Device and method for preparing catalyst nanoparticles, single-walled carbon nanotubes, and device and method for macro synthesis of single-walled carbon nanotubes

Through a multi-step chemical gas phase synthesis process, the preheating of the sheath mixed gas and the carbon source mixed gas is successfully achieved by successfully achieving the generation of catalyst nanoparticle flow with high volume concentration and narrow diameter distribution, solving the yield of single-wall carbon nanotubes and the problem of insufficient dimensional uniformity, macro synthesis of Nissan kilograms and preparation of single-wall carbon nanotubes with high crystallinity are achieved.

CN119034825AActive Publication Date: 2024-11-29JIANGXI COPPER TECHNOLOGY RESEARCH INSTITUTE CO LTD

Patent Information

Application Number
CN202411370059.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-29
Publication Date
2024-11-29
Estimated Expiration
2044-09-29

AI Technical Summary

Technical Problem

The prior art is difficult to achieve the preparation of single-wall carbon nanotubes with high yield and narrow diameter distribution, especially in macro synthesis at the level of kilograms above the daily kilogram level, the concentration and size distribution of catalyst nanoparticles are difficult to effectively control, resulting in uniform yield and size. Insufficient sex.

Method used

Using a multi-step chemical vapor phase synthesis process, the catalyst and condenser inhibitor are mixed in the evaporator and steam is formed, and then ionized in the microplasma reactor to form a stream of catalyst nanoparticles, and the sheath mixed gas is used to reduce it in the reaction chamber. Or oxidation prevents collision and aggregation between catalyst nanoparticles, thereby obtaining a high volume concentration and narrow diameter distribution of catalyst nanoparticles, and then reacts with the carbon source mixed gas under suitable temperature and time conditions to synthesize a controlled diameter Single-walled carbon nanotubes.

Benefits of technology

It has achieved the generation of catalyst nanoparticle streams with preferred size distribution under extremely high volume concentration conditions, overcome the problems of single-wall carbon nanotubes in terms of yield and size uniformity, and achieved macro synthesis of daily kilograms, and the catalyst nanometers are The uniformity and stability of the particles are guaranteed.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119034825A_ABST
    Figure CN119034825A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation device and method of catalyst nanoparticles, a single-walled carbon nanotube and a macro synthesis device and method of the single-walled carbon nanotube. The device is composed of a catalyst preparation unit, a growth unit and a product collection unit, the catalyst preparation unit is integrated with a micro-plasma reactor, a catalyst and coagulant inhibitor carrier gas preheater, a conveyor and an evaporator, and efficient and fine catalyst preparation is formed. A preheated argon flow, continuously flowing micro-plasma, a preheated sheath mixed gas curtain and a preheated carbon source mixed gas curtain are utilized, and a multi-step chemical vapor phase process is adopted to perform fine structure regulation and control on an iron catalyst, so that concentrated generation of iron nano particle flows with narrow sizes distributed at-1.5 nm and-3.5 nm under the condition of nano particles with high volume concentration is successfully realized; by using the iron nanoparticles, the single-walled carbon nanotubes with high crystallinity and narrow diameter distribution can be synthesized, and macro synthesis of kilogram-level daily output can be realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention particularly relates to a device and method for preparing catalyst nanoparticles, a device and method for synthesizing single-walled carbon nanotubes and a macro-scale synthesis thereof, and belongs to the technical field of nano material preparation. Background Art

[0002] Single-walled carbon nanotubes (SWCNTs) have unique morphological, physical and mechanical properties such as high aspect ratio and high flexibility, making them high-performance conductive and reinforcing materials. Single-walled carbon nanotubes establish a strong and long-range conductive network structure between active material particles, which has become a key feature of lithium batteries, such as improved cycle life, improved rate performance and cohesion between active materials. This is especially important for silicon-containing negative electrode systems with high volume expansion. Single-walled carbon nanotubes can greatly alleviate the degradation problem and effectively promote the industrial application of silicon as a high-capacity negative electrode active material. However, how to achieve the preparation of SWCNTs has always been a key factor restricting its development.

[0003] Floating chemical vapor deposition (FCCVD) is a common method for synthesizing single-walled carbon nanotubes. A solution of a catalyst precursor and a hydrocarbon is fed into a heated reaction vessel, where the catalyst precursor is heated and decomposed. As the carrier gas enters a temperature zone suitable for the decomposition of hydrocarbons, the nucleation and growth of carbon nanotubes are carried out, but it has been difficult to break through the kilogram-level production per day. Jung et al. reduced the concentration of the catalyst in the catalyst precursor solution, and although they were able to obtain highly crystalline SWCNTs with a G / D ratio of 62.5, they sacrificed the yield. High yield and size uniformity are obstacles that are difficult to overcome at the same time, and the amount of the product is difficult to break through the 100-gram level per day (Chemical Engineering Journal 228 (2013) 1050-1056). Mordkovich et al. increased the reaction zone diameter to 324 mm and the reaction zone length to 5 meters by expanding the volume of the reactor to extend the reaction time. Although the reaction space and time required for the catalyst were increased, the maximum yield of the initial product was 72 g / day, and the purity was between 25-50%, which was still a long way from the kilogram level per day (Diamond & Related Materials 83 (2018) 15-20). The reason is that FCCVD cannot obtain nanocatalyst particles with sufficient concentration and narrow size distribution, so it is difficult to form a large amount of single-walled carbon nanotubes. This is also the core factor that single-walled carbon nanotubes are difficult to achieve ton-level preparation (Diamond & Related Materials 83 (2018) 15-20, Materials Today: Proceedings 5 ​​(2018) 25951-25955, Carbon 146 (2019) 789-812). Sawyer et al. used a customized microplasma reactor to evaporate iron nanoparticles with a narrow size distribution of 3 nm (Journal of AerosolScience 161 (2022) 105915). Although it shows that microplasma can effectively produce small-sized nanoparticles, how to obtain high concentrations remains a problem. Summary of the invention

[0004] The main purpose of the present invention is to provide a device and method for preparing catalyst nanoparticles, a device and method for synthesizing single-walled carbon nanotubes and large quantities thereof, so as to overcome the deficiencies in the prior art.

