Metal lithium and magnesium separation method
Through the vacuum air-stage condensation method, the separation of lithium and magnesium is separated by different condensation temperatures, and the problem of difficulty in separation and low purity in high-purity lithium purification and lithium magnesium alloy recovery is solved, and the separation of high-purity lithium and magnesium is achieved, which simplifies the The process and reduce costs are suitable for industrial promotion.
Patent Information
- Application Number
- CN202411154901.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-26
AI Technical Summary
The prior art has problems of separation difficulties, low purity and high cost in the purification of high purity lithium and recycling of lithium magnesium alloys. Especially when the lithium magnesium alloy has complex composition and low lithium content, it leads to energy consumption in the recycling process. High and technical complexity increases.
Using the vacuum airification-classified condensation method, the lithium-containing magnesium raw material is vacuum airtreated to obtain magnesium vapor and lithium vapor, and the high-purity metal lithium and magnesium are separated by different condensation temperatures, and the vacuum airtreation is divided into the tube furnace. A condensation and a second condensation region achieves 100% separation of lithium and magnesium.
The separation of high-purity lithium and magnesium is achieved, the steps are simplified, and the costs are reduced. It is suitable for the preparation of high-purity lithium and the recycling of waste lithium-magnesium alloys, which significantly improves the efficiency and purity of lithium-magnesium separation.
Smart Images

Figure CN119020610A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of lithium-magnesium separation, and in particular relates to a method for separating metallic lithium and magnesium. Background Art
[0002] High-purity lithium has important applications in many industries, especially in high-performance batteries and special ceramics. During the lithium purification process, a variety of impurities including magnesium need to be removed to ensure the performance and reliability of the product. Currently, high-purity lithium is demagnetized by adding B2O3, but there are problems such as high cost, long process, and low lithium purity.
[0003] In addition, the recycling of waste lithium-magnesium alloy is an important part of the recycling of lithium resources, which is of great significance to protecting the environment, saving resources and achieving green and sustainable development. At present, the recycling technology of waste lithium-magnesium alloy mainly includes physical methods and chemical methods: the physical methods include: such as mechanical separation and melt separation, which physically separate lithium from the alloy. Chemical methods include: converting it into a reusable form through chemical reactions, such as acid leaching, solvent extraction, etc. Although the recycling of lithium-magnesium alloy seems feasible and beneficial in theory, there are still many challenges in actual operation: the first is the cost issue: the energy consumption in the recycling process is high, and the technical requirements are complex, and the requirements for equipment are also high, which will increase the cost of recycling. The second is the technical difficulty: the composition of lithium-magnesium alloy is complex, the lithium content is relatively low, the technical difficulty of effectively extracting lithium is relatively large, and the purity of the recovered lithium is very low.
[0004] In summary, whether it is the preparation of high-purity lithium or the recovery of lithium-magnesium alloy, there are problems such as difficult separation and low purity. Summary of the invention
[0005] The purpose of the present invention is to provide a method for separating metallic lithium and magnesium. The separation method provided by the present invention can achieve a 100% separation effect of lithium and magnesium, and has low cost. It is suitable for removing magnesium from high-purity lithium and recovering waste lithium-magnesium alloys.
[0006] In order to achieve the above object, the present invention provides the following technical solutions:
[0007] The present invention provides a method for separating metallic lithium and magnesium, comprising the following steps:
[0008] The lithium-magnesium-containing raw material is vacuum gasified to obtain magnesium vapor and lithium vapor; the lithium vapor is first condensed to obtain metallic lithium, and the magnesium vapor is second condensed to obtain metallic magnesium, wherein the temperature of the first condensation is greater than the temperature of the second condensation.
[0009] Preferably, the vacuum degree of the vacuum gasification is 1-5Pa.
[0010] Preferably, the vacuum gasification temperature is 650-850° C. and the time is 1-6 hours.
[0011] Preferably, the temperature of the first condensation is 450-400°C.
[0012] Preferably, the temperature of the second condensation is 350-250°C.
