Bamboo fiber-based electromagnetic wave absorbing material and preparation method thereof
By using bamboo fiber-based electromagnetic wave absorption materials synthesized by aniline, bamboo fiber and graphene oxide, and combining epoxy resin to prepare electromagnetic wave absorption covers, the problem of insufficient electromagnetic wave absorption performance of bamboo fiber materials is solved, and efficient electromagnetic wave absorption effect is achieved. Bamboo fiber application field.
Patent Information
- Application Number
- CN202410743536.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-11
- Publication Date
- 2024-11-22
AI Technical Summary
Existing bamboo fiber materials have insufficient performance in electromagnetic wave absorption and are difficult to meet diversified market demand.
Using aniline, bamboo fiber and graphene oxide as raw materials, bamboo fibers are synthesized through low-temperature in-situ polymerization, and combined with epoxy resin to prepare an electromagnetic wave absorber to optimize the microstructure and electromagnetic wave absorption performance of the material. .
It has achieved efficient absorption performance of bamboo fiber-based electromagnetic wave absorbing materials, with a peak electric field reduction of 50% and a peak magnetic field reduction of 50%. It is suitable for radiation-proof clothing, electromagnetic shielded car clothing and other products, broadening the application direction of bamboo fiber materials.
Smart Images

Figure CN119012665A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of bamboo fibers, and in particular to a bamboo fiber-based electromagnetic wave absorbing material and a preparation method thereof, and a bamboo fiber-based electromagnetic wave absorbing cover and a preparation method thereof. Background Art
[0002] Bamboo fiber is a new type of fiber material, which is generally divided into two types: bamboo fiber (BF) and bamboo viscose fiber (BVF). BF is prepared by a variety of physical methods, thus retaining the antibacterial, deodorizing and UV protection features of bamboo itself. BVF is made of bamboo through special chemical treatment and technical processing. Compared with BF, its antibacterial, deodorizing and UV protection features are relatively weaker, but it has better durability, better comfort, stronger wear resistance and other characteristics, which also makes it popular among the public.
[0003] At present, bamboo fiber has been widely used in building materials, furniture, automobiles and textiles. Especially in the textile field, bamboo fiber has attracted people's attention due to its good air permeability and antibacterial properties. And with the improvement of people's environmental awareness, the market demand for bamboo fiber as an environmentally friendly and renewable fiber material is also growing. Therefore, by utilizing the characteristics and existing application directions of bamboo fiber, its functions such as conductivity and absorption of electromagnetic waves can be expanded to meet the diversified market demand. Summary of the invention
[0004] The purpose of the present invention is to solve the shortcomings of the prior art and to propose a bamboo fiber-based electromagnetic wave absorbing material and a preparation method thereof, and a bamboo fiber-based electromagnetic wave absorbing cover and a preparation method thereof.
[0005] A bamboo fiber-based electromagnetic wave absorbing material, the raw materials of which include: aniline, bamboo fiber and graphene oxide; the mass ratio of aniline, bamboo fiber and graphene oxide is 3.0-3.1:1-6:0-0.15, and the mass of graphene oxide is not 0.
[0006] Preferably, aniline is in situ polymerized on the surfaces of bamboo fiber and graphene oxide.
[0007] Preferably, the bamboo fiber-based electromagnetic wave absorbing material has an RLmin of ≤-30.23 dB and an effective absorption bandwidth of ≤6.88 GHz.
[0008] The method for preparing the above-mentioned bamboo fiber-based electromagnetic wave absorbing material comprises the following steps:
[0009] (1) mixing aniline and L-camphorsulfonic acid solution, adding bamboo fiber and graphene oxide aqueous dispersion, and ultrasonically dispersing to obtain a first material;
[0010] (2) dissolving the initiator in a L-camphorsulfonic acid solution to obtain a second material;
[0011] (3) placing the first material in an ice bath environment, maintaining the temperature of the first material at 5±1° C., then dropwise adding the second material thereto, stirring, washing, filtering, and drying.
[0012] Preferably, in step (1), the mass concentration of the graphene oxide aqueous dispersion is 2.8-3.2 g / L.
[0013] Preferably, the concentration of the L-camphorsulfonic acid solution used in step (1) is the same as that of the L-camphorsulfonic acid solution used in step (2).
[0014] Preferably, in step (1), the concentration of the L-camphorsulfonic acid solution is 0.25-1.50 mol / L, and the volume ratio of aniline to the L-camphorsulfonic acid solution is 2.8-3.2:27-33.
[0015] Preferably, in step (2), the initiator is a persulfate, preferably ammonium persulfate.
[0016] Preferably, in the second material, the initiator concentration is 0.25-1.50 mol / L.
[0017] Preferably, in the second material, the concentration of the initiator is the same as the concentration of L-camphorsulfonic acid.
[0018] Preferably, in step (3), deionized water and anhydrous ethanol are used for washing and filtration until the filtrate is neutral and colorless.
[0019] Preferably, in step (3), the drying temperature is 48-52° C. and the drying time is 22-26 h.
[0020] A bamboo fiber-based electromagnetic wave absorption cover is made of the bamboo fiber-based electromagnetic wave absorption material, and its electric field peak value is ≤103V / m, and its magnetic field peak value is ≤0.09uT.
[0021] Preferably, the raw materials include: the above-mentioned bamboo fiber-based electromagnetic wave absorbing material, epoxy resin and curing agent, the mass ratio of the above-mentioned bamboo fiber-based electromagnetic wave absorbing material to the epoxy resin is 2.5-3.5:6.5-7.5, and the mass ratio of the curing agent to the epoxy resin is 2.5-3.5:6.5-7.5.
[0022] Preferably, the curing agent is benzyl alcohol.
[0023] The bamboo fiber-based electromagnetic wave absorbing cover is prepared by mixing the bamboo fiber-based electromagnetic wave absorbing material with epoxy resin, adding a curing agent, mixing evenly, and injecting the mixture into a mold and letting it stand.
[0024] Preferably, the standing time is 6-10 days.
[0025] The present invention synthesizes a bamboo fiber-based electromagnetic wave absorbing material by a low-temperature in-situ polymerization method, and conducts a comprehensive exploration and research on its microstructure, components, electromagnetic wave absorbing performance, conductive performance, thermal stability, etc.
