Colorless and transparent poly (urethane-urea) elastomer based on mismatched supramolecular interaction as well as preparation method and application of colorless and transparent poly (urethane-urea) elastomer
By introducing aliphatic mixed chain extenders into thermoplastic poly(urethane-urea), mismatched supramolecular effects are formed, and the problems of elastomer materials being easily discolored and transparent under ultraviolet light are solved, and colorless transparency and high mechanical properties are achieved The combination of performance significantly improves the anti-aging properties of the material.
Patent Information
- Application Number
- CN202411100378.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-27
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-09-27
AI Technical Summary
The problems of existing elastomer materials that tend to discolor and reduce transparency under ultraviolet irradiation affect their mechanical properties and application value.
Using the preparation method of colorless transparent poly(urethane-urea) materials based on mismatch supramolecular action, the aliphatic mixed chain extender adipic acid dihydrazide and 1,4 are introduced into the thermoplastic poly(urethane-urea). -Butanediamine, forming a mismatched supramolecular action, improving the mechanical toughness and anti-aging properties of the material.
It has achieved colorless and transparent state under ultraviolet aging conditions, with excellent anti-aging properties and high mechanical strength, reducing the risk of material discoloration under ultraviolet light and improving the practical application value of the material.
Smart Images

Figure HDA0005064213410000011 
Figure HDA0005064213410000012 
Figure HDA0005064213410000021
Abstract
Description
Technical Field
[0001] This invention relates to the field of high-performance polymer material synthesis technology, specifically to a colorless and transparent poly(urethane-urea) elastomer based on mismatch supramolecular interactions, its preparation method, and its applications. Background Technology
[0002] The information disclosed in this background section is intended only to enhance understanding of the overall background of the invention and is not necessarily to be construed as an admission or in any way implying that such information constitutes prior art known to those skilled in the art.
[0003] Elastomers are widely used polymer materials in industries such as industrial applications, lubricants, molds, tires, vehicles, and prosthetics due to their unique ability to return to their original shape after deformation. With continuous technological advancements, the elastomer market is showing strong growth momentum.
[0004] The widespread application and market prospects of elastomers stem from their unique combination of superior mechanical properties, recyclability, and durability. To further improve the performance of elastomers, molecular design methods offer an effective approach by introducing rigid aromatic structures into the polymer matrix, significantly enhancing material strength and extending supramolecular interactions. However, aromatic structures also present significant challenges, particularly regarding discoloration and decreased transparency under ultraviolet irradiation. For example, Chinese patent document CN115716901A discloses a method and its application for synergistic toughening of thermoplastic poly(urethane-urea) using rigid-flexible supramolecular fragments. This invention adds two mixed chain extenders capable of forming rigid and flexible supramolecular interactions after the prepolymer formation stage during the synthesis of thermoplastic poly(urethane-urea) materials. This hybridizes the rigid and flexible supramolecular interactions within the polymer chain, enabling the material to effectively dissipate the energy applied by external forces when subjected to external stress, thereby improving the material's toughness. However, due to the introduction of aromatic structures, the material itself is colored and prone to discoloration and decreased transparency under ultraviolet irradiation. Chinese patent document CN115010896A discloses a method for preparing a thermoplastic elastomer with excellent resilience and high strength, comprising the following steps: A) placing at least two soft segment monomers in a solvent and then adding a hard segment monomer, reacting under the action of a catalyst to obtain an initial reactant; B) reacting a chain extender with the initial reactant to obtain a thermoplastic elastomer. The thermoplastic elastomer provided by this invention possesses high strength and high modulus through multiple hydrogen bonds in the hard segment monomers, and excellent toughness and high resilience through the thermodynamic incompatibility of the soft segment monomers. However, the elongation at break of this invention is too low, and it still involves the use of benzene ring-containing materials.
[0005] Therefore, how to maintain the high mechanical properties of elastomers while solving the problems of easy discoloration and decreased transparency of materials under ultraviolet irradiation has become an important topic in the research of elastomer materials. Summary of the Invention
[0006] To address the shortcomings of existing technologies, this invention provides a colorless and transparent poly(urethane-urea) elastomer based on mismatch supramolecular interactions, its preparation method, and its applications. This invention uses industrially common thermoplastic poly(urethane-urea) as a model system, selecting an aliphatic molecular structure to ensure its stable colorless and transparent properties, and introducing mismatch supramolecular interactions to significantly improve its mechanical toughness. The preparation method of this invention is simple, low-cost, and capable of large-scale production. The thermoplastic poly(urethane-urea) obtained by this invention can stably maintain its colorless and transparent state under ultraviolet aging conditions, exhibiting excellent anti-aging properties, while also possessing high strength and high toughness mechanical properties, making it highly applicable in practice.
