Preparation method of lanthanum-doped oxide semiconductor transistor
By doping the indium oxide film with lanthanum element, the oxygen vacancy concentration is regulated by atomic layer deposition method, the trade-off relationship and bias stability of mobility and threshold voltage in indium oxide materials are solved, and a high-performance oxide semiconductor field effect transistor is realized Preparation.
Patent Information
- Application Number
- CN202411103979.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-08-13
AI Technical Summary
Due to the high intrinsic carrier concentration and high defect state density, it is difficult for indium oxide materials to effectively control mobility and threshold voltage through the gate electric field, and the bias voltage stability is low.
The indium oxide film doped with lanthanum element is used to control the lanthanum doping ratio through atomic layer deposition method, and the oxygen vacancies concentration is regulated, so as to achieve coordinated optimization of mobility, threshold voltage and bias stability.
Effectively reduce the intrinsic carrier concentration of indium oxide film, improve threshold voltage and device stability, and is suitable for high-performance dynamic memory, display thin film transistors and flexible circuits.
Smart Images

Figure CN119008704A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of oxide semiconductors, and in particular to a method for preparing a lanthanum-doped oxide semiconductor field effect transistor. Background Art
[0002] Oxide semiconductor channel materials have been a research hotspot in recent years. They have extremely low off-state leakage current, excellent field-effect mobility, and thermal budget compatible with back-end processes. They have broad application prospects in dynamic memory, display thin film transistors, flexible devices, and back-end compatible logic circuits. Among many oxide semiconductor field-effect transistors, indium oxide has attracted much attention due to its high field-effect mobility. However, on the one hand, due to the high intrinsic carrier concentration of indium oxide itself, it is difficult to effectively control it through the gate electric field, and there is a trade-off relationship between mobility and threshold voltage. On the other hand, indium oxide also has a high defect state density and low indium-oxygen bond energy, which limits its bias stability. In order to deal with the above problems, element doping is an important and foreseeable approach. Some metal cations have a higher binding energy with oxygen than indium ions themselves, which can be used as oxygen vacancy inhibitors. Doping into the channel can effectively reduce the intrinsic carrier concentration of indium oxide films, thereby achieving adjustable threshold voltage and good bias stability. Among many elements, the metal cation of lanthanum has a very high binding energy with oxygen (789 kJ / mol), exceeding that of indium (360 kJ / mol), zinc (284 kJ / mol), gallium (374 kJ / mol) and other elements, and has great application potential in oxide semiconductor doping. Summary of the invention
[0003] In view of the above-mentioned deficiencies in the prior art, an object of the present invention is to provide a method for preparing a lanthanum-doped oxide semiconductor field effect transistor, thereby realizing an oxide semiconductor device with adjustable mobility and threshold voltage and good bias stability.
[0004] The technical solution provided by the present invention is as follows:
[0005] A method for preparing an oxide semiconductor field effect transistor, the oxide semiconductor field effect transistor comprising a substrate, a gate electrode, a gate electrode dielectric, a channel layer and a source-drain electrode, characterized in that the channel layer is a lanthanum-doped indium oxide film, the channel layer adopts an atomic layer deposition (ALD) method, the atomic layer deposition temperature is controlled within the range of 100° C. to 400° C., one La atomic layer deposition is inserted into each n In atomic layer deposition cycle, and the cycle is repeated x times to obtain a lanthanum-doped indium oxide film, and the specific steps include:
[0006] 1) placing the substrate in an atomic layer deposition chamber, and accurately controlling the indium source content entering the chamber by the electromagnetic valve switch time t1, the corresponding t1 range is 0.01 to 10 s, ensuring that the precursor adsorption is a self-limiting reaction, and then purging with nitrogen or argon, the purge time t2 is controlled by the electromagnetic valve, and the corresponding t2 time range is 1 to 100 s;
[0007] 2) The oxygen source content introduced into the chamber is precisely controlled by the solenoid valve switch time t3, and the corresponding t3 range is 0.01 to 50 seconds. After the precursor reacts completely, nitrogen or argon is used for purging. The purging time t4 is controlled by the solenoid valve, and the corresponding t4 time range is 1 to 100 seconds.
