Active coke adsorbent as well as preparation method and application thereof

By mixing anthracite, bonded bituminous coal and weak bituminous coal in a specific proportion, and adding strong alkali and weak acid salt catalysts, an active coke adsorbent with high wear resistance and high denitrification rate was prepared, and the denitrification performance in the prior art was solved. The problem of the contradiction between low and ignition point has achieved efficient application in the purification of coal combustion flue gas.

CN119034684APending Publication Date: 2024-11-29CHINA ENERGY GRP NINGXIA COAL IND CO LTD +1

Patent Information

Application Number
CN202411425261.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-12
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The existing active coke adsorbents are difficult to take into account both the superior denitrification performance and the high ignition point. At the same time, the denitrification performance is not long-lasting, resulting in low desulfurization and denitrification efficiency, insufficient wear resistance, and easy ignition in the purification of coal combustion flue gas.

Method used

By mixing anthracite, bonded bituminous coal and weak bituminous coal in a specific proportion, adding a strong alkali and weak acid salt catalyst, and after carbonization and activation treatment, an active coke adsorbent with high wear resistance and moderate ignition point was prepared.

Benefits of technology

It significantly improves the denitrification rate and wear resistance of the active coke adsorbent, ensures its efficient application in dry flue gas desulfurization and denitrification technology, extends service life, and reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005081966350000091
    Figure BDA0005081966350000091
Patent Text Reader

Abstract

The invention provides an active coke adsorbent as well as a preparation method and application thereof. The preparation method comprises the following steps: adding a catalyst into feed coal, and mixing to obtain coal paste; sequentially carrying out carbonization treatment and activation treatment on the coal paste to obtain an active coke adsorbent; the raw material coal comprises anthracite, cohesive bituminous coal with the caking index GR, I of 70-85 and weak cohesive bituminous coal with the caking index GR, I of 5-25, and the weight ratio of the anthracite to the cohesive bituminous coal to the weak cohesive bituminous coal is (40-85): (10-30): (5-30). According to the invention, the adsorption performance and stability of the obtained active coke adsorbent are significantly improved by optimizing the variety, composition and proportion of the feed coal. The obtained active coke adsorbent not only has good abrasive resistance and relatively high denitration rate, but also is moderate in ignition point, and is suitable for being used as an efficient desulfurizing agent and a denitration agent in a dry flue gas desulfurization and denitration technology.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of coal materials, and in particular to an activated coke adsorbent, a preparation method and application thereof. Background Art

[0002] The large amount of SO2 and NOx generated by coal combustion is the main cause of acid rain and acid mist, which has caused great harm to the ecological environment and human health. The activated coke dry flue gas desulfurization and denitrification technology can effectively remove sulfur oxides and nitrogen oxides from coal combustion flue gas by utilizing the adsorption and catalytic properties of activated carbon.

[0003] In the activated coke dry flue gas desulfurization and denitrification technology, activated coke is a porous carbon material specially used for flue gas desulfurization and denitrification. Its preparation method is similar to that of activated carbon, and its main characteristics are small specific surface area, high wear resistance and briquetting strength, high desulfurization value, and low price. At present, the industry generally uses cylindrical activated coke with a diameter of 5mm or 9mm, which generally has the following problems: the product wear resistance is greater than 97%, the strength is low, and the loss is large during recycling; the product has less micropore distribution, low desulfurization and denitrification rate, and slow adsorption and desorption rate; the product has a low ignition point and is easy to ignite during the regeneration process. The product has low denitrification performance, which restricts the application of activated carbon dry flue gas purification technology. At the same time, the general commercial flue gas purification mainly emphasizes the desulfurization value of activated coke, and the requirements for denitrification rate and ignition point are relatively loose. However, with the increasingly severe air pollution problem, the removal of nitrogen oxides in flue gas cannot be ignored.

[0004] The main problems of current activated coke products are as follows: (1) Low wear resistance. (2) The denitrification rate is generally low, below 45%. (3) The ignition point is low, generally around 400°C. (4) The denitrification rate and ignition point are contradictory. This is because in order to increase the denitrification rate of the product, the product is treated with alkaline substances, which will also cause the ignition point of the product to decrease. This is the main technical bottleneck in the activated coke preparation process.

