Denitration catalyst as well as preparation method and application thereof
By loading the composite oxide MCuOx and rare earth elements on the FAU molecular sieve matrix, a denitrification catalyst with high efficiency anti-poisoning and ultra-wide temperature range catalytic activity was prepared, which solved the problems of sulfur dioxide poisoning and activity reduction in the prior art, and achieved efficient Flue gas purification.
Patent Information
- Application Number
- CN202411166101.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-08-23
AI Technical Summary
The activity of existing denitrification catalysts has decreased in the environment of sulfur dioxide poisoning, making it difficult to take into account both high-temperature and low-temperature catalytic activities, and there is difficulty in recycling and processing of toxic material V2O5.
The layered FAU molecular sieve matrix and the composite oxide MCuOx are used as catalysts, and prepared by hydrothermal reaction and ion exchange, and rare earth elements are doped to improve redox capacity and anti-toxicity performance to form an efficient denitrification catalyst.
Maintain high catalytic activity and nitrogen selectivity in a high SO2 environment, reduce the impact of sulfur dioxide poisoning, simplify the preparation process and reduce costs.
Smart Images

Figure CN119034794A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of environmental protection catalysts and relates to a molecular sieve confined denitration catalyst and a preparation method and application thereof. Background Art
[0002] Nitrogen oxides (NO x ) is the main source of air pollution, mainly from the combustion of fossil fuels. Excessive emissions can cause environmental and climate problems such as acid rain, photochemical smog and global warming. Traditional denitrification technology uses ammonia selective catalytic reduction (NH3-SCR) method, with V2O5-WO3 / TiO2 or its modified substances as catalysts, and the operating temperature is usually 300-400℃. However, this catalyst has low activity at 250℃, and V2O5 is toxic, and its recovery and treatment have become a development bottleneck. Catalysts with copper oxide (CuO) and modified copper oxide as active components have attracted widespread attention from researchers due to their good low-temperature catalytic activity, high nitrogen selectivity and environmental protection characteristics.
[0003] At present, in practical applications, when SCR denitrification catalysts are used for boiler flue gas treatment, they will encounter the problem of sulfur dioxide poisoning leading to catalyst deactivation. This is because the coal ash produced during the boiler combustion process contains a certain amount of sulfur dioxide gas, which will cover the catalyst surface and react with ammonia and copper-based active components to generate ammonium sulfate and cover the catalyst surface, which reduces the number of exposed active sites. At the same time, this will also lead to the formation of copper sulfate that is not easy to decompose, destroying the redox ability of the catalyst and causing irreversible deactivation of the catalyst.
[0004] CN102416320A discloses a denitration catalyst, and relates to the technical field of catalysts. The catalyst is composed of the following components in parts by weight: 75-85 parts of titanium dioxide; 10-12 parts of tungsten trioxide; 3-6 parts of silicon dioxide; 2-3 parts of vanadium pentoxide; 3-6 parts of kapok pulp; 2-7 parts of glass fiber; 2-3 parts of stearic acid; the components are mixed according to the weight proportions, stirred evenly, and then aged, pre-extruded, secondary aged, extruded, dried once, dried twice, calcined at high temperature, and finished product trimmed in sequence, and then the finished catalyst can be packaged.
[0005] CN107737588A discloses a denitration catalyst, the raw materials of which are 35-45 parts by weight of titanium dioxide, 2-5 parts by weight of antimony oxide, 10-20 parts by weight of glass fiber, 1-3 parts by weight of vanadium pentoxide, 3-6 parts by weight of molybdenum oxide, and 3-6 parts by weight of tungsten oxide.
[0006] The denitrification catalyst described in the above scheme is difficult to take into account both high-temperature and low-temperature catalytic activity, and after being poisoned by sulfur dioxide, the activity of the catalyst drops sharply. Therefore, improving the denitrification performance of the denitrification catalyst in the presence of sulfur dioxide is very important for saving the flue gas purification cost of the coal-fired industry and improving the exhaust gas treatment efficiency. Summary of the invention
[0007] In order to solve the above technical problems, the present invention aims to provide a denitration catalyst and its preparation method and use. The denitration catalyst of the present invention has high surface acidity and redox ability, and the composite oxide MCuO located on the surface and pores of the layered FAU molecular sieve matrix x The catalyst's ability to resist sulfur dioxide poisoning has been improved, ensuring that the catalyst still has high catalytic activity in a high SO2 environment, or even maintains its original activity, and has high catalytic activity and nitrogen selectivity within the operating temperature range of 250-400°C.
