 Nm 3 / h, blowing time is 10 h, and 1.56 kg of high-grade nickel matte is obtained.

[0132] High matte nickel was leached at normal pressure in sulfuric acid solution, with a leaching temperature of 70 °C, a leaching time of 8 h, a leaching liquid-solid ratio of 6 L / kg, and a leaching end point pH of 6. A normal pressure leaching solution and 1.33 kg of normal pressure leaching slag were obtained, with metal leaching rates of 40.40% nickel, 52.43% cobalt, 0.43% copper, and 0.99% iron. The normal pressure leaching solution was subjected to a process of removing lead with barium hydroxide, with a barium hydroxide addition amount of 200 (the molar ratio of barium hydroxide to lead in the normal pressure leaching solution), and the lead concentration of the lead-removed solution was 0.0005 g / L. The lead-removed solution was concentrated and crystallized, with a crystallization rate of 30.99%, to obtain a nickel sulfate product with a lead content of 0.0004% and a cobalt content of 0.24%. The nickel sulfate crystallization effect was not good, and the cobalt impurities in the nickel sulfate product were high, which could not meet the nickel sulfate standard for batteries.

[0133] Comparative Example 7 Take 30.0 kg of platinum-palladium concentrate, add 2.40 kg of lime, 6.50 kg of silica, and 2.10 kg of hematite, and smelt at 1400 °C for 40 min. Smelting obtains 7.08 kg of low-grade nickel matte, adds 2.12 kg of silicon dioxide, and blows at 1350 °C with a blowing airflow of 2.0 Nm 3 / h, blowing time is 10 h, and 1.56 kg of high-grade nickel matte is obtained.

[0134] High matte nickel was leached at normal pressure in sulfuric acid solution, with a leaching temperature of 70 °C, a leaching time of 8 h, a leaching liquid-solid ratio of 6 L / kg, and a leaching end point pH of 6. A normal pressure leaching solution and 1.33 kg of normal pressure leaching slag were obtained, with metal leaching rates of 40.40% nickel, 52.43% cobalt, 0.43% copper, and 0.99% iron. The normal pressure leaching solution was subjected to a black nickel cobalt removal process, with a black nickel addition amount of 18 (the molar ratio of black nickel to cobalt in the normal pressure leaching solution), and the cobalt concentration of the solution after cobalt removal was 0.006 g / L; the solution after cobalt removal was concentrated and crystallized, with a crystallization rate of 36.62%, to obtain a nickel sulfate product with a lead content of 0.0023% and a cobalt content of 0.006%. The nickel sulfate crystallization effect was not good, and the lead impurity in the nickel sulfate product was high, which could not meet the nickel sulfate standard for batteries.

[0135] Comparative Example 8 Take 30.0 kg of platinum-palladium concentrate, add 2.40 kg of lime, 6.50 kg of silica, and 2.10 kg of hematite, and smelt at 1400 °C for 40 min. Smelting obtains 7.08 kg of low-grade nickel matte, adds 2.12 kg of silicon dioxide, and blows at 1350 °C with a blowing airflow of 2.0 Nm 3 / h, blowing time is 10 h, and 1.56 kg of high-grade nickel matte is obtained.

[0136] High matte nickel was leached at normal pressure in sulfuric acid solution, with leaching temperature of 70 ℃, leaching time of 8 h, leaching liquid-solid ratio of 6 L / kg, leaching end point pH of 6, and obtained normal pressure leaching solution and 1.33 kg normal pressure leaching residue, with metal leaching rates of 40.40% nickel, 52.43% cobalt, 0.43% copper, and 0.99% iron. The normal pressure leaching solution was subjected to the process of removing lead with barium hydroxide, with the amount of barium hydroxide added being 200 (the molar ratio of barium hydroxide to lead in the normal pressure leaching solution), and the lead concentration of the solution after lead removal was 0.0005 g / L; after the process of removing cobalt with black nickel, with the amount of black nickel added being 18 (the molar ratio of black nickel to cobalt in the normal pressure leaching solution), and the cobalt concentration of the solution after cobalt removal was 0.007 g / L; the solution after cobalt removal was concentrated and crystallized, with a crystallization rate of 45.71%, to obtain a nickel sulfate product with a lead content of 0.0002% and a cobalt content of 0.02%, and the nickel sulfate product met the nickel sulfate standard for type I batteries. The cobalt tetroxide product is prepared from the cobalt slag through acid dissolution-extraction-pyrolysis.