[0007] This invention is achieved through the following technical solution:
[0008] In a first aspect, the present invention provides a method for preparing a colorless and transparent poly(urethane-urea) elastomer based on mismatch supramolecular interactions, comprising the steps of:
[0009] (1) In a solvent and under the action of a catalyst, diisocyanate and oligomeric polyol react to form a prepolymer;
[0010] (2) The organic solution of aliphatic mixed chain extender is mixed with the prepolymer, reacted, and then degassed and dried to obtain a colorless and transparent poly(urethane-urea) elastomer based on mismatch supramolecular action;
[0011] The aliphatic mixed chain extender is a combination of adipate dihydrazide (ADH) and 1,4-butanediamine (BDA).
[0012] According to a preferred embodiment of the present invention, in step (1), the solvent is one or a combination of two or more of N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide or N-methylpyrrolidone; the mass ratio of diisocyanate to solvent is 1:5-20.
[0013] According to a preferred embodiment of the present invention, in step (1), the catalyst is one or a combination of two or more of dibutyltin dilaurate (DBTDL), stannous octoate or triethylenediamine; the molar ratio of the catalyst to the diisocyanate is 0.01-0.05:1, preferably 0.025:1.
[0014] According to a preferred embodiment of the present invention, in step (1), the diisocyanate is 4,4'-dicyclohexylmethane diisocyanate (HMDI) or isophorone diisocyanate (IPDI).
[0015] According to a preferred embodiment of the present invention, in step (1), the oligomeric polyol is one or a combination of two or more of polytetrahydrofuran, polydimethylsiloxane or polycaprolactone.
[0016] According to a preferred embodiment of the present invention, in step (1), the molar ratio of diisocyanate to oligomeric polyol is 1:0.2-1, preferably 1:0.5.
[0017] According to a preferred embodiment of the present invention, in step (1), the reaction temperature of the diisocyanate and the oligomeric polyol is 60-100°C, the reaction time is 1-3 h, and the reaction is carried out under stirring conditions.
[0018] According to a preferred embodiment of the present invention, in step (2), the molar ratio of adipic acid dihydrazide (ADH) and 1,4-butanediamine (BDA) in the aliphatic mixed chain extender is 0.5-2:0.5-2, preferably 1:1.
[0019] According to a preferred embodiment of the present invention, in step (2), the mass concentration of the organic solution of the aliphatic mixed chain extender is 1-5%; the solvent used in the organic solution of the aliphatic mixed chain extender is one or a combination of two or more of N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide or N-methylpyrrolidone.
[0020] According to a preferred embodiment of the present invention, in step (2), the molar amount of the aliphatic mixed chain extender is 40-60% of the molar amount of the diisocyanate, preferably 50%.
[0021] According to a preferred embodiment of the present invention, in step (2), the reaction temperature is room temperature, the reaction time is 2-7 hours, and the reaction is carried out under stirring conditions.
[0022] According to a preferred embodiment of the present invention, in step (2), the degassing method is vacuum degassing; the drying conditions are: drying at 70-90℃ for 10-14h, and then vacuum drying at 90-110℃ for 6-10h.
[0023] In a second aspect, the present invention provides a colorless and transparent poly(urethane-urea) elastomer based on mismatch supramolecular interaction, which is prepared by the above method.
[0024] In a third aspect, the present invention provides the application of a colorless and transparent poly(urethane-urea) elastomer based on mismatch supramolecular interaction in the field of UV-resistant, high mechanical strength, damage-resistant, recyclable transparent materials.
[0025] The technical features and beneficial effects of this invention are as follows:
[0026] 1) The method of the present invention is simple and easy to implement, the raw materials are readily available, the cost is low, and the requirements for reaction conditions and equipment are not high, enabling large-scale preparation in a 20L reactor.