[0008] To achieve this object, the present invention adopts the following technical solutions:
[0009] In a first aspect, the present invention provides a denitration catalyst, the denitration catalyst comprising a layered FAU molecular sieve matrix and a composite oxide active component supported on the surface and in the pores of the layered FAU molecular sieve matrix, wherein the chemical formula of the composite oxide active component is MCuO x , M is a rare earth doping element, wherein x is the molar amount of oxygen atoms in the composite oxide, and 1≤x≤2.
[0010] In the denitration catalyst provided by the present invention, the morphology of the FAU molecular sieve matrix is layered, so it has a strong interlayer mass transfer ability and can convert NO x , NH3 and other gases quickly diffuse to the active sites, and the active component of the composite oxide MCuO x The presence of MO-Cu asymmetric oxygen vacancies can enhance the NO x The introduction of rare earth elements can improve the overall redox capacity of the catalyst. At the same time, combined with the highly dispersed MCuO anchored in the molecular sieve framework, x Active sites make it difficult for sulfur dioxide to be chemically adsorbed on the catalyst. The denitration catalyst provided by the present invention has strong Bronsted acid sites and Lewis acid sites, which can increase the catalyst's ability to adsorb NH3 and its ability to resist poisoning by sulfur dioxide.
[0011] The following are preferred technical solutions of the present invention, but are not intended to limit the technical solutions provided by the present invention. Through the following preferred technical solutions, the technical objectives and beneficial effects of the present invention can be better achieved and realized.
[0012] Preferably, the layered FAU molecular sieve matrix comprises an X-type molecular sieve or a Y-type molecular sieve, preferably an X-type molecular sieve.
[0013] Preferably, the silicon-aluminum ratio of the layered FAU molecular sieve matrix is (1-30):1, for example, it can be 1:1, 2:1, 3:1, 4:1, 5:1, 6:1, 7:1, 8:1, 9:1, 10:1, 12:1, 14:1, 16:1, 18:1, 20:1, 22:1, 24:1, 26:1, 28:1, 29:1 or 30:1, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0014] Preferably, based on the total molar amount of silicon element and composite oxide active component in the FAU molecular sieve, the molar fraction of the composite oxide active component is 5-30%, for example, it can be 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 28% or 30%, but is not limited to the listed values, and other values not listed within the numerical range are also applicable, preferably 10-25%.
[0015] Preferably, in the composite oxide active component, the molar ratio of the rare earth doping element to the copper element is (0.05-0.2):1, for example, it can be 0.05:1, 0.06:1, 0.07:1, 0.08:1, 0.09:1, 0.1:1, 0.11:1, 0.12:1, 0.12:1, 0.13:1, 0.14:1, 0.15:1, 0.16:1, 0.17:1, 0.18:1, 0.19:1 or 0.2:1, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0016] In the present invention, the molar ratio of the rare earth doping element and the copper element will affect its performance. The molar ratio of the rare earth doping element and the copper element is controlled at (0.05-0.2):1. The denitration catalyst can maintain high-temperature catalytic activity and also has excellent low-temperature activity. If the cerium ratio is too low, the high-temperature performance of the catalyst after 350°C decreases. If the cerium ratio is too high, the low-temperature performance of the catalyst before 300°C is poor.
[0017] Preferably, the rare earth doping element includes any one of cerium, neodymium, samarium, cobalt, europium, yttrium, dysprosium, ytterbium, lanthanum or praseodymium, or a combination of at least two thereof, wherein typical but non-limiting combinations include a combination of cerium and neodymium, a combination of neodymium and samarium, a combination of cobalt and europium, a combination of dysprosium, ytterbium and lanthanum, a combination of cerium, neodymium and samarium, a combination of cerium, neodymium, samarium, cobalt and europium, a combination of cobalt, europium, yttrium, dysprosium, ytterbium and lanthanum, and a combination of cerium, neodymium, samarium, cobalt, europium, yttrium, dysprosium, ytterbium, lanthanum and praseodymium.
[0018] In a second aspect, the present invention provides a method for preparing the denitration catalyst as described in the first aspect, the preparation method comprising the following steps:
[0019] Aluminum source, sodium hydroxide, silicon source, rare earth doping element source, copper source and water are mixed and stirred, and then subjected to hydrothermal reaction to obtain a first product; the first product is mixed with ammonium nitrate solution to perform ion exchange to obtain a second product; and the second product is roasted to obtain the denitration catalyst.