[0137] The atmospheric leaching residue was subjected to the first stage of pressure leaching in sulfuric acid solution. After the atmospheric leaching residue was mixed with the sulfuric acid solution, the concentration of sulfuric acid in the obtained liquid was 40 g / L, the leaching temperature was 180 ℃, the leaching time was 4 h, the leaching liquid-solid ratio was 12 L / kg, the oxygen partial pressure was 0.4 MPa, and the first stage of pressure leaching liquid and 0.02 kg of the first stage of pressure leaching residue were obtained. The metal leaching rates were 97.85% for nickel, 97.22% for cobalt, 86.78% for copper, and 24.64% for iron. The first stage of pressure leaching had a poor effect, with high copper and iron contents in the first stage of pressure leaching liquid, and no good selective separation effect was obtained for nickel and copper.

[0138] Comparative Example 9 Take 30.0 kg of platinum-palladium concentrate, add 2.40 kg of lime, 6.50 kg of silica, and 2.10 kg of hematite, and smelt at 1400 °C for 40 min. Smelting obtains 7.08 kg of low-grade nickel matte, adds 2.12 kg of silicon dioxide, and blows at 1350 °C with a blowing airflow of 2.0 Nm 3 / h, blowing time is 10 h, and 1.56 kg of high-grade nickel matte is obtained.

[0139] High matte nickel was leached at normal pressure in sulfuric acid solution, with leaching temperature of 70 ℃, leaching time of 8 h, leaching liquid-solid ratio of 6 L / kg, leaching end point pH of 6, and obtained normal pressure leaching solution and 1.33 kg normal pressure leaching residue, with metal leaching rates of 40.40% nickel, 52.43% cobalt, 0.43% copper, and 0.99% iron. The normal pressure leaching solution was subjected to the process of removing lead with barium hydroxide, with the amount of barium hydroxide added being 200 (the molar ratio of barium hydroxide to lead in the normal pressure leaching solution), and the lead concentration of the solution after lead removal was 0.0005 g / L; after the process of removing cobalt with black nickel, with the amount of black nickel added being 18 (the molar ratio of black nickel to cobalt in the normal pressure leaching solution), and the cobalt concentration of the solution after cobalt removal was 0.007 g / L; the solution after cobalt removal was concentrated and crystallized, with a crystallization rate of 45.71%, to obtain a nickel sulfate product with a lead content of 0.0002% and a cobalt content of 0.02%, and the nickel sulfate product met the nickel sulfate standard for type I batteries. The cobalt tetroxide product is prepared from the cobalt slag through acid dissolution-extraction-pyrolysis.

[0140] The atmospheric leaching residue was subjected to the first stage of pressure leaching in sulfuric acid solution. After the atmospheric leaching residue was mixed with the sulfuric acid solution, the concentration of sulfuric acid in the obtained liquid was 8 g / L, the leaching temperature was 120 ℃, the leaching time was 40 min, the leaching liquid-solid ratio was 3 L / kg, the oxygen partial pressure was 0.02 MPa, and the first stage of pressure leaching liquid and 1.23 kg of the first stage of pressure leaching residue were obtained. The metal leaching rates were 12.39% nickel, 7.47% cobalt, 0.64% copper, and 12.77% iron. The first stage of pressure leaching was not good, the nickel content in the first stage of pressure leaching residue was high, and nickel and copper did not obtain a good selective separation effect.

[0141] Comparative Example 10 Take 30.0 kg of platinum-palladium concentrate, add 2.40 kg of lime, 6.50 kg of silica, and 2.10 kg of hematite, and smelt at 1400 °C for 40 min. Smelting obtains 7.08 kg of low-grade nickel matte, adds 2.12 kg of silicon dioxide, and blows at 1350 °C with a blowing airflow of 2.0 Nm 3 / h, blowing time is 10 h, and 1.56 kg of high-grade nickel matte is obtained.