[0013] Preferably, the metallic lithium and magnesium separation is carried out in a tubular furnace, which is divided into a vacuum gasification area, a first condensation area and a second condensation area. The lithium-magnesium-containing raw material is located in the vacuum gasification area. The first condensation area obtains metallic lithium, and the second condensation area obtains metallic magnesium.
[0014] Preferably, after the tubular furnace is evacuated to 1-5 Pa, the tubular furnace is heated; in the tubular furnace: the temperature of the vacuum vaporization zone is 650-850°C, the temperature of the first condensation zone is 450-400°C, and the temperature of the second condensation zone is 350-250°C.
[0015] Preferably, the lithium-magnesium-containing raw material comprises lithium ingots or waste lithium-magnesium alloy;
[0016] The mass percentage of magnesium in the lithium ingot is greater than 0.01%;
[0017] The types of the waste lithium-magnesium alloy include one or more of MgLi5, MgLi10, MgLi15, MgLi20 and MgLi25.
[0018] Preferably, the mass percentage of lithium in the MgLi5 lithium-magnesium alloy is 4.5-5.5%.
[0019] The mass percentage of lithium in MgLi10 lithium-magnesium alloy is 9-11%.
[0020] The mass percentage of lithium in MgLi15 lithium-magnesium alloy is 14-16%.
[0021] The mass percentage of lithium in MgLi20 lithium-magnesium alloy is 19-21%.
[0022] The mass percentage of lithium element in MgLi25 lithium-magnesium alloy is 24-26%.
[0023] Preferably, the purity of the metallic lithium obtained by the first condensation is greater than 99.9%; the purity of the metallic magnesium obtained by the second condensation is greater than 99.9%.
[0024] The present invention provides a method for separating metallic lithium and magnesium, comprising the following steps: vacuum gasification of a raw material containing lithium and magnesium to obtain magnesium vapor and lithium vapor; first condensation of the lithium vapor to obtain metallic lithium, and second condensation of the magnesium vapor to obtain metallic magnesium, wherein the temperature of the first condensation is greater than the temperature of the second condensation. The present invention adopts a vacuum gasification-grading condensation method, firstly converting lithium and magnesium in the raw material containing lithium and magnesium from a solid phase to a gas phase, and then realizing the separation of lithium and magnesium by different condensation temperatures of gas phase magnesium and gas phase lithium. The separation method provided by the present invention can obtain high-purity lithium and magnesium elements, and the separation method has simple steps, low cost, and is suitable for industrial promotion. The results of the embodiment show that the present invention achieves a 100% separation effect of magnesium and lithium in the raw material through vacuum gasification-grading condensation, and can be mainly applied in two fields, one is the removal of magnesium when preparing high-purity lithium, and the other is the recovery of waste lithium-magnesium alloy. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is a physical picture of lithium condensation and magnesium condensation in the tubular furnace in Examples 1 to 3 of the present invention. DETAILED DESCRIPTION
[0026] The present invention provides a method for separating metallic lithium and magnesium, comprising the following steps:
[0027] The lithium-magnesium-containing raw material is vacuum gasified to obtain magnesium vapor and lithium vapor; the lithium vapor is first condensed to obtain metallic lithium, and the magnesium vapor is second condensed to obtain metallic magnesium, wherein the temperature of the first condensation is greater than the temperature of the second condensation.
[0028] In the present invention, unless otherwise specified, all preparation raw materials / components are commercially available products well known to those skilled in the art.
[0029] The present invention vacuum gasifies a lithium-magnesium-containing raw material to obtain magnesium vapor and lithium vapor. In the present invention, the lithium-magnesium-containing raw material preferably includes a lithium ingot or a waste lithium-magnesium alloy. The mass percentage of the magnesium element in the lithium ingot is preferably greater than 0.01%. The magnesium element contained in the lithium ingot is an impurity element. The types of the waste lithium-magnesium alloy preferably include one or more of MgLi5, MgLi10, MgLi15, MgLi20 and MgLi25. The mass percentage of the lithium element in the MgLi5 lithium-magnesium alloy is preferably 4.5-5.5%. The mass percentage of the lithium element in the MgLi10 lithium-magnesium alloy is preferably 9-11%. The mass percentage of the lithium element in the MgLi15 lithium-magnesium alloy is preferably 14-16%. The mass percentage of the lithium element in the MgLi20 lithium-magnesium alloy is preferably 19-21%. The mass percentage of the lithium element in the MgLi25 lithium-magnesium alloy is preferably 24-26%. In the present invention, the vacuum degree of the vacuum gasification is preferably 1-5 Pa. The temperature of the vacuum gasification is preferably 650-850° C., more preferably 700-850° C., and more preferably 700° C., 750° C. or 850° C. The time of the vacuum gasification is preferably 1-6 hours, and more preferably 1 hour, 3 hours or 6 hours.