[0020] The preparation method of the denitration catalyst provided by the present invention is simple and easy to operate, and the denitration catalyst is prepared by adding a molecular sieve raw material and a raw material of an active component together for hydrothermal reaction, and then performing ion exchange. Since the molecular sieve of the FAU structure has a stable topological structure and low crystal formation energy, it can be successfully crystallized at a lower temperature after adding sodium hydroxide. Therefore, compared with the conventional preparation method in the prior art (such as the synthesis of Cu-SSZ-13, Cu-SAPO-34 and Cu-ZSM-5 molecular sieve catalysts), the step of adding an organic template is omitted, and a hydrothermal process of more than 12 hours is not required, which saves preparation time and cost.
[0021] Preferably, the silicon source comprises sodium silicate.
[0022] Preferably, the aluminum source comprises sodium metaaluminate.
[0023] Preferably, the rare earth doping element source includes any one of cerium nitrate hexahydrate, neodymium nitrate, samarium nitrate, cobalt nitrate, europium nitrate, yttrium nitrate, dysprosium nitrate, ytterbium nitrate, lanthanum nitrate or praseodymium nitrate, or a combination of at least two of them, wherein typical but non-limiting combinations include a combination of cerium nitrate hexahydrate and neodymium nitrate, a combination of neodymium nitrate and samarium nitrate, a combination of samarium nitrate and cobalt nitrate, a combination of cobalt nitrate, europium nitrate and yttrium nitrate, a combination of cerium nitrate hexahydrate, neodymium nitrate and samarium nitrate, a combination of cerium nitrate hexahydrate, neodymium nitrate, samarium nitrate, cobalt nitrate and europium nitrate, a combination of cobalt nitrate, europium nitrate, yttrium nitrate, dysprosium nitrate, ytterbium nitrate and lanthanum nitrate, and a combination of cerium nitrate hexahydrate, neodymium nitrate, samarium nitrate, cobalt nitrate, europium nitrate, yttrium nitrate, dysprosium nitrate, ytterbium nitrate, lanthanum nitrate and praseodymium nitrate.
[0024] Preferably, the copper source comprises copper nitrate.
[0025] Preferably, the molar ratio of the sodium hydroxide to the aluminum element in the aluminum source is 1:(5-10), for example, it can be 1:5, 1:6, 1:7, 1:8, 1:9 or 1:10, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0026] Preferably, the stirring time is 1-2 h, for example, 1 h, 1.2 h, 1.4 h, 1.6 h, 1.8 h or 2 h, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0027] Preferably, the stirred mixture is allowed to stand before the hydrothermal reaction.
[0028] Preferably, the standing time is 6-10 hours, for example, 6 hours, 7 hours, 8 hours, 9 hours or 10 hours, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0029] Preferably, the hydrothermal reaction time is 4-8 h, for example, 4 h, 5 h, 6 h, 7 h or 8 h, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0030] In the preparation method of the present invention, the standing time and the hydrothermal time are controlled within a reasonable range, and the activity and the ability of the obtained catalyst to resist SO2 poisoning are more excellent. The standing time and the hydrothermal time will affect the crystallinity of the molecular sieve in the catalyst. If the standing time or the hydrothermal time is too short, the molecular sieve skeleton will not grow completely, and the MCuO can not be successfully anchored. x The catalytic performance of the active components under NH3-SCR conditions with or without SO2 will decrease accordingly; and if the static time or hydrothermal time is too long, the rare earth doping element source and copper source will be dissolved and enriched on the surface of the molecular sieve, and cannot be dispersed and anchored in the pores, thereby affecting the NH3-SCR catalytic performance and resistance to SO2 poisoning.