[0142] High matte nickel was leached at normal pressure in sulfuric acid solution, with leaching temperature of 70 ℃, leaching time of 8 h, leaching liquid-solid ratio of 6 L / kg, leaching end point pH of 6, and obtained normal pressure leaching solution and 1.33 kg normal pressure leaching residue, with metal leaching rates of 40.40% nickel, 52.43% cobalt, 0.43% copper, and 0.99% iron. The normal pressure leaching solution was subjected to the process of removing lead with barium hydroxide, with the amount of barium hydroxide added being 200 (the molar ratio of barium hydroxide to lead in the normal pressure leaching solution), and the lead concentration of the solution after lead removal was 0.0005 g / L; after the process of removing cobalt with black nickel, with the amount of black nickel added being 18 (the molar ratio of black nickel to cobalt in the normal pressure leaching solution), and the cobalt concentration of the solution after cobalt removal was 0.007 g / L; the solution after cobalt removal was concentrated and crystallized, with a crystallization rate of 45.71%, to obtain a nickel sulfate product with a lead content of 0.0002% and a cobalt content of 0.02%, and the nickel sulfate product met the nickel sulfate standard for type I batteries. The cobalt tetroxide product is prepared from the cobalt slag through acid dissolution-extraction-pyrolysis.

[0143] The atmospheric leaching residue was subjected to the first stage of pressure leaching in a sulfuric acid solution. The concentration of sulfuric acid in the obtained solution after the atmospheric leaching residue was mixed with the sulfuric acid solution was 10 g / L, the leaching temperature was 150 °C, the leaching time was 1 h, the leaching liquid-solid ratio was 10 L / kg, the oxygen partial pressure was 0.2 MPa, and the first stage of pressure leaching solution and 1.09 kg of the first stage of pressure leaching residue were obtained. The metal leaching rates were 75.03% for nickel, 68.06% for cobalt, 11.03% for copper, and 4.40% for iron.

[0144] The first stage pressure leaching residue was subjected to the second stage pressure leaching in sulfuric acid solution. The concentration of sulfuric acid in the obtained liquid after the first stage pressure leaching residue was mixed with sulfuric acid solution was 10 g / L, the leaching temperature was 150 ℃, the leaching time was 40 min, the leaching liquid-solid ratio was 2 L / kg, the oxygen partial pressure was 0.02 MPa, and the second stage pressure leaching liquid and 0.78 kg of precious metal slag were obtained. The metal leaching rates were 61.38% for nickel, 66.19% for cobalt, 30.86% for copper, and 11.49% for iron. The second stage pressure leaching effect was not good, the slag rate was high, the nickel and copper contents in the precious metal slag were high, the nickel and copper were not well separated, and the precious metals were not well enriched.

[0145] Comparative Example 11 Take 30.0 kg of platinum-palladium concentrate, add 2.40 kg of lime, 6.50 kg of silica, and 2.10 kg of hematite, and smelt at 1400 °C for 40 min. Smelting obtains 7.08 kg of low-grade nickel matte, adds 2.12 kg of silicon dioxide, and blows at 1350 °C with a blowing airflow of 2.0 Nm 3 / h, blowing time is 10 h, and 1.56 kg of high-grade nickel matte is obtained.

[0146] High matte nickel was leached at normal pressure in sulfuric acid solution, with leaching temperature of 70 ℃, leaching time of 8 h, leaching liquid-solid ratio of 6 L / kg, leaching end point pH of 6, and obtained normal pressure leaching solution and 1.33 kg normal pressure leaching residue, with metal leaching rates of 40.40% nickel, 52.43% cobalt, 0.43% copper, and 0.99% iron. The normal pressure leaching solution was subjected to the process of removing lead with barium hydroxide, with the amount of barium hydroxide added being 200 (the molar ratio of barium hydroxide to lead in the normal pressure leaching solution), and the lead concentration of the solution after lead removal was 0.0005 g / L; after the process of removing cobalt with black nickel, with the amount of black nickel added being 18 (the molar ratio of black nickel to cobalt in the normal pressure leaching solution), and the cobalt concentration of the solution after cobalt removal was 0.007 g / L; the solution after cobalt removal was concentrated and crystallized, with a crystallization rate of 45.71%, to obtain a nickel sulfate product with a lead content of 0.0002% and a cobalt content of 0.02%, and the nickel sulfate product met the nickel sulfate standard for type I batteries. The cobalt tetroxide product is prepared from the cobalt slag through acid dissolution-extraction-pyrolysis.