[0027] 2) This invention, based on the existing production process of thermoplastic poly(urethane-urea), adds a new aliphatic mixed chain extender, solving the problem of material discoloration and decreased transparency under ultraviolet irradiation caused by the introduction of aromatic structures. It achieves colorless, transparent, and anti-aging thermoplastic poly(urethane-urea), maintaining a stable colorless and transparent state under ultraviolet aging conditions, exhibiting excellent anti-aging properties. Simultaneously, it achieves reinforcement and toughening of colorless and transparent poly(urethane-urea). This invention uses a mixed chain extender with mismatched hydrazine and amino groups, which can form mismatched supramolecular interactions in the molecular structure of the elastomer, i.e., mismatched supramolecular interactions. The stronger binding force and more hydrogen bonds between the hydrazine and amino groups make it stand out in different mismatched combinations, exhibiting the best mechanical properties. The colorless, transparent, and anti-aging properties are due to the absence of benzene ring structures in the elastomer structure of this invention, making it less prone to absorbing ultraviolet light and producing discoloration groups. The addition of aromatic structures increases the material's ability to absorb ultraviolet (UV) light, due to the interaction between ultraviolet photons and the π electron cloud, promoting electron transitions to higher energy levels. This interaction not only alters the material's color, turning it yellow or brown after prolonged use, but also raises concerns about material safety and transparency due to changes in chemical composition and microstructure caused by ultraviolet radiation. Therefore, benzene ring-free elastomers can significantly reduce these concerns.
[0028] 3) Only specific types of chain extenders can achieve the excellent effects of this invention. If the type of chain extender is unsuitable, the ratio of the two chain extenders is unsuitable, or the amount of chain extender is unsuitable, the performance of the resulting elastomer will be affected.
[0029] 4) The strategy of improving the mechanical properties of colorless and transparent poly(urethane-urea) elastomers through mismatched supramolecular effects provided by this invention is not limited to thermoplastic poly(urethane-urea) systems, but also has potential application value for toughening other colorless and transparent polymer materials. Attached Figure Description
[0030] Figure 1 This is a comparison of the mechanical properties and surface morphology after long-term ultraviolet irradiation of benzene ring-containing and benzene ring-free elastomers reported in the current literature.
[0031] Figure 2 The bar chart shows the toughness data of three elastomers with mismatched hydrazine and amino groups (Example 1), mismatched hydrazine and hydroxyl groups (Comparative Example 4), and mismatched amino and hydroxyl groups (Comparative Example 5).
[0032] Figure 3 This is a bar chart showing the toughness data of five elastomers: Example 1, Comparative Example 1, Comparative Example 2, Example 2, and Example 3.
[0033] Figure 4The hydrazine- and amino mismatched benzene ring-free elastomer SPU-HA prepared in Example 1 exhibits a toughness >300 MJ / m² reported in current literature. -3 Comparison of mechanical properties of benzene ring-free elastomers.
[0034] Figure 5 This is a bar chart showing the change in transparency of the benzene-ring-containing SPU-DA prepared in Comparative Example 3 and the benzene-ring-free SPU-HA prepared in Example 1 after aging for different numbers of days. Detailed Implementation
[0035] The present invention will be further illustrated below with reference to specific embodiments. It should be understood that these embodiments are for illustrative purposes only and are not intended to limit the scope of the invention. Experimental methods in the following embodiments, unless otherwise specified, are generally performed under conventional conditions or as recommended by the manufacturer.
[0036] It should be noted that the terminology used herein is for the purpose of describing particular implementations only and is not intended to limit the exemplary implementations according to this disclosure.
[0037] The present invention will be further described in detail below with reference to specific embodiments. It should be noted that the specific embodiments are explanations of the present invention and not limitations thereof.
[0038] Terminology Explanation:
[0039] PTMEG 2000: Polytetrahydrofuran (molecular weight 2000), purchased from Aladdin Biochemical Technology Co., Ltd.;
[0040] HMDI: 4,4'-Dicyclohexylmethane diisocyanate;
[0041] DBTDL: Dibutyltin dilaurate, used as a catalyst;
[0042] DMF: N,N-dimethylformamide;
[0043] BDA: 1,4-Butanediamine;
[0044] ADH: adipic acid dihydrazide;
[0045] DABA: 4,4'-diaminobenzilide;
[0046] BDO: 1,4-Butanediol;
[0047] Room temperature: has a meaning known in this technical field, generally referring to 25±2℃;
[0048] Mechanical property testing method: INSTRON 3344 electronic universal testing machine. The specimens were cut into rectangular shapes with dimensions of 25mm x 5mm x 0.6mm. Testing was conducted at room temperature with a tensile rate of 50mm / min. Each specimen was measured at least five times, and the average value was taken.