[0026] The conductivity of the obtained bamboo fiber-based electromagnetic wave absorbing material can reach 1.6S / cm; while the RLmin can reach -37.91dB, the thickness is 2mm, the frequency is 14.08GHz; the effective absorption bandwidth is 6.52GHz, the frequency range is 11.84-17.36GHz, and the thickness is 2mm.
[0027] The present invention combines bamboo fiber-based electromagnetic wave absorption material with epoxy resin to prepare a corresponding physical product, an electromagnetic wave absorption cover, and conducts performance testing on it. The electric field peak is as low as 85V / m, and the magnetic field peak is as low as 0.06uT. It can reduce the electric field intensity and magnetic field intensity by about 50%, and has a significant absorption effect on electromagnetic waves. It is fully expected to be applied to products and directions such as radiation protection clothing, electromagnetic shielding car clothes, electromagnetic wave absorption blankets and darkroom wall materials.
[0028] The present invention has the advantages of simple preparation, light texture, thin thickness, wide effective absorption frequency band, strong electromagnetic wave absorption capacity, etc., and has the original characteristics of bamboo fiber materials such as UV protection and softness. It not only meets the selection criteria of electromagnetic wave absorption materials "thin, wide, light, and strong", but also takes into account the original characteristics of bamboo fiber materials. Therefore, the present invention is fully expected to become a new choice of low-cost, environmentally friendly, and efficient electromagnetic wave absorption materials, and at the same time broadens the application direction of bamboo fiber materials, increases the market demand for bamboo fiber products, and provides a reference for the research and development of electromagnetic wave absorption materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 Effects of graphene oxide addition amount (a), L-camphorsulfonic acid concentration (b), ammonium persulfate concentration (c) and bamboo fiber addition amount (d) on the conductivity of bamboo fiber-based electromagnetic wave absorbing materials.
[0030] Figure 2 Fourier infrared spectra of bamboo viscose fiber (BVF), bamboo fiber-based electromagnetic wave absorbing material (PANI / BVF) obtained in Comparative Example 2, bamboo fiber-based electromagnetic wave absorbing material (GO / PANI / BVF) obtained in Example 3, bamboo fibril (BF), bamboo fiber-based electromagnetic wave absorbing material (PANI / BF) obtained in Comparative Example 1, and bamboo fiber-based electromagnetic wave absorbing material (GO / PANI / BF) obtained in Example 2.
[0031] Figure 3X-ray diffraction patterns of bamboo viscose fiber (BVF), bamboo fiber-based electromagnetic wave absorbing material (PANI / BVF) obtained in Comparative Example 2, bamboo fiber-based electromagnetic wave absorbing material (GO / PANI / BVF) obtained in Example 3, bamboo fibril (BF), bamboo fiber-based electromagnetic wave absorbing material (PANI / BF) obtained in Comparative Example 1, and bamboo fiber-based electromagnetic wave absorbing material (GO / PANI / BF) obtained in Example 2.
[0032] Figure 4 These are scanning electron microscope images of bamboo viscose fiber (a, b), bamboo fiber-based electromagnetic wave absorbing material obtained in Comparative Example 2 (d, e) and bamboo fiber-based electromagnetic wave absorbing material obtained in Example 3 (g, h), as well as transmission electron microscope images of bamboo viscose fiber (c), bamboo fiber-based electromagnetic wave absorbing material obtained in Comparative Example 2 (f) and bamboo fiber-based electromagnetic wave absorbing material (i) obtained in Example 3.
[0033] Figure 5 These are scanning electron microscope images of bamboo fibers (a, b), bamboo fiber-based electromagnetic wave absorbing materials obtained in comparative example 1 (d, e) and bamboo fiber-based electromagnetic wave absorbing materials obtained in example 2 (g, h); and transmission electron microscope images of bamboo fibers (c), bamboo fiber-based electromagnetic wave absorbing materials obtained in comparative example 1 (f) and bamboo fiber-based electromagnetic wave absorbing materials obtained in example 2 (i).
[0034] Figure 6 EDS spectra of bamboo viscose fiber (a), bamboo fiber-based electromagnetic wave absorbing material (b) obtained in Comparative Example 2, bamboo fiber-based electromagnetic wave absorbing material (c) obtained in Example 3, bamboo fiber (i), bamboo fiber-based electromagnetic wave absorbing material (j) obtained in Comparative Example 1, and bamboo fiber-based electromagnetic wave absorbing material (k) obtained in Example 2, and the element contents are shown in the inset table;
[0035] Also, SEM images of the bamboo fiber-based electromagnetic wave absorbing material (d) obtained in Example 3 and the bamboo fiber-based electromagnetic wave absorbing material (i) obtained in Example 2, the element distribution of C(e), N(f), O(g) and S(h) in the bamboo fiber-based electromagnetic wave absorbing material obtained in Example 3, and the element distribution diagram of C(m), N(n), O(o) and S(p) in the bamboo fiber-based electromagnetic wave absorbing material obtained in Example 2.
[0036] Figure 7 TG curves (a) and DSC curves (b) of bamboo viscose fiber (BVF), bamboo fiber-based electromagnetic wave absorbing material (PANI / BVF) obtained in Comparative Example 2, bamboo fiber-based electromagnetic wave absorbing material (GO / PANI / BVF) obtained in Example 3, bamboo fibril (BF), bamboo fiber-based electromagnetic wave absorbing material (PANI / BF) obtained in Comparative Example 1, and bamboo fiber-based electromagnetic wave absorbing material (GO / PANI / BF) obtained in Example 2.
[0037] Figure 8 Relative dielectric constant (a, b), relative magnetic permeability (c, d) and tangent loss (e, f) of each group of samples
[0038] Fig. 9 It is the RL value of the bamboo viscose fiber (a), the bamboo fiber-based electromagnetic wave absorbing material (c) obtained in Comparative Example 2, the bamboo fiber-based electromagnetic wave absorbing material (e) obtained in Example 3, the bamboo fiber (b), the bamboo fiber-based electromagnetic wave absorbing material (d) obtained in Comparative Example 1 and the bamboo fiber-based electromagnetic wave absorbing material (f) obtained in Example 2.