[0147] The atmospheric leaching residue was subjected to the first stage of pressure leaching in a sulfuric acid solution. The concentration of sulfuric acid in the obtained solution after the atmospheric leaching residue was mixed with the sulfuric acid solution was 10 g / L, the leaching temperature was 150 °C, the leaching time was 1 h, the leaching liquid-solid ratio was 10 L / kg, the oxygen partial pressure was 0.2 MPa, and the first stage of pressure leaching solution and 1.09 kg of the first stage of pressure leaching residue were obtained. The metal leaching rates were 75.03% for nickel, 68.06% for cobalt, 11.03% for copper, and 4.40% for iron.

[0148] The first-stage pressure leaching residue was subjected to the second-stage pressure leaching in the sulfuric acid solution. The concentration of sulfuric acid in the obtained liquid after the first-stage pressure leaching residue was mixed with the sulfuric acid solution was 50 g / L, the leaching temperature was 200 °C, the leaching time was 4 h, the leaching liquid-solid ratio was 15 L / kg, the oxygen partial pressure was 1.0 MPa, and the second-stage pressure leaching solution and 20.6 g of precious metal slag were obtained. The metal leaching rates were 99.84% for nickel, 99.68% for cobalt, 99.64% for copper, and 16.98% for iron.

[0149] Test results: The comprehensive recovery rate of nickel is 98.26%, the comprehensive recovery rate of copper is 98.32%, the comprehensive recovery rate of cobalt is 94.35%, the comprehensive recovery rate of gold is 93.72%, the comprehensive recovery rate of silver is 86.38%, the comprehensive recovery rate of platinum is 87.02%, and the comprehensive recovery rate of palladium is 97.06%.

[0150] The second stage of pressure leaching was not effective, the reaction conditions were harsh and the equipment requirements were high, and the recovery rate of silver in precious metals was low.

[0151] The comprehensive recovery rates of metals in Examples 1-13 are shown in Table 1.

[0152] Table 1 Comprehensive recovery rate of metals in Examples 1-13

[0153] The test results of the noble metal enrichment ratios in Examples 1-13 are shown in Table 2.

[0154] Table 2 Precious metal enrichment ratio in Examples 1-13

[0155] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit it. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present application.

[0156] In addition, those skilled in the art will appreciate that, although some embodiments herein include certain features included in other embodiments but not other features, the combination of features of different embodiments is meant to be within the scope of the present application and form different embodiments. For example, in the above claims, any one of the claimed embodiments may be used in any combination. The information disclosed in this background technology section is intended only to deepen the understanding of the overall background technology of the present application and should not be regarded as an admission or in any form of implication that the information constitutes prior art known to those skilled in the art.

Claims

1. A method for comprehensive extraction and utilization of multiple metals in platinum-palladium concentrate, characterized in that: include: Smelting and blowing platinum-palladium concentrate to prepare high-grade nickel matte; The high-matte nickel is mixed with the first acid solution, and leached at normal pressure, wherein the endpoint pH of the normal pressure leaching is 4-7, to obtain a normal pressure leaching solution and a normal pressure leaching residue, wherein the normal pressure leaching solution is purified and impurities are removed, and then evaporated and crystallized to obtain a nickel product and a purified residue, and the purified residue is prepared by acid dissolution-extraction-pyrolysis to obtain a cobalt product; The atmospheric pressure leaching residue is mixed with the second acid solution, and the first stage pressure leaching is performed to obtain the first stage pressure leaching solution and the first stage pressure leaching residue, and the first stage pressure leaching solution is returned to perform the atmospheric pressure leaching; The first stage pressure leaching residue is mixed with the third acid solution, and the second stage pressure leaching is carried out to obtain precious metal slag and the second stage pressure leaching liquid. The second stage pressure leaching liquid is purified and evaporated and crystallized to obtain a copper product and a copper product crystallization liquid. The copper product crystallization liquid is returned to the normal pressure leaching. The precious metal slag is treated to obtain gold, silver, platinum, palladium, osmium, ruthenium, rhodium and iridium precious metals.