[0005] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention includes: A first aspect of an embodiment of the present invention provides a method for preparing catalyst nanoparticles with high volume concentration and narrow diameter distribution, comprising: Introducing a catalyst and an anticoagulant into an evaporator, and mixing and evaporating the catalyst and the anticoagulant in the evaporator to form a catalyst precursor vapor; Introducing the catalyst precursor vapor into a micro plasma reactor to ionize it to form a first catalyst nanoparticle flow, and delivering the first catalyst nanoparticle flow into a reaction chamber having a second temperature at a first flow rate; A sheath mixed gas is input into the reaction chamber, and the sheath mixed gas surrounds the first catalyst nanoparticle flow and maintains a second flow rate, the catalyst nanoparticles in the first catalyst nanoparticle flow are reduced or oxidized by the sheath mixed gas, and the sheath mixed gas quickly diffuses to the central area of ​​the first catalyst nanoparticle flow and prevents collision and aggregation between the catalyst nanoparticles, thereby obtaining a second catalyst nanoparticle flow, wherein the particle size distribution range of the catalyst nanoparticles contained in the second catalyst nanoparticle flow is smaller than the particle size distribution range of the catalyst nanoparticles contained in the first catalyst nanoparticle flow.

[0006] A second aspect of an embodiment of the present invention provides a method for synthesizing large quantities of single-walled carbon nanotubes with controllable diameters, comprising: Under the second temperature condition, the catalyst nanoparticles have a particle size of 1 nm to 6 nm and a concentration of not less than 2×10 16 cm -3 The catalyst nanoparticle flow and the carbon source mixed gas are mixed and reacted within 1 millisecond to 10 milliseconds to obtain single-walled carbon nanotubes with controllable diameter.

[0007] A third aspect of the embodiments of the present invention provides a single-walled carbon nanotube, which is prepared by the method for macro-synthesis of single-walled carbon nanotubes with controllable diameters.

[0008] A fourth aspect of an embodiment of the present invention provides a device for preparing catalyst nanoparticles with high volume concentration and narrow diameter distribution, comprising: A catalyst supply mechanism, an anticoagulant supply mechanism, an evaporator, a microplasma generator, a sheath mixed gas supply mechanism and a reaction mechanism, wherein the catalyst supply mechanism and the anticoagulant supply mechanism are connected to the evaporator respectively, the evaporator is connected to the microplasma generator, the reaction mechanism comprises a reaction chamber, a heating mechanism, a catalyst nanoparticle flow injection port and a sheath mixed gas air curtain injection port communicated with the reaction chamber, the sheath mixed gas air curtain injection port is arranged around the catalyst nanoparticle flow injection port, the microplasma generator is connected to the catalyst nanoparticle flow injection port, the sheath mixed gas supply mechanism is connected to the sheath mixed gas air curtain injection port, and the heating mechanism is used to maintain the ambient temperature in the reaction chamber at a second temperature; The catalyst supply mechanism is used to preheat the catalyst and introduce the catalyst into the evaporator, the anticoagulant supply mechanism is used to preheat the catalyst and introduce the anticoagulant into the evaporator, the evaporator is used to evaporate and mix the introduced catalyst and anticoagulant to form a catalyst precursor vapor, the microplasma generator is used to decompose the catalyst precursor vapor to form a first catalyst nanoparticle flow, and introduce the first catalyst nanoparticle flow into the reaction chamber, the sheath mixed gas supply mechanism is used to preheat the sheath mixed gas and introduce the sheath mixed gas into the reaction chamber, the sheath mixed gas is distributed around the catalyst nanoparticle flow, and the sheath mixed gas can reduce or oxidize the catalyst nanoparticle flow, and the sheath mixed gas can quickly diffuse to the central area of ​​the catalyst nanoparticle flow and prevent collision and aggregation between catalyst nanoparticles.

[0009] A fifth aspect of an embodiment of the present invention provides a device for macro-scale synthesis of single-walled carbon nanotubes with controllable diameters, comprising: A catalyst nanoparticle preparation unit comprises a catalyst supply mechanism, an anticoagulant supply mechanism, an evaporator, and a microplasma generator, wherein the catalyst supply mechanism and the anticoagulant supply mechanism are respectively connected to the evaporator, and the evaporator is connected to the microplasma generator. The catalyst supply mechanism is used to preheat the catalyst and introduce the catalyst into the evaporator, the anticoagulant supply mechanism is used to preheat the catalyst and introduce the anticoagulant into the evaporator, the evaporator is used to evaporate and mix the introduced catalyst and anticoagulant to form catalyst precursor vapor, and the microplasma generator is used to decompose the catalyst precursor vapor to form a first catalyst nanoparticle flow, and introduce the first catalyst nanoparticle flow into a reaction chamber; The reaction unit comprises a carbon source mixed gas supply mechanism, a sheath mixed gas supply mechanism and a reaction mechanism, wherein the reaction mechanism comprises a reaction chamber, a heating mechanism and a catalyst nanoparticle flow injection port, a sheath mixed gas air curtain injection port and a carbon source mixed gas injection port which are connected to the reaction chamber, wherein the sheath mixed gas air curtain injection port is arranged around the catalyst nanoparticle flow injection port, the micro plasma generator is connected to the catalyst nanoparticle flow injection port, the sheath mixed gas supply mechanism is connected to the sheath mixed gas air curtain injection port, the carbon source mixed gas supply mechanism is connected to the carbon source mixed gas injection port, and the heating mechanism The structure is used to maintain the ambient temperature in the reaction chamber at a second temperature, the sheath mixed gas supply mechanism is used to preheat the sheath mixed gas and introduce the sheath mixed gas into the reaction chamber, the carbon source mixed gas supply mechanism is used to preheat the carbon source mixed gas and introduce the carbon source mixed gas into the reaction chamber, the sheath mixed gas is distributed around the catalyst nanoparticle flow, and the sheath mixed gas can reduce or oxidize the catalyst nanoparticle flow, and the sheath mixed gas can quickly diffuse to the central area of ​​the catalyst nanoparticle flow and prevent collision and aggregation between catalyst nanoparticles.