[0005] Based on this, how to optimize the preparation method of activated coke adsorbent and adjust the microstructure of the obtained activated coke adsorbent so that it can have both superior denitrification performance and a higher ignition point while maintaining long-lasting denitrification performance is one of the important technical problems that need to be solved in this field. Summary of the invention

[0006] The main purpose of the present invention is to provide an activated coke adsorbent, a preparation method and application thereof, so as to solve the problem that the activated coke adsorbent in the prior art is difficult to achieve both superior denitration performance and a higher ignition point, and the denitration performance is not persistent.

[0007] In order to achieve the above-mentioned purpose, the first aspect of the present invention provides a method for preparing an activated coke adsorbent, comprising: step S1, adding a catalyst to raw coal, mixing and obtaining a coal paste; step S2, carbonizing the coal paste to obtain a carbonized material; step S3, activating the carbonized material to obtain an activated coke adsorbent; the raw coal comprises anthracite, cohesive bituminous coal having a cohesive index GR,I of 70 to 85, and weakly cohesive bituminous coal having a cohesive index GR,I of 5 to 25, and the weight ratio of the anthracite, the cohesive bituminous coal and the weakly cohesive bituminous coal is (40 to 85): (10 to 30): (5 to 30).

[0008] Furthermore, the weight ratio of anthracite, caking bituminous coal and weakly caking bituminous coal is (60-70):(20-25):(10-15).

[0009] Furthermore, before adding the catalyst to the raw coal, step S1 also includes the steps of grinding and sieving the raw coal; preferably, the sieving process uses a 180-200 mesh screen, and the screening rate of the raw coal is 80%-90%.

[0010] Furthermore, the catalyst includes a strong base weak acid salt and a strong acid weak base salt, and the weight ratio of the strong base weak acid salt to the strong acid weak base salt is (1.0-1.2):1; preferably, the strong base weak acid salt is selected from one or more of sodium carbonate, sodium acetate, sodium phosphate and sodium hypochlorite; and / or the strong acid weak base salt is selected from one or more of copper sulfate, ferric chloride, ammonium chloride and ferric sulfate.

[0011] Furthermore, in step S1, based on the total weight of the raw coal being 100%, the amount of catalyst added is 0.2% to 2.0%.

[0012] Furthermore, in step S2, the temperature of the carbonization treatment is 400°C to 800°C, and the yield of the carbonization treatment is 65% to 80%.

[0013] Furthermore, in step S3, the temperature of the activation treatment is 800° C. to 1000° C., and the yield of the activation treatment is >80%.

[0014] The second aspect of the present invention provides an activated coke adsorbent, which is prepared by the above-mentioned method for preparing the activated coke adsorbent.

[0015] Furthermore, the activated coke adsorbent has a wear resistance of 95% to 99%, an ignition point of 460° C. to 505° C., and a denitrification rate of 40% to 55%.

[0016] The third aspect of the present invention provides a use of the above-mentioned activated coke adsorbent as a desulfurizer and a denitrifier in the activated coke dry flue gas desulfurization and denitrification process.

[0017] By applying the technical solution of the present invention, the adsorption performance and stability of the obtained activated coke adsorbent are significantly improved by optimizing the type, composition and ratio of raw coal. The prepared activated coke adsorbent not only has good wear resistance and high denitration rate, but also has a moderate ignition point, and is suitable for use as an efficient desulfurizer and denitrifier in dry flue gas desulfurization and denitration technology. DETAILED DESCRIPTION

[0018] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below in conjunction with the embodiments.

[0019] As described in the background art, the activated coke adsorbent in the prior art has the problem of being difficult to balance superior denitration performance and high ignition point, and the denitration performance is not durable. In order to solve the above technical problems, the first aspect of the present invention provides a method for preparing an activated coke adsorbent, comprising: step S1, adding a catalyst to raw coal, mixing to obtain a coal paste; step S2, carbonizing the coal paste to obtain a carbonized material; step S3, activating the carbonized material to obtain an activated coke adsorbent; the raw coal includes anthracite, caking bituminous coal with a caking index GR,I of 70 to 85, and weakly caking bituminous coal with a caking index GR,I of 5 to 25, and the weight ratio of anthracite, caking bituminous coal and weakly caking bituminous coal is (40 to 85): (10 to 30): (5 to 30).