[0039] Fig.10 These are the electromagnetic radiation test diagrams of the electromagnetic wave absorption covers obtained by each group. DETAILED DESCRIPTION
[0040] The present invention will be further explained below in conjunction with specific embodiments.
[0041] The moso bamboo fiber (BF) used below was purchased from Sichuan Mousheng New Material Technology Co., Ltd., with a moisture content of 5%. Preparation process: Moso bamboo is processed through the steps of flaking, steaming, crushing, degumming, combing, etc., and finally made into BF. After ultrasonic cleaning, it is dried for standby use.
[0042] The bamboo viscose fiber (BVF) used below was purchased from Shandong Xumou Textile Co., Ltd., with a moisture content of 5%. Preparation process: Pure pulp (α-cellulose) is extracted from bamboo, and then cellulose spinning solution is obtained through chemical treatment, and then BVF is prepared through wet spinning technology. After ultrasonic cleaning, it is dried for standby use.
[0043] The epoxy resin and benzyl alcohol used below were purchased from Dongguan Beimou New Materials Co., Ltd.
[0044] Example 1
[0045] like Figure 1 As shown in (a), the curves of the influence of the addition amount of graphene oxide on the conductivity of the sample are basically consistent. When the addition amount is 90 mg, that is, when the addition ratio of graphene oxide to aniline is 3:100, the conductivity of the sample reaches the best, which is 1.6S / cm and 1.3S / cm respectively.
[0046] When a small amount of graphene oxide is added, most of the oxygen-containing groups of graphene oxide are destroyed by polyaniline, replacing its conjugated structure. At this time, graphene oxide acts like a resistor, reducing the conductivity of the sample.
[0047] As the content of graphene oxide increases, graphene oxide forms a conductive network with polyaniline aggregated on the surface of bamboo viscose fiber and bamboo fibril, which gradually increases the conductivity of the sample. However, after reaching the peak, the excess unpolymerized graphene oxide still reduces the conductivity of the sample.
[0048] from Figure 1 (b) It can be seen that the curves of the effect of L-camphorsulfonic acid concentration on the conductivity of the sample are slightly different, and the optimal values appear at 1 mol / L and 1.25 mol / L respectively. The overall trends are basically similar. With the increase of L-camphorsulfonic acid concentration, the conductivity first increases and then decreases.
[0049] This is because the optimal synthesis environment of polyaniline is pH = 2-3. Appropriate concentration of L-camphorsulfonic acid within a certain range can reduce the pH value of the reaction system, thereby promoting the formation of polyaniline and the effective polymerization of polyaniline on the surface of bamboo fiber.
[0050] like Figure 1 As shown in (c), with the increase of ammonium persulfate concentration, the conductivity of the sample first increases and then decreases. When the concentration of ammonium persulfate is too low, the polymerization reaction between graphene oxide and aniline is not sufficient, and the generated graphene oxide / polyaniline cannot completely cover the bamboo fiber or the wrapping layer is too thin, resulting in a low conductivity.
[0051] When the concentration of ammonium persulfate is too high, there are too many active centers for the polymerization reaction between graphene oxide and aniline, and the reaction is violent, resulting in local oxidation of aniline to generate small molecules. As a result, the graphene oxide / polyaniline is unevenly coated on the surface of the bamboo fiber or the coating layer falls off due to the violent reaction, thereby reducing its conductivity. The optimal values of the samples are ammonium persulfate concentrations of 1 mol / L and 1.25 mol / L, respectively.
[0052] like Figure 1 As shown in (d), with the increase of bamboo fiber addition, the conductivity of the samples first increased and then decreased. When the amount of bamboo fiber added was low, more graphene oxide / polyaniline conductive polymer layers would aggregate on the bamboo fiber surface and easily fall off, resulting in an uneven conductive layer, thus affecting the conductivity of the sample.
[0053] As the amount of bamboo fiber added increases, a proper amount of bamboo fiber is tightly wrapped by the graphene oxide / polyaniline conductive polymer layer, which improves the conductivity of the sample. As the amount of bamboo fiber added continues to increase, the generated graphene oxide / polyaniline cannot completely wrap all the added bamboo fibers, which reduces the conductivity of the sample.
[0054] Therefore, the optimal addition amount of bamboo viscose fiber is 2g, and the optimal addition amount of bamboo raw fiber is 3g.
[0055] In summary, the above-mentioned most preferred method is used for sample preparation, as shown in Examples 2 and 3 below.
[0056] Example 2
[0057] A method for preparing a bamboo fiber-based electromagnetic wave absorbing material comprises the following steps:
[0058] (1) 3 mL of aniline and 30 mL of a 1.25 mol / L left-handed camphorsulfonic acid solution were mixed, and magnetic stirring was performed for 0.5 h. Then, 3 g of bamboo fiber and a graphene oxide aqueous dispersion having a mass concentration of 3 g / L (prepared by ultrasonically dispersing 90 mg of graphene oxide powder in 30 mL of deionized water) were added, and ultrasonic dispersion was performed for 0.5 h to obtain a first material.
[0059] (2) dissolving 5.7 g of ammonium persulfate in 20 mL of 1.25 mol / L L-camphorsulfonic acid solution to obtain a second material;
[0060] (3) The first material was placed in an ice bath environment, the temperature of the first material was maintained at 5±1°C, and the second material was then added dropwise thereto, and electromagnetic stirring was performed for 6 hours. The product was washed with deionized water and anhydrous ethanol for multiple times and filtered until the filtrate was neutral and colorless, and then placed in a drying oven at 50°C for 24 hours to obtain L-CSA-doped GO / PANI / BF composite fibers.
[0061] The electrical conductivity of the GO / PANI / BF composite fiber obtained in this example is 1.6 S / cm.