[0049] UV aging test method: QUV / spray UV aging tester, light wavelength: 340nm, light intensity: 0.77W / m 2 The cyclic process conditions were: irradiation with ultraviolet light at 60℃ for 8 hours, followed by condensation at 50℃ for 4 hours.
[0050] Fracture strength: The ratio of the tensile force required to break a material to the cross-sectional area at which the material breaks, i.e., stress;
[0051] Elongation at break: The ratio of the length of a material after being stretched to its length before being stretched when it breaks under external force is called elongation at break, and it is expressed as a percentage.
[0052] Toughness: refers to a material's ability to absorb energy during plastic deformation and fracture.
[0053] Dissipated energy: The portion of energy lost within a material that cannot be used to perform useful work.
[0054] Example 1: Preparation of an aliphatic colorless and transparent thermoplastic poly(urethane-urea) containing amino and hydrazine mismatched chain extenders, with an ADH:BDA molar ratio of 1:1 as the mixed chain extender.
[0055] In a 250 mL round-bottom flask, 2.62 g (0.01 mol) HMDI, 10 g (0.005 mol) PTMEG2000, 150 μL (0.00025 mol) DBTDL, and 22 g anhydrous DMF were added. The mixture was heated in an oil bath at 80 °C for 2 h with magnetic stirring. 0.435 g (0.0025 mol) ADH and 0.22 g (0.0025 mol) BDA were dissolved in 20 g anhydrous DMF. After the reaction was complete, heating was stopped, and the system was allowed to cool to room temperature. Then, the mixed DMF solution of ADH and BDA was added, and the reaction was carried out with magnetic stirring for 5 h. The mixture was then poured into a silicone mold for vacuum degassing. After degassing until no more bubbles were generated, the mold was dried in an 80 °C oven for 12 h, and then further dried in a 100 °C vacuum oven for 8 h to remove residual DMF. The target aliphatic transparent thermoplastic poly(urethane-urea) elastomer was obtained after demolding. It is denoted as SPU-HA.
[0056] Comparative Example 1: Preparation of an aliphatic colorless and transparent thermoplastic poly(urethane-urea) containing only amino chain extenders.
[0057] In a 250 mL round-bottom flask, add 2.62 g HMDI, 10 g PTMEG2000, 150 μL DBTDL, and 22 g anhydrous DMF. Heat in an oil bath at 80 °C for 2 h with magnetic stirring. Dissolve 0.44 g (0.005 mol) BDA in 20 g anhydrous DMF. After the reaction is complete, turn off the heating and allow the system to cool to room temperature. Then add the BDA DMF solution and react with magnetic stirring for 5 h. Pour the mixture into a silicone mold for vacuum degassing. After degassing until no more bubbles are generated, dry in an 80 °C oven for 12 h, and then place in a 100 °C vacuum oven for 8 h to further remove residual DMF. Demold to obtain the target aliphatic transparent thermoplastic poly(urethane-urea) elastomer, denoted as SPU-A.
[0058] Comparative Example 2: Preparation of aliphatic colorless and transparent thermoplastic poly(urethane-urea) containing only hydrazine-based chain extenders
[0059] In a 250 mL round-bottom flask, add 2.62 g HMDI, 10 g PTMEG2000, 150 μL DBTDL, and 22 g anhydrous DMF. Heat in an oil bath at 80 °C for 2 h with magnetic stirring. Dissolve 0.87 g (0.005 mol) ADH in 20 g anhydrous DMF. After the reaction is complete, turn off the heating and allow the system to cool to room temperature. Then add the ADH-DMF solution and react with magnetic stirring for 5 h. Pour the mixture into a silicone mold for vacuum degassing. After degassing until no more bubbles are generated, dry in an 80 °C oven for 12 h, and then place in a 100 °C vacuum oven for 8 h to further remove residual DMF. Demold to obtain the target aliphatic transparent thermoplastic poly(urethane-urea) elastomer, denoted as SPU-H.