[0010] Compared with the prior art, the advantages of the present invention include: The present invention successfully achieved the synthesis of nanoparticles with extremely high volume concentration (more than 2×10 16 cm -3 ) conditions, a stream of catalyst nanoparticles with an optimal size distribution not exceeding 6 nm was generated in a concentrated manner. This innovative breakthrough effectively overcomes the difficulties faced by highly crystalline single-walled carbon nanotubes in terms of narrow diameter distribution and yield, and opens up new paths for the development of related fields.

[0011] The present invention preheats the carrier gas, sheath mixed gas and carbon source mixed gas, which not only reduces the heating load of the reactor, but also avoids the increase of the concentration of catalyst nanoparticles. At the same time, the introduction of preheating gas also reduces unnecessary collisions between catalyst nanoparticles, thereby effectively inhibiting the excessive growth of catalyst nanoparticles and ensuring the uniformity and stability of the catalyst nanoparticles.

[0012] The present invention uses a preheated carrier gas, a continuously flowing micro plasma, a preheated sheath mixed gas curtain and a carbon source mixed gas curtain, and adopts a multi-step chemical vapor phase process to finely control the structure of the iron catalyst, and successfully achieves the nanoparticles with high volume concentration (more than 2×10 16 cm -3 ) conditions, a concentrated stream of iron nanoparticles with narrow size distributions of ~1.5 nm and ~3.5 nm was generated, as shown in Fig.10Statistical results in . Furthermore, using these catalyst nanoparticles, single-walled carbon nanotubes with high crystallinity and narrow diameter distribution (particle sizes are mainly concentrated in 1.13nm~1.54nm, 0.86nm~0.94nm, and average particles are concentrated in 1.30nm, 0.91nm) can be synthesized, and macro-scale synthesis with a daily output of kilograms can be achieved. The present invention shows significant advantages in the macro-scale preparation of single-walled carbon nanotubes with controllable diameters, and has great commercial value and broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] Figure 1 This is a schematic diagram of the structure of a device for macro-synthesis of single-walled carbon nanotubes using microplasma provided in a typical embodiment of the present invention; Figure 2 A partial cross-sectional view of a portion of a catalyst preparation unit and a growth unit provided in a typical implementation case of the present invention; Figure 3 A schematic diagram of the principle of a microplasma macro-synthesis of single-walled carbon nanotubes provided in a typical embodiment of the present invention; Figure 4 Thermogravimetric characterization diagram of single-walled carbon nanotubes prepared by the device of the present invention in Example 1 of the present invention; Figure 5 This is a scanning electron microscope image of the single-walled carbon nanotubes prepared in Example 3 of the present invention; Figure 6 This is a Raman spectrum of the single-walled carbon nanotubes prepared in Example 5 of the present invention; Figure 7 This is a local Raman spectrum of the RBM characteristic peak of the single-walled carbon nanotube prepared in Example 5 of the present invention; Figure 8 This is a transmission electron microscope image of the single-walled carbon nanotube prepared in Example 5 of the present invention; Fig. 9 This is a transmission electron microscope image of the single-walled carbon nanotube prepared in Example 5 of the present invention; Fig.10 The diameter distribution statistics of iron nanoparticles and SWCNTs were measured by transmission electron microscopy for the samples prepared in Example 5 of the present invention. DETAILED DESCRIPTION

[0014] In view of the deficiencies in the prior art, the inventor of this case has proposed the technical solution of the present invention after long-term research and extensive practice. The technical solution, its implementation process and principle will be further explained as follows.

[0015] A first aspect of an embodiment of the present invention provides a method for preparing catalyst nanoparticles with high volume concentration and narrow diameter distribution, comprising: Introducing a catalyst and an anticoagulant into an evaporator, and mixing and evaporating the catalyst and the anticoagulant in the evaporator to form a catalyst precursor vapor; Introducing the catalyst precursor vapor into a micro plasma reactor to ionize it to form a first catalyst nanoparticle flow, and delivering the first catalyst nanoparticle flow into a reaction chamber having a second temperature at a first flow rate; A sheath mixed gas is input into the reaction chamber, and the sheath mixed gas surrounds the first catalyst nanoparticle flow and maintains a second flow rate, the catalyst nanoparticles in the first catalyst nanoparticle flow are reduced or oxidized by the sheath mixed gas, and the sheath mixed gas quickly diffuses to the central area of ​​the first catalyst nanoparticle flow and prevents collision and aggregation between the catalyst nanoparticles, thereby obtaining a second catalyst nanoparticle flow, wherein the particle size distribution range of the catalyst nanoparticles contained in the second catalyst nanoparticle flow is smaller than the particle size distribution range of the catalyst nanoparticles contained in the first catalyst nanoparticle flow.

[0016] In a more specific embodiment, the method for preparing catalyst nanoparticles with high volume concentration and narrow diameter distribution specifically comprises: The catalyst and the anticoagulant are introduced into the evaporator respectively by using a carrier gas with a first temperature, wherein the first temperature is 100° C. to 500° C.

[0017] Furthermore, the flow rate of the carrier gas is 0.05 L / min to 15 L / min.

[0018] Furthermore, the carrier gas includes an inert gas, and the inert gas is selected from at least one of argon, nitrogen, and helium, preferably argon.

[0019] Furthermore, the first flow velocity is greater than 5 m / s.

[0020] Furthermore, the first flow velocity is 5 m / s to 12 m / s.