[0031] Preferably, the hydrothermal reaction temperature is 100-120°C, for example, it can be 100°C, 102°C, 104°C, 106°C, 108°C, 110°C, 112°C, 114°C, 116°C, 118°C or 120°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0032] Preferably, the concentration of the ammonium nitrate solution is 1-4 mol / L, for example, it can be 1 mol / L, 1.5 mol / L, 2 mol / L, 2.5 mol / L, 3 mol / L, 3.5 mol / L or 4 mol / L, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0033] Preferably, the mass ratio of the first product to the ammonium nitrate solution is 1:(15-30), for example, it can be 1:15, 1:16, 1:17, 1:18, 1:19, 1:20, 1:21, 1:22, 1:23, 1:24, 1:25, 1:26, 1:27, 1:28, 1:29 or 1:30, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0034] Preferably, the ion exchange temperature is 60-100°C, for example, 60°C, 65°C, 70°C, 75°C, 80°C, 85°C, 90°C, 95°C or 100°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0035] Preferably, the ion exchange time is 8-15 h, for example, 8 h, 9 h, 10 h, 11 h, 12 h, 13 h, 14 h or 15 h, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0036] Preferably, the ion exchange is repeated 1-3 times, for example, 1 time, 2 times or 3 times, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0037] Preferably, the drying temperature is 70-90°C, for example, 70°C, 75°C, 80°C, 85°C or 90°C, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0038] Preferably, the drying time is 8-16 h, for example, 8 h, 9 h, 10 h, 11 h, 12 h, 13 h, 14 h, 15 h or 16 h, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0039] Preferably, the calcination temperature is 400-600°C, for example, it can be 400°C, 420°C, 440°C, 460°C, 480°C, 500°C, 520°C, 540°C, 580°C or 600°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0040] In the preparation method of the denitration catalyst provided by the present invention, the activity and resistance to SO2 poisoning of the catalyst obtained by controlling the calcination temperature in the range of 400-600°C are more excellent. If the calcination temperature is too high, the molecular sieve framework will collapse, covering the MCuO xActive sites are formed, resulting in the inability of active components to be exposed and contact with reactants such as NO and NH3, leading to reduced catalyst performance; while too low a calcination temperature will lead to a decrease in the crystallinity of the molecular sieve and incomplete skeleton growth, which will greatly reduce the NH3-SCR catalytic performance of the catalyst in the presence of SO2.
[0041] Preferably, the heating rate of the calcination is 1-10°C / min, for example, it can be 1°C / min, 2°C / min, 3°C / min, 4°C / min, 5°C / min, 6°C / min, 7°C / min, 8°C / min, 9°C / min or 10°C / min, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0042] Preferably, the calcination time is 3-10 h, for example, 3 h, 4 h, 5 h, 6 h, 7 h, 8 h, 9 h or 10 h, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0043] In a third aspect, the present invention provides a use of a denitration catalyst as described in the first aspect, wherein the denitration catalyst is used for ammonia selective catalytic reduction of nitrogen oxides.
[0044] Preferably, the operating temperature of the catalyst is 100-550°C, for example, it can be 100°C, 150°C, 200°C, 250°C, 300°C, 350°C, 400°C, 450°C, 500°C or 550°C, but is not limited to the listed values. Other unlisted values within the numerical range are also applicable, preferably 150-400°C.
[0045] The denitration catalyst provided by the present invention can be used for the selective catalytic reduction of nitrogen oxides by ammonia and can cover an ultra-wide temperature range of 100-550° C., and the catalyst has excellent resistance to sulfur dioxide poisoning.
[0046] In a third aspect, the present invention provides a denitration reactor, wherein the denitration reactor comprises the denitration catalyst as described in the first aspect.
[0047] In a fourth aspect, the present invention provides a denitration reaction device, the denitration device comprising the denitration reactor described in the third aspect;
[0048] The denitration reaction device is used in a mobile source gas denitration device and / or a fixed source gas denitration device.
[0049] Preferably, the mobile source gas denitrification device includes any one of a diesel engine, a gas turbine or an aircraft engine.
[0050] Preferably, the fixed source gas denitrification device includes an industrial kiln and / or a roasting kiln.
[0051] The numerical range described in the present invention not only includes the point values listed above, but also includes any point values between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the range.
[0052] Compared with the prior art, the present invention has at least the following beneficial effects:
[0053] (1) In the denitration catalyst provided by the present invention, the morphology of the FAU molecular sieve matrix is layered, so it has a strong interlayer mass transfer ability and can convert NO x , NH3 and other gases quickly diffuse to the active sites, and the active component of the composite oxide MCuO x The presence of MO-Cu asymmetric oxygen vacancies can enhance the NO x The introduction of rare earth elements can improve the overall redox capacity of the catalyst. At the same time, combined with the highly dispersed MCuO anchored in the molecular sieve framework, x Active sites make it difficult for sulfur dioxide to be chemically adsorbed on the catalyst. The denitration catalyst provided by the present invention has strong Bronsted acid sites and Lewis acid sites, which can increase the catalyst's ability to adsorb NH3 and its ability to resist poisoning by sulfur dioxide.
[0054] (2) The preparation method of the denitration catalyst provided by the present invention is simple and easy to operate, and the denitration catalyst is prepared by adding the molecular sieve raw material and the raw material of the active component together for hydrothermal reaction, and then ion exchange. Since the molecular sieve of the FAU structure has a stable topological structure and low crystal formation energy, it can be successfully crystallized at a lower temperature after adding sodium hydroxide. Therefore, compared with the conventional preparation method in the prior art (such as the synthesis of Cu-SSZ-13, Cu-SAPO-34 and Cu-ZSM-5 molecular sieve catalysts), the step of adding an organic template is omitted, and there is no need to perform a hydrothermal process of more than 12 hours, saving preparation time and cost.