[0060] Comparative Example 3: Preparation of a transparent thermoplastic poly(urethane-urea) containing benzene rings
[0061] In a 250 mL round-bottom flask, add 2.62 g HMDI, 10 g PTMEG2000, 150 μL DBTDL, and 22 g anhydrous DMF. Heat in an oil bath at 80 °C for 2 h with magnetic stirring. Dissolve 0.435 g (0.0025 mol) ADH and 0.57 g (0.0025 mol) DABA in 20 g anhydrous DMF. After the reaction is complete, turn off the heating and allow the system to cool to room temperature. Then add the mixed DMF solution of ADH and DABA and react with magnetic stirring for 5 h. Pour into a silicone mold for vacuum degassing. After degassing until no more bubbles are generated, dry in an 80 °C oven for 12 h, and then place in a 100 °C vacuum oven for 8 h to further remove residual DMF. Demold to obtain the target aliphatic transparent thermoplastic poly(urethane-urea) elastomer, denoted as SPU-DA.
[0062] Comparative Example 4: Preparation of an aliphatic colorless and transparent thermoplastic poly(urethane-urea) with a mixed chain extender containing hydrazine and hydroxyl mismatched chain extenders and an ADH:BDO molar ratio of 1:1.
[0063] In a 250 mL round-bottom flask, add 2.62 g HMDI, 10 g PTMEG2000, 150 μL DBTDL, and 22 g anhydrous DMF. Heat in an oil bath at 80 °C for 2 h with magnetic stirring. Dissolve 0.435 g (0.0025 mol) ADH and 0.23 g (0.0025 mol) BDO in 20 g anhydrous DMF. After the reaction is complete, turn off the heating and allow the system to cool to room temperature. Then add the mixed DMF solution of ADH and BDO and react with magnetic stirring for 5 h. Pour into a silicone mold for vacuum degassing. After degassing until no more bubbles are generated, dry in an 80 °C oven for 12 h, and then place in a 100 °C vacuum oven for 8 h to further remove residual DMF. Demold to obtain the target aliphatic transparent thermoplastic poly(urethane-urea) elastomer, denoted as SPU-HO.
[0064] Comparative Example 5: Preparation of an aliphatic colorless and transparent thermoplastic poly(urethane-urea) containing amino and hydroxyl mismatched chain extenders, with a BDA:BDO molar ratio of 1:1 as the mixed chain extender.
[0065] In a 250 mL round-bottom flask, add 2.62 g HMDI, 10 g PTMEG2000, 150 μL DBTDL, and 22 g anhydrous DMF. Heat in an oil bath at 80 °C for 2 h with magnetic stirring. Dissolve 0.22 g (0.0025 mol) BDA and 0.23 g (0.0025 mol) BDO in 20 g anhydrous DMF. After the reaction is complete, turn off the heating and allow the system to cool to room temperature. Then add the mixed DMF solution of BDA and BDO and react with magnetic stirring for 5 h. Pour into a silicone mold for vacuum degassing. After degassing until no more bubbles are generated, dry in an 80 °C oven for 12 h, and then place in a 100 °C vacuum oven for 8 h to further remove residual DMF. Demold to obtain the target aliphatic transparent thermoplastic poly(urethane-urea) elastomer, denoted as SPU-AO.
[0066] Example 2: Preparation of an aliphatic colorless and transparent thermoplastic poly(urethane-urea) containing amino and hydrazine mismatched chain extenders, with an ADH:BDA molar ratio of 2:1 as the mixed chain extender.
[0067] In a 250 mL round-bottom flask, 2.62 g (0.01 mol) HMDI, 10 g (0.005 mol) PTMEG2000, 150 μL (0.00025 mol) DBTDL, and 22 g anhydrous DMF were added. The mixture was heated in an oil bath at 80 °C for 2 h with magnetic stirring. 0.581 g (0.0033 mol) ADH and 0.15 g (0.0017 mol) BDA were dissolved in 20 g anhydrous DMF. After the reaction was complete, heating was stopped, and the system was allowed to cool to room temperature. Then, the mixed DMF solution of ADH and BDA was added, and the reaction was carried out with magnetic stirring for 5 h. The mixture was then poured into a silicone mold for vacuum degassing. After degassing until no more bubbles were generated, the mold was dried in an 80 °C oven for 12 h, and then further dried in a 100 °C vacuum oven for 8 h to remove residual DMF. Demolding yielded the target aliphatic transparent thermoplastic poly(urethane-urea) elastomer. It is designated as SPU-H2A.