[0021] Furthermore, the second temperature is 800°C to 1800°C.

[0022] Furthermore, the catalyst precursor vapor volume concentration is 3×10 15 cm -3 ~9×10 18 cm -3 .

[0023] Furthermore, the particle size of the catalyst precursor particles contained in the catalyst precursor vapor is 1 nm to 600 nm.

[0024] In a more specific embodiment, the method for preparing catalyst nanoparticles with high volume concentration and narrow diameter distribution specifically comprises: The sheath mixed gas is firstly preheated to a third temperature, and then the sheath mixed gas is introduced into the reaction chamber.

[0025] Furthermore, the third temperature is 300°C to 1200°C.

[0026] Furthermore, the second flow velocity is 3 m / s~90 m / s.

[0027] Furthermore, the particle size of the catalyst nanoparticles in the first catalyst nanoparticle flow is 1 nm to 12 nm, and the concentration is not less than 2×10 16 cm -3 The particle size of the catalyst nanoparticles in the second catalyst nanoparticle flow is 1 nm to 6 nm, and the concentration is not less than 2×10 16 cm -3 .

[0028] Furthermore, the concentration of the catalyst nanoparticles in the first catalyst nanoparticle flow is 2×10 16 cm -3 ~9×10 20 cm -3 , the concentration of the catalyst nanoparticles in the second catalyst nanoparticle flow is 2×10 16 cm -3 ~9×10 22 cm -3 .

[0029] Furthermore, the particle sizes of the catalyst nanoparticles in the second catalyst nanoparticle flow are concentrated in the range of 1 nm to 2 nm and 3.2 nm to 4 nm. Furthermore, the average particle sizes of the catalyst nanoparticles in the second catalyst nanoparticle flow are 1.5 nm and 3.5 nm.

[0030] Furthermore, the catalyst includes an organic substance containing iron, the anticoagulant includes a compound or mixture containing sulfur, and the sheath mixed gas includes a reducing gas and water vapor or oxygen. The reducing gas in the sheath mixed gas has a reducing effect on the one hand, and on the other hand, the reducing gas also has a synergistic effect with water vapor or oxygen, and has the effects of oxidation, reduction and etching, and can etch the catalyst nanoparticles in the first catalyst nanoparticle flow to further reduce the particle size of the catalyst nanoparticles, and at the same time, prevent the catalyst nanoparticles in the first catalyst nanoparticle flow from further colliding and growing, and remove the amorphous carbon in the first catalyst nanoparticle flow, thereby improving the purity of the product.

[0031] Furthermore, the molar ratio of the iron element in the catalyst to the sulfur element in the flocculant is 2:1 to 60:1.

[0032] Furthermore, the catalyst includes ferrocene and the like.

[0033] Furthermore, the anticoagulant includes at least one of thiophene, dimethyl sulfoxide, sulfur powder, hydrogen sulfide, and sulfur dioxide, or a combination of two or more thereof, but is not limited thereto.

[0034] Furthermore, the reducing gas in the sheath mixed gas includes at least one of hydrogen, carbon monoxide, and ammonia, but is not limited thereto.

[0035] Furthermore, the volume ratio of the reducing gas to the water vapor or the oxygen is 10:1 to 90:1.

[0036] A second aspect of an embodiment of the present invention provides a method for synthesizing large quantities of single-walled carbon nanotubes with controllable diameters, comprising: Under the second temperature condition, the catalyst nanoparticles have a particle size of 1 nm to 6 nm and a concentration of not less than 2×10 16 cm -3 The catalyst nanoparticle flow and the carbon source mixed gas are mixed and reacted within 1 millisecond to 10 milliseconds to obtain single-walled carbon nanotubes with controllable diameter.

[0037] Furthermore, the concentration of the catalyst nanoparticles in the catalyst nanoparticle flow is 2×10 16 cm -3 ~9×10 22 cm -3 .

[0038] Furthermore, the catalyst nanoparticle stream is a second catalyst nanoparticle stream formed by the method for preparing catalyst nanoparticles with high volume concentration and narrow diameter distribution.

[0039] In a more specific embodiment, the method for macro-synthesizing single-walled carbon nanotubes with controllable diameters specifically comprises: The catalyst nanoparticle stream is formed by using the method for preparing catalyst nanoparticles with high volume concentration and narrow diameter distribution; A carbon source mixed gas with a fourth temperature is introduced into the reaction chamber, the carbon source mixed gas is maintained at a third flow rate, and the carbon source mixed gas and the catalyst nanoparticle flow are mixed and reacted within 1 millisecond to 10 milliseconds.

[0040] In a more specific embodiment, the method for macro-synthesizing single-walled carbon nanotubes with controllable diameters specifically comprises: The carbon source mixed gas is first preheated to a fourth temperature, and then the carbon source mixed gas is introduced into the reaction chamber.

[0041] Furthermore, the fourth temperature is 230°C to 650°C.

[0042] Furthermore, the third flow velocity is 3 m / s~90 m / s.

[0043] Furthermore, the carbon source mixed gas includes a carbon source gas and a reducing gas.

[0044] Furthermore, the volume ratio of the carbon source gas to the reducing gas is 1:(1-50).

[0045] Furthermore, the flow ratio of the carbon source gas contained in the carbon source mixed gas to the reducing gas contained in the sheath mixed gas is 1:(2-35).

[0046] Further, the carbon source gas includes at least one of natural gas, methane, ethane, propane, butane, pentane, hexane, ethylene, propylene, ethanol, anthracene or anthracene oil vapor, but is not limited thereto.

[0047] Furthermore, the reducing gas contained in the carbon source mixed gas includes at least one of hydrogen, carbon monoxide, and ammonia, but is not limited thereto.

[0048] A third aspect of the embodiments of the present invention provides a single-walled carbon nanotube, which is prepared by the method for macro-synthesis of single-walled carbon nanotubes with controllable diameters.