[0008] 3) After repeating step 1) and step 2) n times, In atomic layer deposition is obtained;
[0009] 4) placing the deposition substrate in the atomic layer deposition chamber, and accurately controlling the lanthanum source content entering the chamber by the electromagnetic valve switch time t5, the corresponding t5 range is 0.01 to 10 s, ensuring that the precursor adsorption is a self-limiting reaction, and then purging with nitrogen or argon, the purge time t6 is controlled by the electromagnetic valve, and the corresponding t6 time range is 1 to 100 s;
[0010] 5) The oxygen source content introduced into the chamber is precisely controlled by the solenoid valve switch time t7, and the corresponding t7 range is 0.01 to 50 s. After the precursor reaction is complete, nitrogen or argon is used for purging. The purging time t8 is controlled by the solenoid valve, and the corresponding t8 time range is 1 to 100 s. One La atomic layer deposition is obtained;
[0011] 6) Repeat step 1) to step 5) x times to obtain a lanthanum-doped indium oxide thin film.
[0012] Furthermore, the doping molar ratio of lanthanum atoms is 0.01 mol% to 30 mol%, that is, the ratio of lanthanum atoms / (lanthanum atoms+oxygen atoms+indium atoms).
[0013] Furthermore, n is an integer of 1-60, and x is an integer of 1-20.
[0014] Furthermore, in atomic layer deposition, the indium source includes one or more of trimethylindium, diethylindium, triethylindium, and cyclopentadienylindium.
[0015] Furthermore, in the atomic layer deposition, the lanthanum source is tris(N,N'-diisopropylformamidinium)lanthanum.
[0016] Furthermore, in atomic layer deposition, the oxygen source includes one or more of water, oxygen, ozone, hydrogen peroxide, and oxygen plasma.
[0017] Furthermore, in atomic layer deposition, the purge gas includes argon, nitrogen, etc.
[0018] Furthermore, the substrate includes one or more of silicon, sapphire, silicon carbide, gallium nitride, diamond, and a flexible substrate.
[0019] Furthermore, the gate electrode includes one or more of nickel, platinum, gold, tungsten, titanium nitride, and indium tin oxide.
[0020] Furthermore, the gate dielectric includes one or more of silicon oxide, aluminum oxide, hafnium oxide, zirconium oxide, and lanthanum oxide.
[0021] Furthermore, the source-drain electrode material includes one or more of nickel, platinum, gold, tungsten, titanium nitride, and indium tin oxide.
[0022] The oxide semiconductor field effect transistor of the present invention includes but is not limited to a back gate structure, a top gate structure, a double gate structure, a fin structure, and a surrounding gate structure.
[0023] Oxide semiconductor field effect transistors can be used to prepare dynamic random access memory (DRAM). The device structure can be a planar structure or can be used for three-dimensional stacked heterogeneous integrated logic circuits.
[0024] The technical effects of the present invention are as follows:
[0025] The present invention proposes a lanthanum-doped indium oxide channel material using an atomic layer deposition method. By controlling the value of n, the thickness of indium oxide can be precisely controlled, and by controlling the value of x, the content of the doped lanthanum element can be precisely controlled. The lanthanum doping ratio is regulated to control the oxygen vacancy concentration in the channel, thereby achieving coordinated optimization of threshold voltage, mobility, and stability. The optimized oxide semiconductor field effect transistor can be used in high-performance dynamic memory, display thin film transistors, flexible circuits, and back-end compatible logic circuits. Compared with ordinary indium oxide materials, the present invention has the following main advantages:
[0026] 1) By doping with lanthanum, the generation of oxygen vacancies can be suppressed, which can effectively reduce the intrinsic carrier concentration of the indium oxide film, thereby increasing the transistor threshold voltage;
[0027] 2) The lanthanum-oxygen bond dissociation energy is higher, which can improve the bottom position of the conduction band and increase the activation energy of n-type doping, thereby improving the stability of the device. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 Schematic diagram of preparing a channel layer by atomic layer deposition stacking according to the present invention.
[0029] Figure 2 Schematic diagram of the atomic layer deposition process of the present invention.
[0030] Figure 3 Schematic diagram of a transistor according to a specific embodiment of the present invention, wherein (a) is a back gate and (b) is a top gate.
[0031] Figure 4 The figure is a flow chart for preparing a back-gate transistor according to a specific embodiment of the present invention.
[0032] Figure 5 The figure is a flow chart for preparing a top-gate transistor according to a specific embodiment of the present invention.