[0020] It should be noted in advance that the specific definitions of anthracite, caking bituminous coal and weakly caking bituminous coal in the present invention are:

[0021] Anthracite, the most metamorphic coal, is characterized by low volatile matter content, high fixed carbon content and high calorific value. Anthracite produces almost no smoke when burned. Anthracite is hard and not easy to break. It burns with a short flame and a long burning time.

[0022] Cementing bituminous coal is a medium-grade coal with a moderate volatile content and good cementing properties. During the dry distillation process, this coal can form coke and produce a certain amount of smoke when burned, but less than weakly cementing bituminous coal.

[0023] Weakly cohesive bituminous coal is a coal with a low degree of metamorphism. It has a high volatile content and poor cohesiveness. During the heating process, the coke formed by this kind of coal is of poor quality, and it produces more smoke when it burns, and its calorific value is relatively low.

[0024] The technical solution provided by the present invention uses anthracite, caking bituminous coal and weakly caking bituminous coal in a coordinated manner, and matches the three in the above-mentioned dosage relationship, that is, by accurately controlling the type and ratio of the raw coal, the desulfurization value, denitrification rate and ignition point of the obtained activated coke adsorbent are significantly improved. In particular, the introduction of caking bituminous coal and weakly caking bituminous coal can effectively improve the wear resistance of the obtained adsorbent and can also significantly optimize the pore structure growth, so that the obtained activated coke adsorbent has a high denitrification rate and ignition point, while showing a stable and lasting denitrification ability.

[0025] And what needs additional explanation is that the caking index GR,I is an indicator to measure the ability of coal materials to form semi-coke and coke during heating. This value reflects the cohesiveness and coking properties of coal during gasification. The higher the caking index, the more semi-coke and coke the coal forms during gasification, and the gasification efficiency may be reduced. The caking index GR,I of the caking bituminous coal used in the present invention is 70-85, and the caking index GR,I of the weakly caking bituminous coal is 5-25. When the two are matched with anthracite in the above-mentioned weight ratio, used as raw coal and subsequently processed: the caking bituminous coal can form a viscous liquid-based colloid, which can wet the surface of solid coal particles and fill the gaps between particles, improve the cohesiveness, and then as the temperature rises, the colloid undergoes solidification, cracking, condensation and other reactions to form an aromatic carbon network structure, forming a skeleton structure inside the activated coke, and ultimately improving the wear resistance and compressive strength of the activated coke. The main function of weakly adhesive bituminous coal is to improve the pore size distribution structure of activated coke, increase the proportion of mesopores in activated coke, increase the average pore size of activated coke, and help improve the desulfurization value of activated coke.

[0026] In several typical implementations, the weight ratio of anthracite, caking bituminous coal and weakly caking bituminous coal is (60-70): (20-25): (10-15). The inventors further optimized the above dosage ratio through a large number of experiments to more effectively exert the synergistic relationship between the three coal materials, better balance the pore structure and mechanical strength relationship of the adsorbent during the formation process, and ultimately further improve the performance of the obtained activated coke adsorbent, especially in terms of wear resistance and denitrification rate.

[0027] Furthermore, before adding the catalyst to the raw coal, step S1 also includes the steps of grinding and sieving the raw coal; preferably, the sieving process uses a 180-200 mesh screen, and the screening rate of the raw coal is 80%-90%. Through such grinding and sieving process and particle size optimization, the particle size distribution of the raw coal can be made more uniform, thereby improving the efficiency of the subsequent preparation reaction, so that a microstructure with better pore distribution can be formed during the preparation process, thereby making the denitration performance of the obtained activated coke adsorbent better and more stable.