[0055] (3) The denitration catalyst provided by the present invention is used for the selective catalytic reduction of nitrogen oxides by ammonia, and can cover an ultra-wide temperature range of 100-550°C. At the same time, the catalyst has excellent resistance to sulfur dioxide poisoning. BRIEF DESCRIPTION OF THE DRAWINGS
[0056] Figure 1 This is a TEM image of the denitration catalyst described in Example 1 of the present invention. DETAILED DESCRIPTION
[0057] The technical solution of the present invention is further described below in conjunction with the accompanying drawings and through specific implementation methods. However, the following examples are only simplified examples of the present invention and do not represent or limit the scope of protection of the present invention. The scope of protection of the present invention shall be subject to the claims.
[0058] In the following examples, unless otherwise specified, all reagents and consumables were purchased from conventional reagent manufacturers in the field; unless otherwise specified, the experimental methods and technical means used were conventional methods and means in the field.
[0059] Example 1
[0060] This embodiment provides a denitration catalyst, which includes an X-type molecular sieve matrix and a composite oxide active component CeCuO supported on the surface of the X-type molecular sieve matrix. 1.11 ; The silicon-aluminum ratio of the X-type molecular sieve matrix is 1.86:1;
[0061] Based on the total molar amount of silicon element and composite oxide active component in the FAU molecular sieve, the molar fraction of the composite oxide active component is 10%; in the composite oxide active component, the molar ratio of rare earth doping element Ce to copper element is 0.11:1;
[0062] The preparation method of the denitration catalyst provided in this embodiment comprises the following steps:
[0063] (1) 1.216 g of sodium aluminate and 0.08 g of sodium hydroxide were added to 9.5 mL of deionized water, and after stirring evenly, 3.370 g of anhydrous sodium silicate and 8 mL of deionized water were added, followed by 0.473 g of copper nitrate and 0.123 g of cerium nitrate hexahydrate, mixed and stirred for 1 h, allowed to stand for 8 h, and then hydrothermally reacted at 100 ° C for 6 h to obtain the first product.
[0064] (2) The first product was added to 25 mL of 2 mol / L ammonium nitrate solution and stirred at 80° C. for 12 h; then, a new 25 mL of 2 mol / L ammonium nitrate solution was added and stirred at 80° C. for 12 h to obtain the second product.
[0065] (3) The second product was dried at 80° C. for 12 h, placed in a muffle furnace, and calcined at 500° C. for 4 h at a heating rate of 5° C. / min to obtain the denitration catalyst.
[0066] The TEM image of the prepared denitrification catalyst is shown in Figure 1 As shown in the figure, it can be seen that the X-type molecular sieve has a flake morphology with a diameter of about 300nm. In addition, no obvious CeCuO 1.11 The presence of particles indicates that the active component may be highly dispersed in the pores of the molecular sieve.
[0067] Example 2
[0068] This embodiment provides a denitration catalyst, which includes an X-type molecular sieve matrix and a composite oxide active component NdCuO supported on the surface of the X-type molecular sieve matrix. 1.11 ; The silicon-aluminum ratio of the X-type molecular sieve matrix is 1.86:1;
[0069] Based on the total molar amount of silicon element and composite oxide active component in the FAU molecular sieve, the molar fraction of the composite oxide active component is 5%; in the composite oxide active component, the molar ratio of rare earth doping element Nd to copper element is 0.11:1;
[0070] The preparation method of the denitration catalyst provided in this embodiment comprises the following steps:
[0071] (1) 1.216 g of sodium aluminate and 0.03 g of sodium hydroxide were added to 9.5 mL of deionized water, and after stirring evenly, 3.370 g of anhydrous sodium silicate and 8 mL of deionized water were added, followed by 0.237 g of copper nitrate and 0.062 g of neodymium nitrate hexahydrate, and the mixture was stirred for 1 h, allowed to stand for 8 h, and then subjected to hydrothermal reaction at 100 °C for 6 h to obtain the first product.
[0072] (2) The first product was added to 25 mL of 1 mol / L ammonium nitrate solution and stirred at 70° C. for 15 h. This step was repeated twice, with a new ammonium nitrate solution being replaced before each ion exchange. After a total of three ion exchanges, the second product was obtained.
[0073] (3) The second product was dried at 70° C. for 16 h, placed in a muffle furnace, and calcined at 400° C. for 8 h at a heating rate of 2° C. / min to obtain the denitration catalyst.