[0049] Furthermore, the G / D ratio of the single-walled carbon nanotube is greater than 50.

[0050] Furthermore, the diameters of the single-walled carbon nanotubes are mainly concentrated in the range of 1.13 nm to 1.54 nm and 0.86 nm to 0.94 nm, and the average diameter is mainly concentrated in the range of 1.30 nm or 0.91 nm.

[0051] A fourth aspect of an embodiment of the present invention provides a device for preparing catalyst nanoparticles with high volume concentration and narrow diameter distribution, comprising: A catalyst supply mechanism, an anticoagulant supply mechanism, an evaporator, a microplasma generator, a sheath mixed gas supply mechanism and a reaction mechanism, wherein the catalyst supply mechanism and the anticoagulant supply mechanism are connected to the evaporator respectively, the evaporator is connected to the microplasma generator, the reaction mechanism comprises a reaction chamber, a heating mechanism, a catalyst nanoparticle flow injection port and a sheath mixed gas air curtain injection port communicated with the reaction chamber, the sheath mixed gas air curtain injection port is arranged around the catalyst nanoparticle flow injection port, the microplasma generator is connected to the catalyst nanoparticle flow injection port, the sheath mixed gas supply mechanism is connected to the sheath mixed gas air curtain injection port, and the heating mechanism is used to maintain the ambient temperature in the reaction chamber at a second temperature; The catalyst supply mechanism is used to preheat the catalyst and introduce the catalyst into the evaporator, the anticoagulant supply mechanism is used to preheat the catalyst and introduce the anticoagulant into the evaporator, the evaporator is used to evaporate and mix the introduced catalyst and anticoagulant to form a catalyst precursor vapor, the microplasma generator is used to decompose the catalyst precursor vapor to form a first catalyst nanoparticle flow, and introduce the first catalyst nanoparticle flow into the reaction chamber, the sheath mixed gas supply mechanism is used to preheat the sheath mixed gas and introduce the sheath mixed gas into the reaction chamber, the sheath mixed gas is distributed around the catalyst nanoparticle flow, and the sheath mixed gas can reduce or oxidize the catalyst nanoparticle flow, and the sheath mixed gas can quickly diffuse to the central area of ​​the catalyst nanoparticle flow and prevent collision and aggregation between catalyst nanoparticles.

[0052] Furthermore, the catalyst supply mechanism includes a catalyst carrier gas preheater and a catalyst conveyor, the catalyst carrier gas preheater and the catalyst conveyor are connected in sequence, and the catalyst conveyor is connected to the evaporator; the anticoagulant supply mechanism includes an anticoagulant carrier gas preheater and an anticoagulant conveyor, the anticoagulant carrier gas preheater and the anticoagulant conveyor are connected in sequence, and the anticoagulant conveyor is connected to the evaporator.

[0053] A fifth aspect of an embodiment of the present invention provides a device for macro-scale synthesis of single-walled carbon nanotubes with controllable diameters, comprising: A catalyst nanoparticle preparation unit comprises a catalyst supply mechanism, an anticoagulant supply mechanism, an evaporator, and a microplasma generator, wherein the catalyst supply mechanism and the anticoagulant supply mechanism are respectively connected to the evaporator, and the evaporator is connected to the microplasma generator. The catalyst supply mechanism is used to preheat the catalyst and introduce the catalyst into the evaporator, the anticoagulant supply mechanism is used to preheat the catalyst and introduce the anticoagulant into the evaporator, the evaporator is used to evaporate and mix the introduced catalyst and anticoagulant to form catalyst precursor vapor, and the microplasma generator is used to decompose the catalyst precursor vapor to form a first catalyst nanoparticle flow, and introduce the first catalyst nanoparticle flow into a reaction chamber; The reaction unit comprises a carbon source mixed gas supply mechanism, a sheath mixed gas supply mechanism and a reaction mechanism, wherein the reaction mechanism comprises a reaction chamber, a heating mechanism and a catalyst nanoparticle flow injection port, a sheath mixed gas air curtain injection port and a carbon source mixed gas injection port which are connected to the reaction chamber, wherein the sheath mixed gas air curtain injection port is arranged around the catalyst nanoparticle flow injection port, the micro plasma generator is connected to the catalyst nanoparticle flow injection port, the sheath mixed gas supply mechanism is connected to the sheath mixed gas air curtain injection port, the carbon source mixed gas supply mechanism is connected to the carbon source mixed gas injection port, and the heating mechanism The structure is used to maintain the ambient temperature in the reaction chamber at a second temperature, the sheath mixed gas supply mechanism is used to preheat the sheath mixed gas and introduce the sheath mixed gas into the reaction chamber, the carbon source mixed gas supply mechanism is used to preheat the carbon source mixed gas and introduce the carbon source mixed gas into the reaction chamber, the sheath mixed gas is distributed around the catalyst nanoparticle flow, and the sheath mixed gas can reduce or oxidize the catalyst nanoparticle flow, and the sheath mixed gas can quickly diffuse to the central area of ​​the catalyst nanoparticle flow and prevent collision and aggregation between catalyst nanoparticles.

[0054] Furthermore, the catalyst supply mechanism includes a catalyst carrier gas preheater and a catalyst conveyor, the catalyst carrier gas preheater and the catalyst conveyor are connected in sequence, and the catalyst conveyor is connected to the evaporator; the anticoagulant supply mechanism includes an anticoagulant carrier gas preheater and an anticoagulant conveyor, the anticoagulant carrier gas preheater and the anticoagulant conveyor are connected in sequence, and the anticoagulant conveyor is connected to the evaporator.

[0055] Furthermore, the device for macro-synthesis of single-walled carbon nanotubes with controllable diameter also includes: a product collection unit, which is connected to the reaction chamber and is used to perform gas-solid separation on the generated single-walled carbon nanotubes and realize continuous collection.