[0062] Example 3
[0063] A method for preparing a bamboo fiber-based electromagnetic wave absorbing material comprises the following steps:
[0064] (1) 3 mL of aniline and 30 mL of 1 mol / L left-handed camphorsulfonic acid solution were mixed, and magnetic stirring was performed for 0.5 h. Then, 2 g of bamboo viscose fiber and a graphene oxide aqueous dispersion having a mass concentration of 3 g / L (prepared by ultrasonically dispersing 90 mg of graphene oxide powder in 30 mL of deionized water) were added, and ultrasonic dispersion was performed for 0.5 h to obtain a first material;
[0065] (2) dissolving 4.56 g of ammonium persulfate in 20 mL of 1 mol / L left-handed camphorsulfonic acid solution to obtain a second material;
[0066] (3) The first material was placed in an ice bath environment, the temperature of the first material was maintained at 5±1°C, and the second material was then added dropwise thereto, and electromagnetic stirring was performed for 6 hours. The product was washed with deionized water and anhydrous ethanol for multiple times and filtered until the filtrate was neutral and colorless, and then placed in a drying oven at 50°C for 24 hours to obtain L-CSA-doped GO / PANI / BVF composite fibers.
[0067] The electrical conductivity of the GO / PANI / BVF composite fiber obtained in this example is 1.3 S / cm.
[0068] The best conductivity of the bamboo fiber-based electromagnetic wave absorbing material obtained in Example 2 and Example 3 did not reach the range standard of the conductor, and still belonged to semiconductor materials, which basically did not enhance the formation of reflected waves on the surface of the material, resulting in a positive correlation between the conductivity loss of the material and the electromagnetic wave absorption performance. Therefore, the preparation process of the bamboo fiber-based electromagnetic wave absorbing material was optimized, and the electromagnetic wave absorption performance of the material was also improved while the conductivity of the material was improved.
[0069] Comparative Example 1
[0070] (1) 3 mL of aniline and 30 mL of a 1.25 mol / L L-camphorsulfonic acid solution were mixed, magnetically stirred for 0.5 h, and then 3 g of moso bamboo fiber was added, and ultrasonically dispersed for 0.5 h to obtain a first material;
[0071] (2) dissolving 5.7 g of ammonium persulfate in 20 mL of 1.25 mol / L L-camphorsulfonic acid solution to obtain a second material;
[0072] (3) The first material was placed in an ice bath environment, the temperature of the first material was maintained at 5±1°C, and the second material was then added dropwise thereto, and electromagnetic stirring was performed for 6 hours. The product was washed with deionized water and anhydrous ethanol for multiple times and filtered until the filtrate was neutral and colorless, and then placed in a drying oven at 50°C for 24 hours to obtain L-CSA-doped PANI / BF composite fibers.
[0073] Comparative Example 2
[0074] A method for preparing a bamboo fiber-based electromagnetic wave absorbing material comprises the following steps:
[0075] (1) 3 mL of aniline and 30 mL of 1 mol / L camphorsulfonic acid solution were mixed, magnetically stirred for 0.5 h, and then 2 g of bamboo viscose fiber was added, and ultrasonically dispersed for 0.5 h to obtain a first material;
[0076] (2) dissolving 4.56 g of ammonium persulfate in 20 mL of 1 mol / L left-handed camphorsulfonic acid solution to obtain a second material;
[0077] (3) The first material was placed in an ice bath environment, the temperature of the first material was maintained at 5±1°C, and the second material was then added dropwise thereto, and electromagnetic stirring was performed for 6 hours. The product was washed with deionized water and anhydrous ethanol for multiple times and filtered until the filtrate was neutral and colorless, and then placed in a drying oven at 50°C for 24 hours to obtain L-CSA-doped PANI / BVF composite fibers.
[0078] Test Example 1 FT-IR Analysis
[0079] FT-IR was used to analyze the functional group structures of bamboo viscose fiber, PANI / BVF, GO / PANI / BVF, bamboo fibril, PANI / BF and GO / PANI / BF, e.g. Figure 2 shown.
[0080] Bamboo viscose fiber and bamboo fibril show the characteristic peak of bamboo fiber. 3430cm -1 The broad absorption band at 2890cm is due to the stretching vibration of the OH bond. - 1 The characteristic peak at 1640cm is attributed to the stretching vibration of the CH bond. - 1 The absorption peak at 1370 cm is due to the stretching vibration of the C=C bond. - 1 The characteristic peak of secondary hydroxyl appears at 1064cm - 1 At 1040cm - 1 The broad peak at 895 cm - 1 The stretching vibration peak at is caused by the main hydroxyl group.
[0081] The peak shapes of bamboo viscose fiber and bamboo fibril are basically the same, indicating that the positions of their main groups and main bonds have basically not shifted. The direct difference between the two is that the peak of bamboo viscose fiber is higher, which also shows that the groups and bonds of bamboo viscose fiber are more active than those of bamboo fibril.
[0082] By observing the FT-IR curves of PANI / BVF, GO / PANI / BVF, PANI / BF and GO / PANI / BF, the characteristic peaks brought by polyaniline can be clearly seen. - 1 The characteristic peak at 1477 cm is due to the stretching vibration of the C=C bond on the polyaniline quinone ring (N=Q=N). - 1 The absorption peak at 1300cm is caused by the stretching vibration of the C=C bond on the benzene ring (N=B=N) of polyaniline. The bending vibration of the CN bond in aromatic amines causes the absorption peak at 1300cm - 1 The peak position changes at 1137cm - 1 The peak position change at is due to the protonated polyaniline imino group (B-NH + =Q) caused by the bending vibration of the -NH- bond.
[0083] The appearance of these characteristic peaks indicates that the functional amino groups in the aniline monomer are more likely to chemically bond with the polar groups (such as hydroxyl and carboxyl groups) in the bamboo fiber and bamboo viscose fiber. Polyaniline is adsorbed on the polar groups of the bamboo fiber and bamboo viscose fiber through electrostatic action, thereby forming hydrogen bonds. - 1 and 587cm - 1 The absorption peaks appearing nearby are caused by the stretching vibration of the CS bond and the SO bond. The appearance of these two absorption peaks is due to the doping of left-rotatory camphorsulfonic acid, indicating the presence of CSA- in the sample.
[0084] The curves of GO / PANI / BVF and GO / PANI / BF are at 1735cm -1 An absorption peak appeared near the graphene oxide, which was attributed to the stretching vibration of the C=O bond in graphene oxide, indicating the presence of graphene oxide in the composite. Graphene oxide interacted with polyaniline molecules and adsorbed on polyaniline through hydrogen bonds. The FT-IR curve of the sample showed the characteristic peaks of bamboo fiber, graphene oxide and polyaniline, indicating the presence of these substances in the composite.