[0074] Example 3
[0075] This embodiment provides a denitration catalyst, which includes a Y-type molecular sieve matrix and a composite oxide active component CeCuO supported on the surface of the Y-type molecular sieve matrix. 1.2 ; The silicon-aluminum ratio of the Y-type molecular sieve matrix is 3.32:1;
[0076] Based on the total molar amount of silicon element and composite oxide active component in the FAU molecular sieve, the molar fraction of the composite oxide active component is 28%; in the composite oxide active component, the molar ratio of rare earth doping element Ce to copper element is 0.2:1;
[0077] The preparation method of the denitration catalyst provided in this embodiment comprises the following steps:
[0078] (1) 0.608 g of sodium aluminate and 0.12 g of sodium hydroxide were added to 9.5 mL of deionized water, and after stirring evenly, 3.370 g of anhydrous sodium silicate and 8 mL of deionized water were added, followed by 1.208 g of copper nitrate and 0.559 g of cerium nitrate hexahydrate, mixed and stirred for 1 h, allowed to stand for 8 h, and then hydrothermally reacted at 100 ° C for 6 h to obtain the first product.
[0079] (2) The first product was added to 25 mL of 4 mol / L ammonium nitrate solution and stirred at 90° C. for 10 h; then, a new 25 mL of 4 mol / L ammonium nitrate solution was added and stirred at 90° C. for 10 h again to obtain the second product.
[0080] (3) The second product was dried at 90° C. for 10 h, placed in a muffle furnace, and calcined at 600° C. for 4 h at a heating rate of 10° C. / min to obtain the denitration catalyst.
[0081] Example 4
[0082] This embodiment provides a denitration catalyst, which is different from the embodiment 1 only in that when preparing the denitration catalyst, Ce:Cu=0.02:1, and other conditions and parameters are exactly the same as those in the embodiment 1.
[0083] Example 5
[0084] This embodiment provides a denitration catalyst, which is different from the embodiment 1 only in that when preparing the denitration catalyst, Ce:Cu=0.3:1, and other conditions and parameters are exactly the same as those in the embodiment 1.
[0085] Example 6
[0086] This embodiment provides a denitration catalyst, which is different from Embodiment 1 only in that, when preparing the denitration catalyst, the standing time is 4 hours, and other conditions and parameters are exactly the same as those in Embodiment 1.
[0087] Example 7
[0088] This embodiment provides a denitration catalyst, which is different from Embodiment 1 only in that, when preparing the denitration catalyst, the hydrothermal time is 3 hours, and other conditions and parameters are exactly the same as those in Embodiment 1.
[0089] Example 8
[0090] This embodiment provides a denitration catalyst, which is different from Embodiment 1 only in that, when preparing the denitration catalyst, the standing time is 20 hours, and other conditions and parameters are exactly the same as those in Embodiment 1.
[0091] Example 9
[0092] This embodiment provides a denitration catalyst, which is different from Embodiment 1 only in that, when preparing the denitration catalyst, the hydrothermal time is 24 hours, and other conditions and parameters are exactly the same as those in Embodiment 1.
[0093] Example 10
[0094] This embodiment provides a denitration catalyst, which is different from the embodiment 1 only in that the calcination temperature is 300° C. when preparing the denitration catalyst, and the other conditions and parameters are exactly the same as those in the embodiment 1.
[0095] Embodiment 11
[0096] This embodiment provides a denitration catalyst, which is different from the embodiment 1 only in that the calcination temperature is 700° C. when preparing the denitration catalyst, and the other conditions and parameters are exactly the same as those in the embodiment 1.
[0097] Comparative Example 1
[0098] This comparative example provides a denitration catalyst, which is different from Example 1 only in that no cerium nitrate hexahydrate is added when preparing the denitration catalyst, and other conditions and parameters are exactly the same as those in Example 1.
[0099] Comparative Example 2
[0100] This comparative example provides a denitration catalyst, which is different from Example 1 only in that, when preparing the denitration catalyst, copper nitrate is replaced by an equimolar amount of iron nitrate, and other conditions and parameters are exactly the same as those in Example 1.
[0101] Comparative Example 3
[0102] The preparation method of the denitration catalyst provided in this comparative example comprises the following steps:
[0103] (1) Add 0.473 g of copper nitrate and 0.123 g of cerium nitrate hexahydrate (Ce:Cu=0.11:1) to 2.406 g of titanium dioxide powder;
[0104] (2) The above powder was evaporated to dryness at 80°C with stirring, and then placed in a muffle furnace and calcined at 500°C for 4 hours at a heating rate of 5°C / min.