[0056] The technical solution, its implementation process and principles will be further explained below in conjunction with the accompanying drawings and specific implementation cases. Unless otherwise specified, the functional devices and processes used in the embodiments of the present invention are known in the art.

[0057] In a typical implementation, see Figure 1 and Figure 2 A device for synthesizing single-walled carbon nanotubes in large quantities by microplasma, comprising a catalyst preparation unit 110, a reaction unit 220 and a collection unit 330, wherein the product collection unit 330 is connected to one end of the growth unit 220, and the other end of the growth unit 220 is connected to the catalyst preparation unit 110, wherein the catalyst preparation unit 110 is mainly used to synthesize catalyst nanoparticles with a particle size of 1 nm to 12 nm and a concentration of not less than 2×10 16 cm -3 The reaction unit 220 is mainly used to provide the temperature and space required for synthesizing a catalyst nanoparticle flow with a high concentration and a narrow diameter distribution (i.e., a second catalyst nanoparticle flow) and the temperature and space required for the growth of highly crystalline single-walled carbon nanotubes, so as to convert the first catalyst nanoparticle flow into catalyst nanoparticles with a particle size of 1 nm to 6 nm and a concentration of not less than 2×10 16 cm -3 The second catalyst nanoparticle flow is provided, and the second catalyst nanoparticle flow is reacted with the carbon source mixed gas to synthesize single-walled carbon nanotubes in large quantities. The collecting unit 330 is used to collect the synthesized single-walled carbon nanotubes.

[0058] Specifically, the catalyst preparation unit 110 includes a catalyst carrier gas preheater 111, an anticoagulant carrier gas preheater 112, two conveyors 115, an evaporator 117 and a micro plasma reactor 120. The catalyst carrier gas preheater 111 and the anticoagulant carrier gas preheater 112 are respectively connected to the evaporator 117 via a conveyor 115, and the evaporator 117 is also connected to the micro plasma reactor 120. The growth unit 220 includes a high-temperature growth tube 211, a sheath mixed gas air curtain injection port 223 and a carbon source mixed gas air curtain injection port 225. The high-temperature growth tube 211 has a reaction chamber inside, and the sheath mixed gas curtain injection port 223 is provided with a reaction chamber. The combined gas curtain injection port 223 and the carbon source mixed gas curtain injection port 225 are both connected to the reaction chamber, the micro plasma generator 120 is connected to the high temperature growth tube 211, the sheath mixed gas curtain injection port 223 and the micro plasma generator 120 are coaxially arranged, one end of the micro plasma generator 120 is inserted into the interior of the high temperature growth tube 211, and the other end is connected to the evaporator 117; the product collection unit 300 includes a collection chamber 331, a transition chamber 333, and an exhaust port 335, and the collection chamber 331 is respectively connected to the transition chamber 333, the exhaust port 335 and the growth chamber in the high temperature growth tube 211.

[0059] It should be noted that the catalyst carrier gas preheater 111, the anticoagulant carrier gas preheater 112, the two conveyors 115, the evaporator 117 and the micro plasma reactor 120 used in the present invention are all functional devices known in the art, which can be obtained by commercial purchase or custom processing known in the art, and their specific structures and product models are not limited here. Exemplarily, the micro plasma reactor 120 includes a power supply, an inner electrode, a hollow alumina tube and a curled outer electrode, the curled outer electrode is curled around the hollow alumina tube, the inner electrode is embedded in the hollow alumina tube, the inner electrode diameter is 0.15mm~0.6mm tungsten rod, the curled outer electrode diameter is 0.10mm~0.6mm tantalum wire, the curled outer electrode is coiled around the hollow alumina tube 8~30 times, the power supply parameters are 10W~160W, 350MHz~550 MHz ultra-high frequency power supply. The growth tube 221 may be heated by one or more of electric heating, induction heating, and arc heating.

[0060] In a typical implementation case, a method for preparing a large amount of single-walled carbon nanotubes with controllable diameter using a microplasma large-scale synthesis device for single-walled carbon nanotubes may include the following steps: S1) placing a catalyst and an anticoagulant in a conveyor 115 respectively, and introducing an inert gas to evacuate the entire device; preheating the carrier gas, sheath mixed gas, and carbon source mixed gas with a catalyst carrier gas preheater 111, an anticoagulant carrier gas preheater 112, a sheath mixed gas preheater, and a carbon source mixed gas preheater respectively, so as to preheat the temperatures of the carrier gas, sheath mixed gas, and carbon source mixed gas to 100°C~500°C, 300°C~1200°C, and 230°C~650°C, respectively.

[0061] The catalyst is an organic matter containing iron, and the anticoagulant contains a sulfur compound or a mixture, wherein the molar ratio of iron to sulfur is 2:1~60:1, and illustratively, the catalyst is ferrocene; the anticoagulant is thiophene, dimethyl sulfoxide, sulfur powder, hydrogen sulfide, sulfur dioxide or other sulfur-containing compounds or mixtures; specifically, the carrier gas is argon, and the flow rate of the carrier gas is 0.05 L / min~15L / min; the sheath mixed gas contains reducing gas and other gases, and the inlet flow rate of the sheath mixed gas is 3 m / s~90m / s; the flow ratio of the carbon source gas and the reducing gas in the carbon source mixed gas is 1:(2~35), and the inlet flow rate of the carbon source mixed gas is 3 m / s~90m / s.