[0085] Experimental Example 2 XRD Analysis
[0086] The crystal planes and crystal forms of bamboo viscose fiber, PANI / BVF, GO / PANI / BVF, bamboo fibril, PANI / BF and GO / PANI / BF were studied by XRD analysis. Figure 3 As shown. From the diffraction peak curves of bamboo viscose fiber and bamboo fibril, it can be seen that the characteristic diffraction peaks of the two are close, both near 2θ=15° and 22.5°. This is exactly the position of the characteristic diffraction peak of cellulose type II, which also shows that its crystal structure belongs to cellulose type II. It can be clearly seen from the curve that the diffraction peak intensity of bamboo fibril is greater than that of bamboo viscose fiber. This may be because other chemical substances are added to bamboo viscose fiber during production, and the chemical substances form crystal centers. Cellulose molecules are centered on these crystal centers and gradually aggregate to form small crystals, resulting in the diffraction peak intensity being lower than that of large crystal bamboo fibril.
[0087] The XRD curves of PANI / BVF, GO / PANI / BVF, PANI / BF and GO / PANI / BF are similar in shape. The diffraction peaks of the polyaniline generated by polymerization appear near 2θ=15.4°, 21.5° and 24.4°, corresponding to the (010), (100) and (110) crystal planes, respectively, indicating that polyaniline is generated in the sample. The characteristic peaks of sulfonated polyaniline doped with L-camphorsulfonic acid appear at 2θ=16.5°, 18.1° and 19.1°, which also indicates that doped polyaniline appears in the sample.
[0088] The XRD curves of GO / PANI / BVF and GO / PANI / BF show a weak diffraction peak at 2θ=23.2°. This diffraction peak is caused by the graphene (002) crystal plane because the graphene oxide reagent used contains a trace amount of unoxidized graphene. It can be seen from previous studies that graphene oxide will have a strong diffraction peak at 2θ=11°, which corresponds to the (001) crystal plane of graphene oxide. However, due to the large number of oxygen-containing functional groups on the surface of graphene oxide, such as hydroxyl, carbonyl and carboxyl, which react with polyaniline through hydrogen bonds, polyaniline polymerizes and grows on the two-dimensional template graphene oxide, thereby expanding the spacing of graphene oxide, causing the diffraction peak of graphene oxide to gradually move to the small angle area until it disappears. Therefore, the XRD curves of GO / PANI / BVF and GO / PANI / BF do not show the strong diffraction peak unique to graphene oxide.
[0089] The diffraction peak positions of the XRD curves of the four composite materials, PANI / BVF, GO / PANI / BVF, PANI / BF and GO / PANI / BF, are basically similar, indicating that graphene oxide and bamboo fiber are both templates for the growth of polyaniline and do not significantly change the crystal morphology of polyaniline in the composite materials.
[0090] Experimental Example 3 Microstructure Analysis
[0091] Figure 4 (a, b, d, e, g, h) show the low and high magnification SEM images of bamboo viscose fiber, PANI / BVF and GO / PANI / BVF, respectively. Figure 4 (a, b) It can be seen that the bamboo viscose fiber is straight and twist-free, with a smooth and clean surface. A single bamboo viscose fiber is like a cluster of multiple fiber strands, in a clustered shape, and has fine grooves on the surface in the same longitudinal direction of the fiber. Such surface grooves can increase the surface area and enhance the adhesion of polyaniline.
[0092] like Figure 4 As shown in (d, e), polyaniline particles of different sizes are aggregated on the surface of bamboo viscose fiber with varying degrees of uniformity. Figure 4The same is true for the SEM images of GO / PANI / BVF shown in (g, h). Graphene oxide / polyaniline particles of different sizes are aggregated on the surface of bamboo viscose fibers, wrapping the bamboo viscose fibers. Compared with PANI / BVF, the amount of conductive polymer wrapped in GO / PANI / BVF is greater. This shows that the addition of graphene oxide provides a better growth platform for polyaniline, increasing the content of polyaniline in the composite material. Graphene oxide and polyaniline are bonded through hydrogen bonds, and the amino functional groups of polyaniline are chemically bonded to the hydroxyl groups on the surface of bamboo viscose fibers, thereby forming hydrogen bonds. The effective bonding of the three improves the conductivity and electromagnetic wave absorption properties of the composite material.
[0093] Figure 4 (c, f, i) show the TEM images of bamboo viscose fiber, PANI / BVF and GO / PANI / BVF, respectively. Figure 4 As can be seen in (c), bamboo viscose fiber is composed of many tiny fiber particles. This is because bamboo viscose fiber is made of natural cellulose through multiple chemical treatments and then decomposed and polymerized. Therefore, in the nanoscale TEM image, its fibers appear granular. Figure 4 (f) is the TEM image of PANI / BVF, from which it can be seen that the length of the polyaniline nanorods is about 200 nm and they are cross-stacked together. Figure 4 (i) is the TEM image of GO / PANI / BVF, where the wrinkled film structure of graphene oxide can be seen. The length of polyaniline nanorods is about 200 nm. Polyaniline and graphene oxide are staggered and overlapped. At the same time, the fiber particle structure of bamboo viscose fiber is also staggered.
[0094] The low and high magnification SEM images and high magnification TEM images of bamboo fiber, PANI / BF and GO / PANI / BF are shown in Figure 2. Figure 5 As shown. Figure 5 (a, b) It can be seen that the moso bamboo fibers show the surface texture of natural bamboo, with a rough surface and grooves consistent with the longitudinal direction of the fibers. Multiple fibers are aggregated into a bundle. Such a structure is very conducive to the aggregation of conductive polymers on its surface. Figure 5 (c) The TEM image also shows the surface inhomogeneity.