[0028] In order to more significantly improve the denitration rate of the obtained adsorbent, the inventors have selected, after a large number of experiments, that the catalyst includes a strong base weak acid salt and a strong acid weak base salt, and the weight ratio of the strong base weak acid salt and the strong acid weak base salt is (1.0-1.2):1. The introduction of such a composite catalyst can effectively improve the denitration performance of the obtained activated coke adsorbent while effectively protecting its ignition point, thereby balancing the relationship between the denitration and the ignition point, and obtaining an activated coke adsorbent with better comprehensive performance. In several typical embodiments, the strong base weak acid salt is selected from one or more of sodium carbonate, sodium acetate, sodium phosphate and sodium hypochlorite; and / or the strong acid weak base salt is selected from one or more of copper sulfate, ferric chloride, ammonium chloride and ferric sulfate. Theoretically, whether it is a strong base and a weak acid salt or a strong acid and a weak base salt, the types commonly used in the art can be selected, and the above-mentioned types selected by the inventor after a large number of experiments can better adapt to the raw coal system composed of anthracite, adhesive bituminous coal and weakly adhesive bituminous coal, and better regulate its microscopic pore structure in the process of forming the adsorbent product, and ultimately make the obtained activated coke adsorbent show better adsorption effect on sulfur oxides and nitrogen oxides.

[0029] And, on the basis of the above, in order to more effectively play the role of the catalyst, while improving the reaction efficiency, forming an adsorbent with a better pore structure, and at the same time making the catalyst more evenly loaded into the activated coke adsorbent, effectively protecting its ignition point, preferably in step S1, the total weight of the raw coal is 100%, and the amount of catalyst added is 0.2% to 2.0%, thereby obtaining an activated coke adsorbent with both high denitrification rate and ignition point.

[0030] In several typical implementations, in order to meet the physical and chemical characteristics of the raw coal composed of anthracite, caking bituminous coal and weakly caking bituminous coal, the inventors have optimized the temperature of the carbonization treatment in step S2 to be 400°C to 800°C and the yield of the carbonization treatment to be 65% to 80% through a large number of experiments. Within this temperature range and yield requirement, the organic matter in the raw coal is more fully converted into porous carbon, and the yield reduction caused by excessive carbonization is well suppressed, so that the obtained adsorbent exhibits better desulfurization and denitrification performance and yield.

[0031] Furthermore, after a large number of experiments, the inventors have optimized the temperature of the activation treatment in step S3 to be 800°C to 1000°C, and the yield of the activation treatment is >80%, thereby more effectively optimizing the pore structure of the obtained activated coke adsorbent, improving its adsorption capacity and service life, while maintaining a high yield and increasing its product added value.

[0032] It should be explained here that, in the activation treatment of the present invention, the temperature is the effective temperature, that is, the temperature in the middle of the activation zone of the activation furnace.

[0033] The second aspect of the present invention provides an activated coke adsorbent, which is prepared by the above-mentioned method for preparing the activated coke adsorbent. The obtained activated coke adsorbent not only exhibits excellent performance in flue gas purification but also has wide applicability and good economic benefits, and is an ideal choice in the energy and environmental fields, especially in the field of industrial flue gas purification.

[0034] Furthermore, the activated coke adsorbent has a wear resistance of 95% to 99%, an ignition point of 460°C to 505°C, and a denitration rate of 40% to 55%. In other words, the activated coke adsorbent obtained by the present invention can take into account both a good denitration rate and a high ignition point, and at the same time has extremely high wear resistance, can well withstand mechanical wear during the application process, and has a long service life.

[0035] The third aspect of the present invention provides an application of the above-mentioned activated coke adsorbent as a desulfurizer and denitrifier in the process of activated coke dry flue gas desulfurization and denitrification. The obtained activated coke adsorbent not only has good wear resistance and high denitrification rate, but also has a moderate ignition point, and is suitable for use as an efficient desulfurizer and denitrifier in dry flue gas desulfurization and denitrification technology. This method not only broadens the scope of application of raw coal, but also reduces production costs, improves the economic and environmental benefits of activated coke adsorbents, and provides more reliable and economical adsorption functional materials for activated coke dry flue gas desulfurization and denitrification technology. In addition, the high yield and excellent performance of the activated coke adsorbent give it broad application prospects in the flue gas treatment of heavily polluting industries such as coal-fired power generation, steel smelting, and cement production, which helps to promote these industries to develop in a cleaner and more environmentally friendly direction, and meets the current global urgent need to reduce industrial pollution and protect the environment.

[0036] The present application is further described in detail below in conjunction with specific embodiments. These embodiments should not be construed as limiting the scope of protection claimed in the present application.

[0037] Unless otherwise defined, all professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.