[0033] Figure 6 It is a comparison diagram of transfer characteristic curves of the lanthanum-doped indium oxide transistor according to a specific embodiment of the present invention and the pure indium oxide thin film transistor according to a comparative example.
[0034] In the figure, 1 is substrate; 2 is back gate electrode; 3 is dielectric layer; 31 is In2O3 layer; 32 is La2O3 layer; 4 is channel layer; 5 is Ni layer of source electrode; 6 is Au layer of drain electrode; 7 is Pt layer of top gate electrode; 8 is Au layer of top gate electrode. DETAILED DESCRIPTION
[0035] The present invention provides a method for preparing a lanthanum-doped oxide semiconductor field effect transistor, and is applied to field effect transistors of various structures and storage, display and logic circuits based on field effect transistors.
[0036] The embodiments of the present invention are described in detail below in conjunction with the accompanying drawings. However, those skilled in the art should understand that the following embodiments are only used to illustrate the present invention and should not be regarded as limiting the scope of the present invention.
[0037] The channel layer of the oxide semiconductor field effect transistor of the present invention is a lanthanum-doped indium oxide film, such as Figure 1 As shown, the present invention prepares a lanthanum-doped indium oxide film through the number of atomic layer deposition cycles, and performs one La atomic layer deposition after every n In atomic layer deposition cycles, and repeats x times to obtain a lanthanum-doped indium oxide film. Wherein, x and n are both greater than or equal to 1. The thickness of indium oxide can be precisely controlled by controlling the value of n, and the content of lanthanum doped can be precisely controlled by controlling the value of x. For example, when n=4, lanthanum doping is performed once after every 4 indium oxide atomic layer deposition cycles; when n=8, lanthanum doping is performed once after every 8 indium oxide atomic layer deposition cycles; when n=12, lanthanum doping is performed once after every 12 indium oxide atomic layer deposition cycles; when n=16, lanthanum doping is performed once after every 16 indium oxide atomic layer deposition cycles, and so on. The process within the atomic layer deposition small cycle is as follows. Figure 2 As shown, it is divided into four steps:
[0038] In the first step, the deposition substrate is placed in the atomic layer deposition chamber, and the indium source content entering the chamber is accurately controlled by the solenoid valve switching time t1. The corresponding t1 range is 0.01 to 10 s. After ensuring that the precursor adsorption is a self-limiting reaction, it is purged with nitrogen or argon. The purge time t2 is controlled by the solenoid valve and the time range is 1 to 100 s.
[0039] In the second step, the oxygen source content introduced into the chamber is precisely controlled by the electromagnetic valve switch time t3, and the corresponding t3 range is 0.01 to 50 seconds. After the precursor reacts completely, nitrogen or argon is purged, and the purge time t4 is controlled by the electromagnetic valve, and the time range is 1 to 100 seconds. After repeating the first and second steps n times, a certain thickness of indium oxide is obtained, and the third step is carried out.
[0040] The third step is to place the deposition substrate in the atomic layer deposition chamber, and accurately control the lanthanum source content entering the chamber through the solenoid valve switching time t5, and the corresponding t5 range is 0.01 to 10s. After ensuring that the precursor adsorption is a self-limiting reaction, it is purged with nitrogen or argon. The purge time t6 is controlled by the solenoid valve, and the time range is 1 to 100s.
[0041] The fourth step is to accurately control the oxygen source content entering the chamber through the solenoid valve switching time t7, and the corresponding t7 range is 0.01~50s. After the precursor reacts completely, it is purged with nitrogen or argon. The purge time t8 is controlled by the solenoid valve and the time range is 1~100s.
[0042] Repeat the first step to the fourth step to achieve the growth of the lanthanum-doped indium oxide thin film.
[0043] Embodiment 1
[0044] Based on the structure of lanthanum-doped oxide semiconductor back-gate transistors, Figure 3 As shown in (a), it includes a substrate, a back gate electrode layer located on the substrate, a dielectric layer on the back gate electrode, a channel layer on the dielectric layer, a source layer and a drain layer. The specific preparation steps are as follows:
[0045] Step 1: Substrate cleaning. Select a high-resistance silicon substrate 1 with good electrical insulation and a resistivity of >10 4 Ω·cm. Use standard RCA to clean the substrate. First, soak it in RCA-1 (deionized water: ammonia: hydrogen peroxide = 5:1:1) at 70°C for 10 minutes to clean the metal cations, organic matter and other contaminants on the substrate. After cleaning, blow it dry with high-purity nitrogen. Figure 4 As shown in (a).