[0068] Example 3: Preparation of an aliphatic colorless and transparent thermoplastic poly(urethane-urea) containing amino and hydrazine mismatched chain extenders, with an ADH:BDA molar ratio of 1:2 as the mixed chain extender.
[0069] In a 250 mL round-bottom flask, 2.62 g (0.01 mol) HMDI, 10 g (0.005 mol) PTMEG2000, 150 μL (0.00025 mol) DBTDL, and 22 g anhydrous DMF were added. The mixture was heated in an oil bath at 80 °C for 2 h with magnetic stirring. 0.29 g (0.0017 mol) ADH and 0.29 g (0.0033 mol) BDA were dissolved in 20 g anhydrous DMF. After the reaction was complete, the heating was turned off, and the system was allowed to cool to room temperature. Then, the mixed DMF solution of ADH and BDA was added, and the reaction was carried out with magnetic stirring for 5 h. The mixture was then poured into a silicone mold for vacuum degassing. After degassing until no more bubbles were generated, the mold was dried in an 80 °C oven for 12 h, and then further dried in a 100 °C vacuum oven for 8 h to remove residual DMF. The target aliphatic transparent thermoplastic poly(urethane-urea) elastomer was obtained after demolding. It is designated as SPU-HA2.
[0070] Test case
[0071] Figure 1 This comparison examines the mechanical properties and surface morphology after long-term UV irradiation of benzene ring-containing and benzene ring-free elastomers as reported in current literature. As shown in the figure, although the mechanical properties of benzene ring-containing materials are significantly better than those of benzene ring-free elastomers, with a toughness value even twice that of the benzene ring-free elastomers, they darken in color and may even become opaque after long-term UV exposure, indicating degradation and jeopardizing safety. In contrast, benzene ring-free elastomers do not undergo color changes under UV irradiation and their use remains unaffected.
[0072] Figure 2This is a bar chart showing the toughness data of three elastomers with hydrazine and amino mismatches (SPU-HA, Example 1), hydrazine and hydroxyl mismatches (SPU-HO, Comparative Example 4), and amino and hydroxyl mismatches (SPU-AO, Comparative Example 5). As shown in the chart, the elastomer of Example 1 has a toughness of 1086.9 MJ / m. -3 The elastomer in Comparative Example 4 had a toughness of 641.6 MJ / m. -3 The toughness of the elastomer in Comparative Example 5 was 370.7 MJ / m. -3 Therefore, elastomers containing hydrazine and amino mismatches exhibit the best mechanical properties, which may be due to the stronger binding force between the two, resulting in lower binding energy, and the presence of more and stronger hydrogen bonds.
[0073] Figure 3 This is a bar chart showing the toughness data of five elastomers: Example 1 (SPU-HA), Comparative Example 1 (SPU-A), Comparative Example 2 (SPU-H), Example 2 (SPU-H2A), and Example 3 (SPU-HA2). As shown in the chart, the toughness of the elastomer in Example 1 is 1086.9 MJ / m. -3 The elastomer in Comparative Example 1 had a toughness of 179.4 MJ / m. -3 The toughness of the elastomer in Comparative Example 2 was 364.5 MJ / m. -3 In Example 2, the elastomer toughness was 550.1 MJ / m. -3 The elastomer in Example 3 has a toughness of 438.7 MJ / m. -3 Therefore, elastomers with a 1:1 mismatch ratio of hydrazine and amino groups exhibit the best mechanical properties due to the presence of more mismatch supramolecular interactions.
[0074] Figure 4 The hydrazine- and amino mismatched benzene ring-free elastomer SPU-HA prepared in Example 1 exhibits a toughness >300 MJ / m² reported in current literature. -3 A comparison of the mechanical properties of benzene ring-free elastomers is shown in the figure. As can be seen from the figure, SPU-HA achieves a balance between high mechanical properties and colorless transparency due to the mismatch between the hydrazine and amino groups.
[0075] Figure 5 The benzene-ring-containing SPU-DA prepared in Comparative Example 3 and the benzene-ring-free SPU-HA prepared in Example 1 were subjected to aging (QUV / spray ultraviolet aging tester, light wavelength: 340nm, light intensity: 0.77W / m). 2 The cyclic process conditions were: 8 hours of UV irradiation at 60℃ followed by 4 hours of condensation at 50℃. The resulting bar chart shows the changes in transparency after different number of days. The chart indicates that the transparency of SPU-DA, containing a benzene ring, decreased sharply, while the transparency of SPU-HA remained stable.