[0038] Furthermore, the anthracite used in the present invention has a volatile matter content of 6% to 10%; the volatile matter content of the cohesive bituminous coal is 10% to 30%; and the volatile matter content of the weakly cohesive bituminous coal is 25% to 35%.

[0039] Example 1

[0040] A method for preparing an activated coke adsorbent:

[0041] Anthracite, caking bituminous coal with a caking index GR,I of 75, and weakly caking bituminous coal with a caking index GR,I of 15 are mixed uniformly in a weight ratio of 60:25:15, and then ground and sieved. The passing rate of coal powder with a 200 mesh is 85%, thereby obtaining raw coal;

[0042] Copper sulfate and sodium carbonate were mixed in a mass ratio of 1:1, a binder was added, and then granulated and formed. The diameter of the mold was 9.2 mm and the forming pressure was 110 kgf / cm 2 , a composite catalyst is prepared;

[0043] Adding a composite catalyst with a mass fraction of 0.5% of the raw coal, kneading it evenly into coal paste in a kneading and stirring device, and then granulating it into carbon strips on a granulator; drying the formed strips for more than 48 hours, and carbonizing them, with the carbonization temperature controlled at 750°C and the carbonization yield controlled at 70%, to obtain a carbonized material;

[0044] The carbonized material was activated at an effective temperature of 900° C., and the activation yield of the product was controlled to be 81%, thereby obtaining an activated coke adsorbent.

[0045] Example 2

[0046] A method for preparing an activated coke adsorbent:

[0047] Anthracite, caking bituminous coal with a caking index GR,I of 85, and weakly caking bituminous coal with a caking index GR,I of 5 are mixed uniformly in a weight ratio of 65:20:15, and then ground and sieved. The passing rate of coal powder with a 200 mesh is 85%, thereby obtaining raw coal;

[0048] Copper sulfate and sodium carbonate were mixed in a mass ratio of 1:1.2, a binder was added, and then granulated and formed. The diameter of the mold was 9.2 mm and the forming pressure was 110 kgf / cm 2 , a composite catalyst is prepared;

[0049] Adding a composite catalyst with a mass fraction of 0.4% of raw coal, kneading it evenly into coal paste in a kneading and stirring device, and then granulating it into carbon strips on a granulator; drying the formed strips for more than 48 hours, and carbonizing them, with the carbonization temperature controlled at 400°C and the carbonization yield controlled at 65%, to obtain a carbonized material;

[0050] The carbonized material was activated at an effective temperature of 800°C, and the activation yield of the product was controlled to be 82%, thereby obtaining an activated coke adsorbent.

[0051] Example 3

[0052] A method for preparing an activated coke adsorbent:

[0053] Anthracite, caking bituminous coal with a caking index GR,I of 70, and weakly caking bituminous coal with a caking index GR,I of 25 are mixed uniformly in a weight ratio of 70:20:10, and then ground and sieved. The passing rate of coal powder with a 200 mesh is 85%, thereby obtaining raw coal;

[0054] The catalyst prepared in Example 1 is used as a composite catalyst;

[0055] Adding a composite catalyst with a mass fraction of 0.35% of the raw coal, kneading it evenly into coal paste in a kneading and stirring device, and then granulating it into carbon strips on a granulator; drying the formed strips for more than 48 hours, and carbonizing them, with the carbonization temperature controlled at 800°C and the carbonization yield controlled at 80%, to obtain a carbonized material;

[0056] The carbonized material was activated at an effective temperature of 1000° C. The activation yield of the product was controlled to be 82.5%, thereby obtaining an activated coke adsorbent.

[0057] Example 4

[0058] A method for preparing an activated coke adsorbent:

[0059] The only difference between this embodiment and embodiment 1 is that the weight ratio of anthracite, caking bituminous coal and weakly caking bituminous coal is changed to 70:20:10.

[0060] Example 5

[0061] A method for preparing an activated coke adsorbent:

[0062] The only difference between this embodiment and embodiment 2 is that the weight ratio of anthracite, caking bituminous coal and weakly caking bituminous coal is changed to 70:20:10.

[0063] Example 6

[0064] A method for preparing an activated coke adsorbent:

[0065] The only difference between this embodiment and embodiment 1 is that the weight ratio of anthracite, caking bituminous coal and weakly caking bituminous coal is changed to 50:30:20.