[0030] After obtaining magnesium vapor and lithium vapor, the present invention performs a first condensation on the lithium vapor to obtain metallic lithium, and performs a second condensation on the magnesium vapor to obtain metallic magnesium, wherein the temperature of the first condensation is greater than the temperature of the second condensation. In the present invention, the temperature of the first condensation is preferably 450 to 400°C, and more preferably 400°C, 430°C or 450°C. The temperature of the second condensation is preferably 350 to 250°C, and more preferably 250°C, 300°C or 350°C.
[0031] In the present invention, the metal lithium and magnesium separation is preferably carried out in a tube furnace (that is, the above-mentioned vacuum gasification, first condensation and second condensation are carried out in the tube furnace at the same time), and the tube furnace is preferably divided into a vacuum gasification area, a first condensation area and a second condensation area, and the lithium-magnesium-containing raw material is preferably located in the vacuum gasification area, the first condensation area obtains metal lithium, and the second condensation area obtains metal magnesium. In the present invention, after the tube furnace is evacuated to 1-5 Pa, the tube furnace is then heated; in the tube furnace: the temperature of the vacuum gasification area is preferably 650-850°C, the temperature of the first condensation area is preferably 450-400°C, and the temperature of the second condensation area is preferably 350-250°C. In a specific embodiment, the temperature in the tube furnace from the vacuum gasification area to the first condensation area and then to the second condensation area preferably changes to 700-850°C, 600°C, 500°C, 400°C, 300°C, 200°C and 100°C in sequence.
[0032] In the present invention, during the process of heating the lithium-magnesium-containing raw material to the vacuum evaporation temperature, part of the magnesium vapor evaporates first, and then the lithium-magnesium vapor evaporates together. Due to the different condensation properties of the two metals, the lithium vapor condenses at the first condensation temperature, and the magnesium vapor condenses at the second condensation temperature. In the tubular furnace, the magnesium vapor and the lithium vapor move from the vacuum vaporization area to the first condensation area and the second condensation area, so that the lithium-magnesium-containing raw material is volatilized and condensed in the tubular furnace.
[0033] In the present invention, the purity of the metallic lithium obtained by the first condensation is preferably greater than 99.9%. The purity of the metallic magnesium obtained by the second condensation is preferably greater than 99.9%.
[0034] In order to further illustrate the present invention, the technical solutions provided by the present invention are described in detail below in conjunction with embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0035] Example 1
[0036] The raw material used in this embodiment is a crude lithium ingot: lithium content 98.5%, magnesium content 0.04%, set the program, vacuum degree 1 ~ 5Pa, gasification temperature 700 ℃, time 6h, lithium condensation zone temperature 400 ℃, magnesium condensation zone temperature 250 ℃. The crude lithium ingot is placed in a vacuum tube furnace near the left side, the temperature settings of the tube furnace from left to right are 700 ℃, 600 ℃, 500 ℃, 400 ℃, 300 ℃, 200 ℃, 100 ℃, evacuated to 1 ~ 5Pa, and heated until the end of the experiment, the magnesium content in the lithium condensation zone is <0.001%, and the magnesium content in the magnesium condensation zone is >99.9%.
[0037] Example 2
[0038] The raw material used in this embodiment is magnesium-lithium alloy (MgLi20), and the program is set to vacuum degree 1-5Pa, gasification temperature 750°C, time 3h, lithium condensation zone temperature 430°C, and magnesium condensation zone temperature 300°C. The magnesium-lithium alloy is placed in a vacuum tube furnace near the left side, and the temperature settings of the tube furnace from left to right are 750°C, 600°C, 500°C, 400°C, 300°C, 200°C, and 100°C, and the vacuum is evacuated to 1-5Pa, and heating is started until the end of the experiment. The purity of the lithium condensation zone is >99.9%, and the purity of the magnesium condensation zone is >99.9%.