[0062] S2) heating the temperature of the reaction chamber in the high temperature growth tube 211 to 620° C. to 3200° C. to form a high temperature reaction zone with a stable temperature field in the reaction chamber, and at the same time, starting the micro plasma generator 120, setting the power of the micro plasma generator 120 to 10 W to 160 W and the frequency to 350 MHz to 550 MHz; S3) The catalyst and the anticoagulant in the two conveyors 115 are respectively transported to the evaporator 117 by the preheated carrier gas in a mass ratio of 2:1 to 60:1 for evaporation to form a volume concentration of 3×10 15 cm -3 ~9×10 18 cm -3 cm -3 , the catalyst precursor vapor with a particle size of 1 nm to 600 nm, the catalyst precursor vapor is ionized by the micro plasma generator 120 to form a particle size of 1 nm to 12 nm and a concentration of 2×10 16 cm -3 ~9×10 20 cm -3 The first catalyst nanoparticle flow ejected from the microplasma generator 120 interacts with the sheath mixed gas in the reaction chamber at a flow rate greater than 5 m / s. The catalyst nanoparticle flow is reduced or slightly oxidized by the sheath mixed gas. At the same time, the sheath mixed gas quickly diffuses to the center of the first catalyst nanoparticle flow, preventing further collision and aggregation of the catalyst nanoparticles, and forming a catalyst nanoparticle with a particle size of 1 nm to 6 nm and a concentration of 2×10 16 cm -3 ~9×10 22 cm -3 a second catalyst nanoparticle stream; Next, the preheated carbon source mixed gas is introduced into the reaction chamber, and the carbon source mixed gas reacts with the catalyst nanoparticles within 6 milliseconds, thereby achieving highly crystalline single-walled carbon nanotubes (SWCNTs) with controllable diameter.

[0063] S4) The products generated in the reaction chamber are separated and collected by the collection unit 330, and are continuously collected by the transition chamber 333 to obtain the initial products.

[0064] The G / D ratio of the single-walled carbon nanotubes prepared by the present invention exceeds 50, the controllable diameters of the highly crystalline single-walled carbon nanotubes are concentrated in 1.13nm~1.54nm, 0.86nm~0.94nm, the average diameters are concentrated in 1.30nm and 0.91nm, and the production capacity can reach kilograms per day.

[0065] Specifically, taking ferrocene as a catalyst, the process of ferrocene vapor forming ferrocene nanoparticles in a microplasma reactor can be divided into the following three stages, which can be referred to Figure 3 As shown: Introduction and preheating stage: The preheated argon gas carrying the vapor of ferrocene and anticoagulant (sulfur) is introduced into the microplasma under high temperature conditions. This step provides the necessary initial conditions and energy for subsequent chemical reactions.

[0066] Dissociation and initial formation stage: In the high temperature environment of the microplasma reactor, ferrocene rapidly dissociates into cyclopentadienyl (Cp) and Fe atomic vapor. At the same time, sulfur atomic vapor also participates in the reaction. In this process, a small part of argon and Fe atoms are ionized by the microplasma. Since the residence time in the microplasma is no more than 6ms, the collision opportunities between Fe atomic vapors are relatively few. At the same time, some sulfur atoms gather around iron atoms, effectively inhibiting the excessive growth of iron atoms. At the outlet of the microplasma generator, most of the Fe atoms (more than 99%) remain in the gas phase, and only less than 1% of Fe forms small clusters of n=2 to n=6. As the airflow enters the downstream of the microplasma generator, the collisions between iron atomic vapor and iron clusters gradually increase, and larger particles begin to form. Outside the microplasma environment, the charge remains conserved during the collision between particles, and the total charge in the Fe particle group also remains stable. Due to the electrostatic enhancement effect, charged particles grow rapidly, while neutral particles grow relatively slowly. In addition, hydrogen (for oxidation or etching) in the sheath mixed gas further prevents the collision and growth of iron nanoparticles, ultimately forming iron nanoparticles with a bimodal size distribution (~1.5 nm and ~3.5 nm).

[0067] Growth and stabilization stage: In the final stage of iron nanoparticle growth, the charge repulsion mechanism effectively prevents the collision of large particles. As small neutral particles are completely consumed, the particle size distribution gradually approaches a stable state. At this time, a preheated hydrocarbon gas curtain is introduced to crack the high-concentration iron nanoparticles, thereby growing single-walled carbon nanotubes with a bimodal size (average diameter of 1.30 nm and 0.91 nm) and concentrated distribution.

[0068] This process makes full use of the characteristics of the microplasma reactor and achieves efficient synthesis of iron nanoparticles and concentrated growth of single-walled carbon nanotubes by precisely controlling reaction conditions and parameters.

[0069] In the microplasma reactor, the dissociation of ferrocene produces neutral and ionized iron vapor, and the electrostatic interaction not only promotes the formation and growth of small particles, but also successfully limits the aggregation of large particles. Since the residence time in the microplasma reactor is 1 millisecond to 10 milliseconds, the growth of most large particles mainly occurs at the rear end of the microplasma reactor. When these particles meet the preheated sheath mixed gas curtain at a certain speed, the possibility of their collision growth is further suppressed, thus forming a high concentration of bimodal size distribution of iron nanoparticles, mainly distributed in ~1.5 nm and ~3.5 nm. Subsequently, when these nanoparticles meet the preheated carbon source mixed gas curtain, single-walled carbon nanotubes (SWCNTs) with high crystallinity and sharp diameter distribution can be grown, with average diameters of 1.30 nm and 0.91 nm, respectively, achieving a daily kilogram-level synthesis efficiency.

[0070] The technical solution of the present invention is further described below in conjunction with specific embodiments.

[0071] Example 1 This embodiment is implemented by a device for macro-synthesis of single-walled carbon nanotubes in microplasma provided by the present invention. In this embodiment, ferrocene is used as a catalyst, sulfur powder is used as an anti-coagulant, argon is used as a carrier gas, hydrogen and water vapor with a volume ratio of 10:1 to 90:1 are used as a sheath mixed gas, and methane and hydrogen with a volume ratio of 1: (1 to 50) are used as a carbon source mixed gas.