[0095] like Figure 5 As shown in (d, e), polyaniline particles of different sizes aggregate on the surface and in the grooves of the bamboo fibers, forming a coating on the bamboo fibers, but the coating is uneven. Figure 5 The same is true for the SEM images of GO / PANI / BF shown in (g, h), but the coating amount is significantly increased, indicating that graphene oxide is indeed an excellent two-dimensional template material for promoting the growth of polyaniline. Figure 5(f) is the TEM image of PANI / BF. It can be seen that polyaniline is aggregated on the surface of bamboo fibers. At the same time, the shadows are of different depths, which shows its unevenness. Figure 5 (i) is the TEM image of GO / PANI / BF, where the wrinkled film structure of graphene oxide can be seen, and the good light transmittance of graphene oxide is shown. Polyaniline nanorods are stacked on the surface of graphene oxide and bamboo fibrils, which indicates that polyaniline is successfully polymerized on the surface of graphene oxide and bamboo fibrils through covalent bonds.
[0096] Graphene oxide and polyaniline are bonded by hydrogen bonds, and the amino functional groups of polyaniline are chemically bonded with the hydroxyl and carboxyl groups on the surface of bamboo fibers to form hydrogen bonds. The effective bonding of the three improves the conductivity and electromagnetic wave absorption performance of the composite material. The presence of covalent bonds enhances the compatibility between graphene oxide and polyaniline, thereby further improving the impedance matching problem. Covalent bonds also enable graphene oxide and polyaniline to firmly adsorb bamboo fibers, maximizing the synergistic effect between conductive polymers and bamboo fibers.
[0097] Test Example 4 EDS Analysis
[0098] Figure 6 The chemical element content and element distribution of bamboo fiber and prepared samples are shown. It can be seen from the figure that C and O are the main elements with high content, most of which come from bamboo viscose fiber and bamboo fiber itself. N and S elements mainly come from polyaniline doped with L-camphorsulfonic acid.
[0099] Compared with bamboo viscose fiber and bamboo fiber, the contents of N and S elements in PANI / BVF and PANI / BF increased, and the contents of C and O elements decreased relatively, which indicated that polyaniline was successfully generated and polymerized on bamboo fiber.
[0100] Compared with PANI / BVF and PANI / BF, the C content of GO / PANI / BVF and GO / PANI / BF increased relatively, and the contents of N, O and S elements fluctuated slightly, indicating that the addition of graphene oxide changed the element content of the sample, and the increased C element mainly came from graphene oxide.
[0101] Figure 6(d, l) It can also be seen that graphene oxide / polyaniline particles of different sizes are aggregated on bamboo viscose fibers and bamboo fibrils. The distribution patterns of C, N, O and S elements of GO / PANI / BVF and GO / PANI / BF are observed, and it is found that their distribution is basically the same. The distribution of C, O and S is more concentrated and the content is larger, while the distribution of N element is more dispersed and the content is less, which is consistent with the results of element content determination. The concentrated distribution of S element also indicates that polyaniline particles are successfully polymerized on bamboo viscose fibers and bamboo fibrils.
[0102] Test Example 5 Thermal Stability Analysis
[0103] Figure 7 (a, b) show the TG and DSC curves of bamboo fiber and the prepared samples. All samples showed partial mass loss and endothermic phenomena between about 60℃ and 180℃, which was caused by the evaporation of water in the samples.
[0104] The bamboo viscose fiber and bamboo raw fiber have a large mass loss between about 250℃ and 550℃, which is due to the decomposition of cellulose contained in bamboo viscose fiber and cellulose and hemicellulose contained in bamboo raw fiber. The bamboo viscose fiber is almost completely consumed at 550℃, indicating that the main component of bamboo viscose fiber is cellulose. The bamboo raw fiber still has a slow mass loss after 550℃, which is related to the carbonization of the lignin it contains.
[0105] The mass loss curves and heat absorption and release of the four samples of PANI / BVF, GO / PANI / BVF, PANI / BF and GO / PANI / BF are basically the same. There was obvious mass loss and heat absorption during the period from about 180℃ to 340℃, which was caused by the decomposition of cellulose in bamboo fiber and the decomposition of polyaniline. During the period from 340℃ to 800℃, the four samples continued to have mass loss and heat release. The reasons for this are multiple. First, it was caused by the continuous decomposition of residual cellulose in bamboo fiber and the carbonization of lignin contained in bamboo fiber. Second, it was caused by the continuous decomposition of residual polyaniline. Third, the graphene oxide in GO / PANI / BVF and GO / PANI / BF reached the melting point and began to decompose slowly. At 800℃, the residues of GO / PANI / BVF and GO / PANI / BF were still about 40%, showing better thermal stability compared with other samples.
[0106] Test Example 6 Electromagnetic Performance Analysis
[0107] In order to study the electromagnetic properties of the sample and thus simulate and analyze its electromagnetic wave absorption performance, the applicant tested the electromagnetic parameters of the sample. Figure 8 Multiple electromagnetic parameter data of 6 samples in the range of 2-18 GHz are shown.
[0108] like Figure 8 As shown in (a, b), the ε′ and ε″ values of bamboo viscose fiber and bamboo raw fiber are stable and low, indicating that their dielectric storage and loss capabilities are poor and they do not have good electromagnetic wave absorption performance. The ε′ and ε″ of PANI / BVF, GO / PANI / BVF, PANI / BF and GO / PANI / BF samples generally show a decreasing trend with the increase of frequency, showing a dielectric dispersion phenomenon. This is because when an electromagnetic field is applied to these samples, the random dipoles are adjusted to be parallel to the external field, thereby generating dipole polarization. The ε′ and ε″ values of GO / PANI / BVF and GO / PANI / BF samples are always higher than those of the other four samples, indicating that the introduction of graphene oxide improves the dielectric storage and loss capabilities of the composite material. This also shows that graphene oxide significantly improves the impedance matching of polyaniline, thereby improving the electromagnetic wave absorption performance of the composite material.
[0109] like Figure 8 As shown in (c, d), some peaks appeared in the relative magnetic permeability of the sample, but these peaks were very small and almost close to the values of the paraffin matrix used in the VNA test. The μ' value of the sample fluctuated slightly above the value "1", while the μ" value fluctuated slightly above the value "0", which shows that the magnetic loss of the sample is very limited and can be ignored.