2. The method for comprehensive extraction and utilization of multiple metals in platinum-palladium concentrate according to claim 1, characterized in that: The smelting and blowing of the platinum-palladium concentrate to prepare high-grade nickel matte comprises: smelting the platinum-palladium concentrate with a flux to obtain low-grade nickel matte containing copper and nickel; blowing the low-grade nickel matte and silicon dioxide to obtain high-grade nickel matte and blowing slag, and returning the blowing slag to carry out the smelting; And / or, the flux includes one or more of silica, hematite, and lime; and / or, the mass of the flux is 20-40% of the mass of the platinum-palladium concentrate; And / or, the smelting temperature is 1350-1450°C; And / or, the smelting time is 20-60 min; And / or, the mass of the silicon dioxide is 20-40% of the mass of the low nickel matte; And / or, the blowing temperature is 1200-1400°C; And / or, the blowing time is 2-12 h; And / or, the blowing air flow rate of the blowing is 1-4 Nm 3 / h.

3. The method for comprehensive extraction and utilization of multiple metals in platinum-palladium concentrate according to claim 1, characterized in that: The first acid solution includes a sulfuric acid solution; And / or, the temperature of the atmospheric pressure leaching is 50-95°C; And / or, the normal pressure leaching time is 3-10 h; And / or, the liquid-to-solid ratio of the first acid solution and the high nickel matte is 2-12 L / kg.

4. The method for comprehensive extraction and utilization of multiple metals in platinum-palladium concentrate according to claim 1, characterized in that: The purification and impurity removal of the atmospheric pressure leachate includes: adding a barium compound to the atmospheric pressure leachate to remove lead, adding black nickel to remove cobalt, obtaining a filtrate and a purified slag, and evaporating and crystallizing the filtrate to obtain a nickel product.

5. The method for comprehensive extraction and utilization of multiple metals in platinum-palladium concentrate according to claim 4, characterized in that: The barium compound includes one or more of barium carbonate, barium chloride, barium sulfide, barium nitrate, and barium hydroxide.

6. The method for comprehensive extraction and utilization of multiple metals in platinum-palladium concentrate according to claim 4, characterized in that: The molar ratio of the barium compound to the lead in the atmospheric pressure leaching solution is 50-500.

7. The method for comprehensive extraction and utilization of multiple metals in platinum-palladium concentrate according to claim 4, characterized in that: The molar ratio of the black nickel to the cobalt in the atmospheric pressure leaching solution is 2-20.

8. The method for comprehensive extraction and utilization of multiple metals in platinum-palladium concentrate according to claim 1, characterized in that: The initial acidity of the first stage of pressure leaching is 10-30 g / L, and the initial acidity of the first stage of pressure leaching refers to: the concentration of the second acid solution in the liquid obtained after the atmospheric pressure leaching residue is mixed with the second acid solution; and / or, the second acid solution comprises a sulfuric acid solution; and / or, the temperature of the first stage of pressure leaching is 140-170°C; And / or, the first stage of pressure leaching time is 1-3 h; and / or, the liquid-to-solid ratio of the second acid solution to the atmospheric pressure leaching residue is 4-10 L / kg; And / or, the oxygen partial pressure of the first stage of pressure leaching is 0.05-0.3 MPa.

9. The method for comprehensive extraction and utilization of multiple metals in platinum-palladium concentrate according to claim 1, characterized in that: The initial acidity of the second stage of pressure leaching is 20-40 g / L, and the initial acidity of the second stage of pressure leaching refers to: the concentration of the third acid solution in the feed solution obtained after the first stage of pressure leaching residue is mixed with the third acid solution; and / or, the third acid solution comprises a sulfuric acid solution; and / or, the temperature of the second stage of pressure leaching is 160-180°C; And / or, the second stage of pressure leaching time is 1-3 h; and / or, the liquid-to-solid ratio of the third acid solution to the first stage pressure leaching residue is 4-10 L / kg; And / or, the oxygen partial pressure of the second stage of pressure leaching is 0.05-0.5 MPa.

10. The method for comprehensive extraction and utilization of multiple metals in platinum-palladium concentrate according to any one of claims 1 to 9, characterized in that: The purification of the second-stage pressurized leaching solution includes: adding one or more of alkali and alkali solution to the second-stage pressurized leaching solution.

Citation Information

Cited By

  • Method for smelting platinum-rich nickel matte

    CN120400553A

  • A method for smelting platinum-rich nickel matte

    CN120400553B