[0066] Example 7

[0067] A method for preparing an activated coke adsorbent:

[0068] The only difference between this embodiment and embodiment 1 is that the weight ratio of anthracite, caking bituminous coal and weakly caking bituminous coal is changed to 80:15:5.

[0069] Example 8

[0070] A method for preparing an activated coke adsorbent:

[0071] The only difference between this embodiment and embodiment 1 is that during the preparation of the composite catalyst, the mass ratio of copper sulfate to sodium carbonate is changed to 0.8:1.

[0072] Example 9

[0073] A method for preparing an activated coke adsorbent:

[0074] The only difference between this embodiment and embodiment 1 is that during the preparation of the composite catalyst, the mass ratio of copper sulfate to sodium carbonate is changed to 1.5:1.

[0075] Example 10

[0076] A method for preparing an activated coke adsorbent:

[0077] The only difference between this embodiment and embodiment 1 is that no composite catalyst is prepared, but copper sulfate is directly used as a catalyst and added to the raw coal at a mass fraction of 2.5% of the raw coal.

[0078] Embodiment 11

[0079] A method for preparing an activated coke adsorbent:

[0080] The only difference between this embodiment and embodiment 1 is that no composite catalyst is prepared, but sodium carbonate is directly used as a catalyst and added to the raw coal at a mass fraction of 0.1%.

[0081] Example 12

[0082] A method for preparing an activated coke adsorbent:

[0083] The only difference between this embodiment and embodiment 1 is that during the carbonization process, the carbonization temperature is changed to 300° C., the carbonization yield is controlled at 60%, and a carbonized material is obtained.

[0084] Embodiment 13

[0085] A method for preparing an activated coke adsorbent:

[0086] The only difference between this embodiment and embodiment 1 is that during the carbonization process, the carbonization temperature is changed to 900° C., the carbonization yield is controlled at 90%, and a carbonized material is obtained.

[0087] Embodiment 14

[0088] A method for preparing an activated coke adsorbent:

[0089] The only difference between this embodiment and embodiment 1 is that during the activation treatment, the effective temperature is changed to 700° C. and the activation yield of the product is controlled to be 60%.

[0090] Embodiment 15

[0091] A method for preparing an activated coke adsorbent:

[0092] The only difference between this embodiment and embodiment 1 is that during the activation treatment, the effective temperature is changed to 1200° C. and the activation yield of the product is controlled to be 85%.

[0093] Comparative Example 1

[0094] A method for preparing an activated coke adsorbent:

[0095] The only difference between this comparative example and Example 1 is that neither caking bituminous coal nor weakly caking bituminous coal is used, but only anthracite is used as raw coal.

[0096] Comparative Example 2

[0097] A method for preparing an activated coke adsorbent:

[0098] The only difference between this comparative example and Example 1 is that anthracite and weakly caking bituminous coal are not used, but only caking bituminous coal is used as raw coal.

[0099] Comparative Example 3

[0100] A method for preparing an activated coke adsorbent:

[0101] The only difference between this comparative example and Example 1 is that anthracite and caking bituminous coal are not used, but only weakly caking bituminous coal is used as raw coal.

[0102] Comparative Example 4

[0103] A method for preparing an activated coke adsorbent:

[0104] The only difference between this comparative example and Example 1 is that the weight ratio of anthracite, caking bituminous coal and weakly caking bituminous coal is changed to 30:35:35.

[0105] Comparative Example 5

[0106] A method for preparing an activated coke adsorbent:

[0107] The only difference between this comparative example and Example 1 is that the weight ratio of anthracite, caking bituminous coal and weakly caking bituminous coal is changed to 92:5:3.

[0108] Test Method

[0109] Bulk weight: Tested in accordance with GB / T30202.1-201.

[0110] Iodine value: tested in accordance with GB / T7702.7-2023.

[0111] Abrasion resistance and compressive strength: tested in accordance with GB / T30202.3-2013.

[0112] Ash content: tested in accordance with GB / T7702.15-2008.

[0113] Fire point: Tested in accordance with GB / T7702.9-2008.

[0114] Desulfurization value: tested in accordance with GB / T30202.4-2013.

[0115] Denitrification rate: tested in accordance with GB / T30202.5-2013.