[0046] Step 2, preparing a back gate electrode 2, such as Figure 4As shown in (b), the process specifically includes the following steps: coating, baking, exposure, development, physical vapor deposition, and lift-off.
[0047] Step 3, using atomic layer deposition to deposit a dielectric material with a thickness of 1 to 100 nm as a gate dielectric layer 3 on the sample obtained in step 2, such as Figure 4 As shown in (c).
[0048] Step 4: A lanthanum-doped indium oxide thin film layer is prepared by atomic layer deposition of the present invention, with a deposition thickness of 1 to 20 nm.
[0049] Step 5, defining and forming a channel layer 4 on the deposited lanthanum-doped indium oxide film, such as Figure 4 As shown in (d), the process specifically includes the following steps: spin coating photoresist, baking, exposure, development, oxygen plasma cleaning to remove residual photoresist, wet etching, etc.
[0050] Step 6, preparing the Ni layer 5 and the Au layer 6 of the source and drain electrodes, such as Figure 4 As shown in (e), the process specifically includes the following steps: coating, baking, exposure, development, physical vapor deposition, and lift-off.
[0051] Embodiment 2
[0052] Based on the top-gate transistor structure of lanthanum-doped oxide semiconductors, Figure 3 As shown in (b), it includes a substrate, a channel layer, a dielectric layer, a source layer and a drain layer located on the substrate 1, and a top gate electrode layer located on the dielectric layer. The specific preparation steps are as follows:
[0053] Step 1: Substrate cleaning. Select a high-resistance silicon substrate 1 with good electrical insulation and a resistivity of >10 4 Ω·cm. Use standard RCA to clean the substrate 1. First, soak it in RCA-1 (deionized water: ammonia: hydrogen peroxide = 5:1:1) at 70°C for 10 minutes to clean the metal cations, organic matter and other contaminants on the substrate. After cleaning, blow it dry with high-purity nitrogen. Figure 5 As shown in (a).
[0054] Step 2: A lanthanum-doped indium oxide thin film layer is prepared by atomic layer deposition of the present invention, with a deposition thickness of 1 to 20 nm.
[0055] Step 3, defining and forming a channel layer 4 on the deposited lanthanum-doped indium oxide film, such as Figure 5 As shown in (b), the process specifically includes the following steps: spin coating photoresist, baking, exposure, development, oxygen plasma cleaning to remove residual photoresist, wet etching, etc.
[0056] Step 4, prepare the Ni layer 7 and Au layer 8 of the source and drain electrodes, as Figure 5As shown in (c), the process specifically includes the following steps: coating, baking, exposure, development, physical vapor deposition, and lift-off.
[0057] Step 5: Deposit a dielectric material with a thickness of 1 to 100 nm as a gate dielectric layer 3 on the sample obtained in step 4 by atomic layer deposition. Figure 5 As shown in (d).
[0058] Step 6, prepare the Pt layer 7 and Au layer 8 of the top gate electrode, such as Figure 5 As shown in (e), the process steps include coating, baking, exposure, development, physical vapor deposition, and stripping.
[0059] The above two embodiments are merely presented as a way of describing the implementation of the present invention. However, those skilled in the art should understand that the above embodiments are only used to illustrate the present invention and should not be regarded as limiting the scope of the present invention.
[0060] The comparative example provides a method for preparing a thin film transistor, and the prepared pure indium oxide thin film transistor is used. The difference between the comparative document 1 and the above-mentioned embodiment 1 is that the channel layer of the transistor of the present invention is a lanthanum-doped indium oxide thin film. The transfer characteristic curve test is performed on the device prepared in the comparative example 1 and the device prepared in the embodiment 1, and the channel length is 1 μm, respectively. Figure 6 As shown in curves A and B, the threshold voltage of the back-gate transistor of pure indium oxide in comparative example 1 is about -0.7V, while the threshold voltage of the lanthanum-doped indium oxide thin film transistor in embodiment 1 is about 0.4V, indicating that lanthanum doping can inhibit the generation of oxygen vacancies and effectively reduce the intrinsic carrier concentration of the indium oxide film, thereby increasing the transistor threshold voltage by more than 1V.