[0105] Performance Testing:
[0106] The catalysts prepared in the above examples and comparative examples were used to conduct denitration activity tests on simulated flue gas. The simulated flue gas contained 500ppm NH3, 500ppm NO, 5% O2, 250ppm SO2, and the balance gas was nitrogen. The above conditions were used to test the NO activity of the catalyst at different temperatures and when 250ppm SO2 was introduced. x Conversion rate, the test results are shown in Table 1:
[0107] Table 1
[0108]
[0109]
[0110] The test results show that:
[0111] (1) It can be seen from Examples 1-3 that the morphology of the FAU molecular sieve matrix is layered and has a strong interlayer mass transfer capacity, which can transfer NO x , NH3 and other gases quickly diffuse to the active sites, and the active component of the composite oxide MCuO x The presence of MO-Cu asymmetric oxygen vacancies can enhance the NO x The introduction of rare earth elements can improve the overall redox capacity of the catalyst. At the same time, combined with the highly dispersed MCuO anchored in the molecular sieve framework, x Active sites make it difficult for sulfur dioxide to be chemically adsorbed on the catalyst. The denitration catalyst provided by the present invention has strong Bronsted acid sites and Lewis acid sites, which can increase the catalyst's ability to adsorb NH3 and its ability to resist poisoning by sulfur dioxide.
[0112] (2) By comparing Example 1 with Examples 4-5, it can be seen that in the denitration catalyst of the present invention, the molar ratio of the rare earth doping element to the copper element will affect the catalytic activity of the catalyst and the ability to resist SO2 poisoning. When the molar ratio of the rare earth doping element to the copper element is controlled at (0.05-0.2):1, the denitration catalyst can maintain high-temperature catalytic activity and excellent low-temperature activity. If the proportion of the rare earth doping element is too low, the high-temperature performance of the catalyst after 300°C decreases. If the proportion of the rare earth doping element is too high, the low-temperature performance of the catalyst before 300°C is poor.
[0113] (3) By comparing Example 1 with Examples 6-9, it can be seen that in the denitration catalyst of the present invention, too short a standing time and a hydrothermal time will affect the crystallinity of the molecular sieve in the catalyst, resulting in incomplete skeleton growth and failure to successfully anchor MCuO x The catalytic performance of the active components under NH3-SCR conditions with or without SO2 decreases accordingly; and if the standing time and hydrothermal time are too long, the cerium source and copper source will be dissolved and enriched on the surface of the molecular sieve, and cannot be dispersed and anchored in the pores, thereby affecting the catalytic performance and anti-poisoning ability of NH3-SCR.
[0114] (4) By comparing Example 1 with Examples 10-11, it can be seen that in the denitration catalyst of the present invention, if the calcination temperature is too high, the molecular sieve framework will collapse, covering the MCuO xActive sites are formed, resulting in the inability of active components to be exposed and contact with reactants such as NO and NH3, leading to reduced catalyst performance; while too low a calcination temperature will lead to a decrease in the crystallinity of the molecular sieve and incomplete skeleton growth, which will greatly reduce the NH3-SCR catalytic performance of the catalyst in the presence of SO2.
[0115] (5) It can be seen from Example 1 and Comparative Examples 1-2 that rare earth elements play an important role in anti-poisoning and enhancing medium and high temperature performance. After the rare earth elements are replaced with other elements such as iron, the NO of the catalyst prepared after passing SO2 gas is x The conversion rate drops significantly, the redox ability of the catalyst decreases, and the medium and high temperature activity also decreases.
[0116] (6) It can be seen from Example 1 and Comparative Example 3 that when conventional titanium dioxide is used as a carrier, the NO x The conversion rate dropped significantly because the active components could not be evenly dispersed on the carrier, so that sulfur dioxide was chemically adsorbed on the catalyst, causing SO2 poisoning of the catalyst. The layered FAU molecular sieve matrix of the present invention has a strong interlayer mass transfer ability, and the highly dispersed MCuO anchored in the molecular sieve framework x Active sites make it difficult for sulfur dioxide to chemically adsorb on the catalyst, and can convert NO x , gases such as NH3 quickly diffuse to the active sites to achieve degradation.
[0117] In summary, the present invention uses FAU molecular sieve with a layered structure as the matrix of the catalyst, and its strong interlayer mass transfer ability can convert NO x , NH3 and other gases quickly diffuse to the active sites, with the composite oxide MCuO x As the active component of the catalyst, there are MO-Cu asymmetric oxygen vacancies in it, which can enhance the NO x The introduction of rare earth elements can improve the overall redox capacity of the catalyst. At the same time, combined with the highly dispersed MCuO anchored in the molecular sieve framework, x Active sites, the catalyst has excellent resistance to sulfur dioxide poisoning in an ultra-wide temperature range of 100-550°C.