[0110] Generally speaking, dielectric loss capacity and magnetic loss capacity are factors that affect the electromagnetic wave absorption performance of composite materials. Figure 8 As shown in (e, f), the dielectric loss tangent of bamboo viscose fiber and bamboo fibril is close to "0", which still shows that the dielectric loss capacity of bamboo viscose fiber and bamboo fibril is weak. This is related to the electrical insulation of bamboo viscose fiber and bamboo fibril. The dielectric loss tangent of the other four composite materials is significantly higher than that of the corresponding bamboo fiber, which shows that the polymerization of graphene oxide and polyaniline on the surface of bamboo fiber can effectively improve the dielectric loss capacity of the composite material, thereby improving the electromagnetic wave absorption performance of the composite material.
[0111] Although the magnetic loss tangent values of the six samples fluctuate, they are all close to "0", which still indicates that their magnetic loss contribution is small. Therefore, the electromagnetic wave absorption capacity of PANI / BVF, GO / PANI / BVF, PANI / BF and GO / PANI / BF mainly comes from their dielectric loss capacity.
[0112] Test Example 7 Analysis of electromagnetic wave absorption performance
[0113] The electromagnetic wave absorption performance of the sample is simulated and calculated based on the transmission line theory. Fig. 9 The RL value curves of bamboo viscose fiber, PANI / BVF, GO / PANI / BVF, bamboo fiber, PANI / BF and GO / PANI / BF are shown. Fig. 9 (a, b) It can be seen that the RLmin of bamboo viscose fiber and bamboo fiber is only about -1dB, the thickness is 4.5mm, and the frequency is around 14.5GHz. It shows weak electromagnetic wave absorption performance, which is consistent with the results of the electromagnetic performance analysis part. The electrical insulation directly leads to the weak electromagnetic wave absorption ability of bamboo fiber.
[0114] The RLmin of PANI / BVF is -22.74dB, the thickness is 2.5mm, the frequency is 14.48GHz; the effective absorption bandwidth is 9.12GHz, the frequency range is 8.88-18GHz, and the thickness is 3mm.
[0115] The RLmin of PANI / BF is -29.58dB, the thickness is 5mm, the frequency is 7.28GHz; the effective absorption bandwidth is 9.44GHz, the frequency range is 7.76-17.2GHz, and the thickness is 3.5mm.
[0116] The RLmin of GO / PANI / BVF is -30.23dB, the thickness is 2.5mm, the frequency is 11.04GHz; the effective absorption bandwidth is 6.88GHz, the frequency range is 11.12-18GHz, and the thickness is 2mm.
[0117] The RLmin of GO / PANI / BF is -37.91dB, the thickness is 2mm, the frequency is 14.08GHz; the effective absorption bandwidth is 6.52GHz, the frequency range is 11.84-17.36GHz, and the thickness is 2mm.
[0118] From the simulation results, GO / PANI / BF showed the best electromagnetic wave absorption performance and the thinnest material thickness, followed by GO / PANI / BVF; PANI / BF had the best effective absorption bandwidth, followed by PANI / BVF. By changing the thickness of the four composite materials, effective absorption of electromagnetic waves in the frequency range of 5-18GHz can be achieved.
[0119] Therefore, the introduction of graphene oxide and polyaniline effectively improves the electromagnetic wave absorption performance of bamboo fiber. The combination of graphene oxide and polyaniline forms a complete and efficient conductive network, while the wave permeability of bamboo fiber prolongs the transmission path of electromagnetic waves in the conductive network and increases the refraction of electromagnetic waves; the joint cooperation between them is an indispensable condition for the composite material to have good electromagnetic wave absorption performance.
[0120] The main reason why the RLmin of GO / PANI / BF is better than that of GO / PANI / BVF is that the raw bamboo fiber is prepared by physical methods, and its tissue composition still retains some of the porous and multi-tube characteristics of bamboo, providing more cavity structures for the reflection and multiple refraction of electromagnetic waves, while the bamboo viscose fiber is prepared by chemical methods, during which a large number of pores and cavities are removed, resulting in the reflection and refraction ability of GO / PANI / BVF being inferior to GO / PANI / BF, and therefore slightly inferior in electromagnetic wave absorption performance.
[0121] Test Example 9 Electromagnetic Radiation Test of Electromagnetic Wave Absorption Cover
[0122] Bamboo viscose fiber, bamboo fibril, GO / PANI / BVF and GO / PANI / BF were mixed with epoxy resin in a mass ratio of 3:7, and then benzyl alcohol was used as a curing agent. The mass ratio of benzyl alcohol to epoxy resin was 3:7. The mixture was stirred evenly, and then poured into a customized mold in the laboratory and allowed to stand for 7 days. After it was completely solidified, it was demolded to obtain the electromagnetic wave absorption cover of the corresponding sample.
[0123] At the same time, an epoxy resin electromagnetic wave absorption cover without adding samples was prepared as a control group. The prepared electromagnetic wave absorption cover was tested by an electromagnetic radiation tester. The experimental results are as follows Fig.10 shown.
[0124] pass Fig.10 (ac) It can be seen that the electric field peak value of the epoxy resin electromagnetic wave absorption cover without adding samples is 206V / m, and the magnetic field peak value is 0.14uT; the electric field peak value of the bamboo viscose fiber electromagnetic wave absorption cover is 226V / m, and the magnetic field peak value is 0.18uT; the electric field peak value of the bamboo fiber electromagnetic wave absorption cover is 193V / m, and the magnetic field peak value is 0.17uT. The test results of the three electromagnetic wave absorption covers are similar, and the absorption effect on the electromagnetic field is not obvious, which proves that their electromagnetic wave absorption performance is weak, which is consistent with the simulation results of the electromagnetic wave absorption performance part.
[0125] pass Fig.10 (d, e) The test results of GO / PANI / BVF and GO / PANI / BF electromagnetic wave absorption covers show that the electric field peak value of GO / PANI / BVF is 103V / m, and the magnetic field peak value is 0.09uT; the electric field peak value of GO / PANI / BF is 85V / m, and the magnetic field peak value is 0.06uT. Compared with the first three items, it can be clearly seen that the bamboo fiber-based electromagnetic wave absorption material obtained by the present invention has a significant absorption effect on electromagnetic waves under actual use. Therefore, the bamboo fiber-based electromagnetic wave absorption material obtained by the present invention is fully expected to be applied to products and directions such as radiation protection clothing, electromagnetic shielding car clothing, electromagnetic wave absorption blankets and darkroom wall materials.