[0061] It should be noted that the above-mentioned embodiments illustrate rather than limit the invention and that those skilled in the art will be able to design alternative embodiments without departing from the scope of the appended claims.
Claims
1. A method for preparing an oxide semiconductor field effect transistor, the oxide semiconductor field effect transistor comprising a substrate, a gate electrode, a gate electrode dielectric, a channel layer and a source-drain electrode, characterized in that: The channel layer is a lanthanum-doped indium oxide film, and the channel layer adopts an atomic layer deposition ALD method. The atomic layer deposition temperature is controlled in the range of 100°C to 400°C. After every n In atomic layer deposition cycles, one La atomic layer deposition is inserted, and the cycle is repeated x times to obtain a lanthanum-doped indium oxide film. The specific steps include: 1) placing the substrate in an atomic layer deposition chamber, controlling the content of the indium source introduced into the chamber by an electromagnetic valve, wherein the electromagnetic valve switch time t1 ranges from 0.01 to 10 seconds, and then purging with nitrogen or argon gas, wherein the purge time t2 is controlled by the electromagnetic valve, and the corresponding t2 time ranges from 1 to 100 seconds; 2) The oxygen source content in the cavity is introduced through the solenoid valve switch time t3, and the corresponding t3 range is 0.01 to 50 seconds, and then purged with nitrogen or argon. The purge time t4 is controlled by the solenoid valve, and the corresponding t4 time range is 1 to 100 seconds; 3) After repeating step 1) and step 2) n times, In atomic layer deposition is obtained; 4) placing the deposition substrate in the atomic layer deposition chamber again, and accurately controlling the lanthanum source content in the chamber by the electromagnetic valve switch time t5, the corresponding t5 range is 0.01 to 10 s, and then purging with nitrogen or argon, the purge time t6 is controlled by the electromagnetic valve, and the corresponding t6 time range is 1 to 100 s; 5) The oxygen source content introduced into the chamber is precisely controlled by the electromagnetic valve switch time t7, and the corresponding t7 range is 0.01 to 50 s, and then purged by nitrogen or argon, and the purge time t8 is controlled by the electromagnetic valve, and the corresponding t8 time range is 1 to 100 s; one La atomic layer deposition is obtained; 6) Repeat step 1) to step 5) x times to obtain a lanthanum-doped indium oxide film.
2. The preparation method according to claim 1, characterized in that The molar ratio of lanthanum atoms to lanthanum atoms+oxygen atoms+indium atoms in the lanthanum-doped indium oxide film is 0.01 mol% to 30 mol%.
3. The preparation method according to claim 1, characterized in that: The n is an integer of 1-60, and the x is an integer of 1-20.
4. The preparation method according to claim 1, characterized in that: The indium source is selected from one or more of trimethylindium, diethylindium, triethylindium, and cyclopentadienylindium.
5. The preparation method according to claim 1, characterized in that: The lanthanum source is tris(N,N'-diisopropylformamidinium)lanthanum.
6. The preparation method according to claim 1, characterized in that: The oxygen source is selected from one or more of water, oxygen, ozone, hydrogen peroxide, and oxygen plasma.
7. The preparation method according to claim 1, characterized in that: The purge gas is argon or nitrogen.
8. The preparation method according to claim 1, characterized in that: The substrate is selected from one or more of silicon, sapphire, silicon carbide, gallium nitride, diamond, and a flexible substrate.
9. The preparation method according to claim 1, characterized in that: The gate electrode is selected from one or more of nickel, platinum, gold, tungsten, titanium nitride, and indium tin oxide, and the gate dielectric is selected from one or more of silicon oxide, aluminum oxide, hafnium oxide, zirconium oxide, and lanthanum oxide.
10. The preparation method according to claim 1, characterized in that: The source-drain electrode material is selected from one or more of nickel, platinum, gold, tungsten, titanium nitride, and indium tin oxide.
Citation Information
Patent Citations
Metal oxide thin film transistor, manufacturing method thereof and array substrate
CN115084277A
In2O3 thin film resistivity control by doping metal oxide insulator for MFMox device applications
US20050151210A1
KR20220026404A
Cited By
Transistor with improved self-heating effect and preparation method thereof
CN119894032A