[0039] Example 3
[0040] The raw material used in this embodiment is magnesium-lithium alloy (MgLi10), and the program is set to vacuum degree 1-5Pa, gasification temperature 850°C, time 1h, lithium condensation zone temperature 450°C, and magnesium condensation zone temperature 350°C. The magnesium-lithium alloy is placed in a vacuum tube furnace near the left side, and the temperature settings of the tube furnace from left to right are 850°C, 600°C, 500°C, 400°C, 300°C, 200°C, and 100°C, and the vacuum is evacuated to 1-5Pa, and heating is started until the end of the experiment. The purity of the lithium condensation zone is >99.9%, and the purity of the magnesium condensation zone is >99.9%.
[0041] It can be seen from the above embodiments that the method provided by the present invention achieves 100% separation of magnesium and lithium in the raw material through vacuum gasification-graded condensation, and can be mainly applied in two fields, one is the removal of magnesium when preparing high-purity lithium, and the other is the recovery of waste lithium-magnesium alloy.
[0042] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. Other embodiments can be obtained based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.
Claims
1. A method for separating metallic lithium and magnesium, characterized in that: The following steps are involved: The lithium-magnesium-containing raw material is vacuum gasified to obtain magnesium vapor and lithium vapor; the lithium vapor is first condensed to obtain metallic lithium, and the magnesium vapor is second condensed to obtain metallic magnesium, wherein the temperature of the first condensation is greater than the temperature of the second condensation.
2. The method for separating metallic lithium and magnesium according to claim 1, characterized in that: The vacuum degree of the vacuum gasification is 1-5Pa.
3. The method for separating metallic lithium and magnesium according to claim 1 or 2, characterized in that: The temperature of the vacuum gasification is 650-850° C., and the time is 1-6 hours.
4. The method for separating metallic lithium and magnesium according to claim 1, characterized in that: The temperature of the first condensation is 450-400°C.
5. The method for separating metallic lithium and magnesium according to claim 1 or 4, characterized in that: The temperature of the second condensation is 350-250°C.
6. The method for separating metallic lithium and magnesium according to claim 1, characterized in that: The metallic lithium-magnesium separation is carried out in a tubular furnace, which is divided into a vacuum gasification area, a first condensation area, and a second condensation area. The lithium-magnesium-containing raw material is located in the vacuum gasification area. The first condensation area obtains metallic lithium, and the second condensation area obtains metallic magnesium.
7. The method for separating metallic lithium and magnesium according to claim 6, characterized in that: After the tubular furnace is evacuated to 1-5 Pa, the tubular furnace is heated; in the tubular furnace: the temperature of the vacuum vaporization zone is 650-850° C., the temperature of the first condensation zone is 450-400° C., and the temperature of the second condensation zone is 350-250° C.
8. The method for separating metallic lithium and magnesium according to claim 1, characterized in that: The lithium-magnesium-containing raw material includes lithium ingots or waste lithium-magnesium alloy; The mass percentage of magnesium in the lithium ingot is greater than 0.01%; The types of the waste lithium-magnesium alloy include one or more of MgLi5, MgLi10, MgLi15, MgLi20 and MgLi25.
9. The method for separating metallic lithium and magnesium according to claim 8, characterized in that: The mass percentage of lithium element in the MgLi5 lithium-magnesium alloy is 4.5-5.5%. The mass percentage of lithium element in the MgLi10 lithium-magnesium alloy is 9-11%. The mass percentage of lithium element in the MgLi15 lithium-magnesium alloy is 14-16%. The mass percentage of lithium element in the MgLi20 lithium-magnesium alloy is 19-21%. The mass percentage of lithium element in the MgLi25 lithium-magnesium alloy is 24-26%.
10. The method for separating metallic lithium and magnesium according to claim 1, characterized in that: The purity of the metallic lithium is greater than 99.9%; the purity of the metallic magnesium is greater than 99.9%.