[0126] In summary, the present invention successfully prepared bamboo fiber-based electromagnetic wave absorbing materials (GO / PANI / BVF and GO / PANI / BF).
[0127] (1) The samples were characterized by FT-IR and XRD. The test results showed that the groups and bonds of bamboo viscose fiber were more active than those of bamboo fiber, and the crystal structure of bamboo fiber belonged to cellulose type II. Graphene oxide combined with L-camphorsulfonic acid-doped polyaniline completely covered the functional group characteristic peaks and crystal diffraction peaks of bamboo fiber.
[0128] (2) The thermal stability of the samples was characterized by TG-DSC. From the analysis of sample mass loss rate and residual amount, it was found that the thermal stability of bamboo fiber-based electromagnetic wave absorbing materials was better than that of original bamboo fiber materials.
[0129] (3) The electromagnetic wave absorption performance of the sample was simulated and calculated through the test data of electromagnetic parameters. The RLmin of GO / PANI / BVF is -30.23dB, the thickness is 2.5mm, the frequency is 11.04GHz; the effective absorption bandwidth is 6.88GHz, the frequency range is 11.12-18GHz, and the thickness is 2mm. The RLmin of GO / PANI / BF is -37.91dB, the thickness is 2mm, the frequency is 14.08GHz; the effective absorption bandwidth is 6.52GHz, the frequency range is 11.84-17.36GHz, and the thickness is 2mm.
[0130] Its excellent performance is mainly attributed to the dielectric loss capacity of the graphene oxide / polyaniline layer and the dipole caused by multiple interfaces, as well as the wave transmittance of bamboo fiber, which provides space for multiple reflections and scattering of electromagnetic waves, extending the propagation path of electromagnetic waves.
[0131] (4) Through the test of bamboo fiber-based electromagnetic wave absorption cover, it can absorb the electromagnetic waves generated by mobile phone signal transmission well and reduce the electric field strength and magnetic field strength by about 50%.
[0132] The bamboo fiber-based electromagnetic wave absorbing material obtained by the present invention has the advantages of simple preparation, light texture, thin thickness, wide effective absorption frequency band, strong electromagnetic wave absorption capacity, etc., and has the original characteristics of the two bamboo fiber materials such as UV protection and softness. It not only meets the selection criteria of electromagnetic wave absorbing materials "thin, wide, light, and strong", but also takes into account the original characteristics of bamboo fiber materials. Therefore, the present invention is fully expected to become a new choice of inexpensive, environmentally friendly, and efficient electromagnetic wave absorbing materials, and also broadens the application direction of bamboo fiber materials.
[0133] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A bamboo fiber-based electromagnetic wave absorbing material, characterized in that: The raw materials include: aniline, bamboo fiber and graphene oxide; the mass ratio of aniline, bamboo fiber and graphene oxide is 3.0-3.1:1-6:0-0.15, and the mass of graphene oxide is not 0.
2. The bamboo fiber-based electromagnetic wave absorbing material according to claim 1, characterized in that: In situ polymerization of aniline on the surfaces of bamboo fiber and graphene oxide.
3. The bamboo fiber-based electromagnetic wave absorbing material according to claim 1, characterized in that: The bamboo fiber-based electromagnetic wave absorbing material has an RLmin of ≤-30.23 dB and an effective absorption bandwidth of ≤6.88 GHz.
4. A method for preparing the bamboo fiber-based electromagnetic wave absorbing material according to any one of claims 1 to 3, characterized in that: The steps include: (1) mixing aniline and L-camphorsulfonic acid solution, adding bamboo fiber and graphene oxide aqueous dispersion, and ultrasonically dispersing to obtain a first material; (2) dissolving the initiator in a L-camphorsulfonic acid solution to obtain a second material; (3) Place the first material in an ice bath environment, maintain the temperature of the first material at 5±1°C, then dropwise add the second material thereto, stir, wash, filter, and dry.
5. The method for preparing the bamboo fiber-based electromagnetic wave absorbing material according to claim 4, characterized in that: In step (1), the mass concentration of the graphene oxide aqueous dispersion is 2.8-3.2 g / L; Preferably, in step (1), the concentration of the L-camphorsulfonic acid solution is 0.25-1.50 mol / L, and the volume ratio of aniline to the L-camphorsulfonic acid solution is 2.8-3.2:27-33.
6. The method for preparing the bamboo fiber-based electromagnetic wave absorbing material according to claim 4, characterized in that: The concentration of the L-camphorsulfonic acid solution used in step (1) is the same as that of the L-camphorsulfonic acid solution used in step (2); Preferably, in the second material, the concentration of the initiator is the same as the concentration of L-camphorsulfonic acid.
7. The method for preparing the bamboo fiber-based electromagnetic wave absorbing material according to claim 4, characterized in that: In step (2), the initiator is a persulfate, preferably ammonium persulfate; Preferably, in the second material, the initiator concentration is 0.25-1.50 mol / L.
8. A bamboo fiber-based electromagnetic wave absorption cover, characterized in that: It is made of the bamboo fiber-based electromagnetic wave absorbing material according to any one of claims 1 to 3; the electric field peak value of the bamboo fiber-based electromagnetic wave absorbing cover is ≤103V / m, and the magnetic field peak value is ≤0.09uT.
9. The bamboo fiber-based electromagnetic wave absorption cover according to claim 8, characterized in that: The raw materials include: the bamboo fiber-based electromagnetic wave absorbing material, epoxy resin and curing agent. The mass ratio of the bamboo fiber-based electromagnetic wave absorbing material to the epoxy resin is 2.5-3.5:6.5-7.5, and the mass ratio of the curing agent to the epoxy resin is 2.5-3.5:6.5-7.
5.
10. A bamboo fiber-based electromagnetic wave absorption cover as claimed in claim 8 or 9, characterized in that: The bamboo fiber-based electromagnetic wave absorbing material according to any one of claims 1 to 3 is mixed with epoxy resin, a curing agent is added, the mixture is evenly mixed, and the mixture is injected into a mold and allowed to stand.
Citation Information
Cited By
Cellulose-based aerogel with dynamic adjustable electromagnetic wave absorption performance and preparation method thereof
CN121021909A