[0116] The above performance tests were performed on the activated coke adsorbents obtained in the examples and comparative examples, and the results are shown in Table 1.

[0117] Table 1

[0118]

[0119] From the above description, it can be seen that the above embodiments of the present invention achieve the preparation of activated coke adsorbent that can take into account both excellent denitrification performance and high ignition point, and the obtained activated coke adsorbent also exhibits excellent wear resistance and desulfurization value.

[0120] Specifically, by comparing Examples 1, 2, 3 with 4, 5, it can be concluded that when activated coke is produced using a single type of coal, the various performance indicators of the activated coke are lower than those of activated coke produced using blended coal.

[0121] It can be concluded from Examples 10 and 11 that the denitrification rate of the activated coke product prepared by using a single catalyst is slightly lower than that by using a composite catalyst.

[0122] It should be noted that the terms "first", "second", etc. in the specification and claims of the present application are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the terms used in this way can be interchangeable where appropriate, so that the embodiments of the present application described herein can be implemented in an order other than those described herein, for example.

[0123] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing an activated coke adsorbent, characterized in that: include: Step S1, adding a catalyst to raw coal and mixing to obtain a coal paste; Step S2, carbonizing the coal paste to obtain a carbonized material; Step S3, performing activation treatment on the carbonized material to obtain the activated coke adsorbent; The raw coal includes anthracite, caking bituminous coal with a caking index GR,I of 70 to 85, and weakly caking bituminous coal with a caking index GR,I of 5 to 25, and the weight ratio of the anthracite, the caking bituminous coal and the weakly caking bituminous coal is (40 to 85): (10 to 30): (5 to 30).

2. The method for preparing an activated coke adsorbent according to claim 1, characterized in that: The weight ratio of the anthracite, the caking bituminous coal and the weakly caking bituminous coal is (60-70):(20-25):(10-15).

3. The method for preparing an activated coke adsorbent according to claim 1 or 2, characterized in that: Before adding the catalyst to the raw coal, step S1 further includes the steps of grinding and sieving the raw coal; Preferably, the screening process uses a sieve of 180-200 mesh, and the screening rate of the raw coal is 80%-90%.

4. The method for preparing an activated coke adsorbent according to any one of claims 1 to 3, characterized in that: The catalyst includes a strong base weak acid salt and a strong acid weak base salt, and the weight ratio of the strong base weak acid salt to the strong acid weak base salt is (1.0-1.2):1; Preferably, the strong base weak acid salt is selected from one or more of sodium carbonate, sodium acetate, sodium phosphate and sodium hypochlorite; and / or, the strong acid weak base salt is selected from one or more of copper sulfate, ferric chloride, ammonium chloride and ferric sulfate.

5. The method for preparing an activated coke adsorbent according to any one of claims 1 to 4, characterized in that: In step S1, based on the total weight of the raw coal being 100%, the amount of the catalyst added is 0.2% to 2.0%.

6. The method for preparing an activated coke adsorbent according to any one of claims 1 to 5, characterized in that: In step S2, the temperature of the carbonization treatment is 400°C to 800°C, and the yield of the carbonization treatment is 65% to 80%.

7. The method for preparing an activated coke adsorbent according to any one of claims 1 to 6, characterized in that: In step S3, the temperature of the activation treatment is 800°C to 1000°C, and the yield of the activation treatment is >80%.

8. An activated coke adsorbent, characterized in that: The activated coke adsorbent is prepared by the method for preparing the activated coke adsorbent according to any one of claims 1 to 7.

9. The activated coke adsorbent according to claim 8, characterized in that: The active coke adsorbent has a wear resistance of 95% to 99%, an ignition point of 460° C. to 505° C., and a denitrification rate of 40% to 55%.

10. Use of the activated coke adsorbent according to claim 8 or 9 as a desulfurizer and a denitrifier in an activated coke dry flue gas desulfurization and denitrification process.

Citation Information

Patent Citations

  • Active carbon used for adsorbing dioxins in waste incineration flue gas, and preparation method thereof

    CN106938846A

  • Tar-free activated carbon and preparation method thereof

    CN115180621A

  • Spontaneous ignition prevention method of active carbon

    JP2008173552A

Cited By

  • Purifying agent prepared based on solid waste and application method

    CN121553939A