[0118] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.
Claims
1. A denitration catalyst, characterized in that: The denitration catalyst comprises a layered FAU molecular sieve matrix and a composite oxide active component loaded on the surface and in the pores of the layered FAU molecular sieve matrix, wherein the chemical formula of the composite oxide active component is MCuO x , M is a rare earth doping element, wherein x is the molar amount of oxygen atoms in the composite oxide, and 1≤x≤2.
2. The denitration catalyst according to claim 1, characterized in that: The layered FAU molecular sieve matrix includes an X-type molecular sieve or a Y-type molecular sieve, preferably an X-type molecular sieve; Preferably, the silicon-aluminum ratio of the layered FAU molecular sieve matrix is (1-30):1; Preferably, based on the total molar amount of silicon element and composite oxide active component in the FAU molecular sieve, the molar fraction of the composite oxide active component is 5-30%, preferably 10-25%; Preferably, in the composite oxide active component, the molar ratio of the rare earth doping element to the copper element is (0.05-0.2):1; Preferably, the rare earth doping element includes any one of cerium, neodymium, samarium, cobalt, europium, yttrium, dysprosium, ytterbium, lanthanum or praseodymium, or a combination of at least two thereof.
3. A method for preparing a denitration catalyst as claimed in claim 1 or 2, characterized in that: The preparation method comprises the following steps: Aluminum source, sodium hydroxide, silicon source, rare earth doping element source, copper source and water are mixed and stirred, and then subjected to hydrothermal reaction to obtain a first product; the first product is mixed with ammonium nitrate solution to perform ion exchange to obtain a second product; the second product is dried and calcined to obtain the denitration catalyst.
4. The preparation method according to claim 3, characterized in that: The silicon source includes sodium silicate; Preferably, the aluminum source comprises sodium metaaluminate; Preferably, the rare earth doping element source includes any one of cerium nitrate hexahydrate, neodymium nitrate, samarium nitrate, cobalt nitrate, europium nitrate, yttrium nitrate, dysprosium nitrate, ytterbium nitrate, lanthanum nitrate or praseodymium nitrate, or a combination of at least two thereof; Preferably, the copper source comprises copper nitrate.
5. The preparation method according to claim 3 or 4, characterized in that: The molar ratio of the sodium hydroxide to the aluminum element in the aluminum source is 1:(5-10); Preferably, the stirring time is 1-2h; Preferably, the stirred mixture is allowed to stand before the hydrothermal reaction; Preferably, the standing time is 6-10h; Preferably, the hydrothermal reaction time is 4-8h; Preferably, the hydrothermal reaction temperature is 100-120°C; Preferably, the concentration of the ammonium nitrate solution is 1-4 mol / L; Preferably, the mass ratio of the first product to the ammonium nitrate solution is 1:(15-30); Preferably, the ion exchange temperature is 60-100°C; Preferably, the ion exchange time is 8-15h; Preferably, the ion exchange is repeated 1-3 times.
6. The preparation method according to any one of claims 3 to 5, characterized in that: The drying temperature is 70-90°C; Preferably, the drying time is 8-16 hours; Preferably, the calcination temperature is 400-600°C; Preferably, the heating rate of the calcination is 1-10°C / min; Preferably, the calcination time is 3-10 hours.
7. A use of the denitration catalyst as claimed in claim 1 or 2, characterized in that: The denitration catalyst is used for the selective catalytic reduction of nitrogen oxides by ammonia.
8. The use of the denitration catalyst according to claim 8, characterized in that: The working temperature of the catalyst is 100-550°C, preferably 150-400°C.
9. A denitration reactor, characterized in that: The denitration reactor comprises the denitration catalyst as claimed in claim 1 or 2.
10. A denitration device, characterized in that: The denitration device comprises the denitration reactor according to claim 9; The denitration device includes a mobile source gas denitration device and / or a fixed source gas denitration device.
Citation Information
Patent Citations
Low-temperature denitrated CeO2-NaX molecular sieve catalyst and preparation method thereof
CN102814191A
Confined molecular sieve denitrification catalyst and preparation method thereof
CN109433254A
Denitration catalyst, method for preparing same and application of denitration catalyst
CN109746025A
Preparation method and application of denitration catalyst
CN114054074A
Wide-temperature vanadium-free denitration catalyst as well as preparation method and application thereof
CN114247465A
Cited By
Low-temperature rare earth-based denitration catalyst with nano synapse structure as well as preparation method and application of low-temperature rare earth-based denitration catalyst