Claims
1. A method for preparing a colorless and transparent poly(urethane-urea) elastomer based on mismatch supramolecular action, comprising the steps of: (1) In a solvent and under the action of a catalyst, diisocyanate and oligomer polyol react to form a prepolymer; (2) mixing an organic solution of an aliphatic mixed chain extender with a prepolymer, reacting, degassing, and drying to obtain a colorless and transparent poly(urethane-urea) elastomer based on mismatch supramolecular action; The aliphatic mixed chain extender is a combination of adipic acid dihydrazide (ADH) and 1,4-butanediamine (BDA).
2. The method for preparing a colorless and transparent poly(urethane-urea) elastomer based on mismatch supramolecular action according to claim 1, wherein step (1) comprises one or more of the following conditions: i. The solvent is one or a combination of two or more of N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide or N-methylpyrrolidone; the mass ratio of diisocyanate to solvent is 1:5-20; ii. The catalyst is one or a combination of two or more of dibutyltin dilaurate (DBTDL), stannous octoate or triethylenediamine; the molar ratio of the catalyst to the diisocyanate is 0.01-0.05:1, preferably 0.025:
1.
3. The method for preparing a colorless and transparent poly(urethane-urea) elastomer based on mismatch supramolecular action according to claim 1, wherein step (1) comprises one or more of the following conditions: i. The diisocyanate is 4,4'-dicyclohexylmethane diisocyanate (HMDI) or isophorone diisocyanate (IPDI; ii. The oligomer polyol is one or a combination of two or more of polytetrahydrofuran, polydimethylsiloxane or polycaprolactone; iii. The molar ratio of diisocyanate to oligomer polyol is 1:0.2-1, preferably 1:0.
5.
4. According to the method for preparing a colorless and transparent poly(urethane-urea) elastomer based on mismatch supramolecular action according to claim 1, in step (1), the reaction temperature of diisocyanate and oligomer polyol is 60-100° C., the reaction time is 1-3 h, and the reaction is carried out under stirring conditions.
5. According to the method for preparing a colorless and transparent poly(urethane-urea) elastomer based on mismatch supramolecular action according to claim 1, in step (2), in the aliphatic mixed chain extender, the molar ratio of adipic acid dihydrazide (ADH) and 1,4-butanediamine (BDA) is 0.5-2:0.5-2, preferably 1:
1.
6. The method for preparing a colorless and transparent poly(urethane-urea) elastomer based on mismatch supramolecular action according to claim 1, wherein step (2) comprises one or more of the following conditions: i. The mass concentration of the organic solution of the aliphatic mixed chain extender is 1-5%; the solvent used for the organic solution of the aliphatic mixed chain extender is one or a combination of two or more of N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide or N-methylpyrrolidone; ii. The molar amount of the aliphatic mixed chain extender is 40-60% of the molar amount of the diisocyanate, preferably 50%.
7. The method for preparing a colorless and transparent poly(urethane-urea) elastomer based on mismatch supramolecular action according to claim 1, wherein step (2) comprises one or more of the following conditions: i. The reaction temperature is room temperature, the reaction time is 2-7h, and the reaction is carried out under stirring conditions; ii. The degassing method is vacuum degassing; the drying conditions are: drying at 70-90°C for 10-14h, and then vacuum drying at 90-110°C for 6-10h.
8. A colorless and transparent poly(urethane-urea) elastomer based on mismatch supramolecular action, prepared by the method according to any one of claims 1 to 7.
9. Application of the colorless and transparent poly(urethane-urea) elastomer based on mismatch supramolecular action as claimed in claim 8 in the field of UV-resistant, high mechanical strength, damage-resistant, and recyclable transparent materials.
Citation Information
Patent Citations
BE655445A
Method for synergistically toughening thermoplastic poly (urethane-urea) by using rigid and soft supramolecular fragments and application of thermoplastic poly (urethane-urea)
CN115716901A
Thermosetting elastomer capable of improving recycling property and enhancing and toughening by utilizing mismatched supramolecular action as well as preparation and application of thermosetting elastomer
CN118184940A
Polyurethane elastomers and their preparation processes
FR1488992A