[0072] A method for preparing a large amount of single-walled carbon nanotubes with controllable diameter comprises the following steps: Ferrocene and sulfur powder are placed in a conveyor 115 respectively, the molar ratio of iron to sulfur in the ferrocene and sulfur powder is 2:1, and an inert gas is introduced to evacuate the entire device; the temperature of the carrier gas argon is preheated to 100°C by the catalyst carrier gas preheater 111 and the anticoagulant carrier gas preheater 112 respectively, and the temperature of the sheath mixed gas and the carbon source mixed gas is preheated to 300°C and 230°C by the sheath mixed gas preheater and the carbon source mixed gas preheater respectively, and the temperature of the reaction chamber in the high-temperature growth tube 211 is heated to 900°C to form a high-temperature reaction zone with a stable temperature field in the reaction chamber. At the same time, the micro plasma generator is started and the power of the micro plasma generator is set to 15W and the frequency is set to 350 MHz.

[0073] The preheated carrier gas argon is introduced into two conveyors 115 respectively, and the flow rate of the carrier gas argon is 1 L / min, so as to transport the ferrocene and sulfur powder in the two conveyors 115 to the evaporator 117 for evaporation, and form particles with a diameter of 1 nm to 600 nm and a volume concentration of 3×10 15 cm -3 ~9×10 18 cm -3The catalyst precursor vapor is ionized by the micro plasma generator 120 to form particles with a diameter of 1 nm to 12 nm and a concentration of 2×10 16 cm -3 ~5×10 17 cm -3 the first catalyst nanoparticle flow ejected from the micro plasma generator 120 enters the reaction chamber in the high temperature growth tube 211 at a flow rate of 6 m / s.

[0074] The preheated sheath mixed gas is introduced into the reaction chamber from the outer space of the reaction chamber in the high-temperature growth tube 211. The flow rate of the sheath mixed gas is 3 m / s~90 m / s. In the reaction chamber, the first catalyst nanoparticle flow interacts with the sheath mixed gas. The catalyst nanoparticle flow is reduced or slightly oxidized by the sheath mixed gas. At the same time, the sheath mixed gas quickly diffuses to the center of the first catalyst nanoparticle flow to prevent further collision and aggregation of the catalyst nanoparticles, and forms a catalyst nanoparticle with a particle size of 1 nm~6 nm and a concentration of 9×10 16 cm -3 ~8×10 17 cm -3 A second catalyst nanoparticle stream.

[0075] Next, the preheated carbon source mixed gas is introduced into the reaction chamber. The flow rate of the carbon source mixed gas is 3 m / s, the flow ratio of methane and hydrogen in the carbon source mixed gas is 1:2, and the carbon source mixed gas reacts with the second catalyst nanoparticles within 10 milliseconds, thereby realizing highly crystalline SWCNTs with controllable diameter.

[0076] The products generated in the reaction chamber are separated and collected by the collection unit 330, and are continuously collected through the transition chamber 333 to obtain the initial products.

[0077] From Table 2, it can be seen that the yield of the initial product obtained in Example 1 is 53 g / h. Under the test condition of an excitation wavelength of 532 nm, the product G / D ratio is calculated to be 50.8, that is, the prepared product contains high-quality single-walled carbon nanotubes. According to the classical formula of Formula 1, the particle size distribution of the single-walled carbon nanotubes is concentrated in the range of 0.8-1.6 nm. Figure 4 Thermogravimetric characterization showed that the TG residue in the product was 33.34wt%.

[0078] Example 2 This embodiment is implemented by a device for macro-synthesis of single-walled carbon nanotubes in microplasma provided by the present invention. In this embodiment, ferrocene is used as a catalyst, dimethyl sulfoxide is used as an inhibitor, argon is used as a carrier gas, carbon monoxide and oxygen with a volume ratio of 10:1 to 90:1 are used as a sheath mixed gas, and methane and hydrogen with a volume ratio of 1: (1 to 50) are used as a carbon source mixed gas.

[0079] A method for preparing a large amount of single-walled carbon nanotubes with controllable diameter comprises the following steps: Ferrocene and dimethyl sulfoxide are placed in a conveyor 115 respectively, the molar ratio of iron and sulfur elements in ferrocene and dimethyl sulfoxide is 9:1, and an inert gas is introduced to evacuate the entire device; the temperature of the carrier gas argon is preheated to 200°C by the catalyst carrier gas preheater 111 and the anticoagulant carrier gas preheater 112 respectively, and the temperature of the sheath mixed gas and the carbon source mixed gas is preheated to 600°C and 280°C by the sheath mixed gas preheater and the carbon source mixed gas preheater respectively, and the temperature of the reaction chamber in the high-temperature growth tube 211 is heated to 1350°C, forming a high-temperature reaction zone with a stable temperature field in the reaction chamber, and at the same time, starting the micro plasma generator, and setting the power of the micro plasma generator to 50W and the frequency to 450 MHz.

[0080] The preheated carrier gas argon is introduced into two conveyors 115 respectively, and the flow rate of the carrier gas argon is 3 L / min, so as to transport the ferrocene and dimethyl sulfoxide in the two conveyors 115 to the evaporator 117 for evaporation, and form particles with a diameter of 1 nm to 600 nm and a volume concentration of 3×10 15 cm -3 ~9×10 18 cm -3 The catalyst precursor vapor is ionized by the micro plasma generator 120 to form particles with a diameter of 1 nm to 10 nm and a concentration of 3×10 16 cm -3 ~8×10 17 cm -3 the first catalyst nanoparticle flow ejected from the micro plasma generator 120 enters the reaction chamber in the high temperature growth tube 211 at a flow rate of 8m / s.

[0081] The preheated sheath mixed gas is introduced into the reaction chamber from the outer space of the reaction chamber in the high-temperature growth tube 211. The flow rate of the sheath mixed gas is 15 m / s. In the reaction chamber, the first catalyst nanoparticle flow interacts with the sheath mixed gas. The catalyst nanoparticle flow is reduced or slightly oxidized by the sheath mixed gas. At the same time, the sheath mixed gas quickly diffuses to the center of the first catalyst nanoparticle flow to prevent further collision and aggregation of the catalyst nanoparticles, and forms a catalyst nanoparticle with a particle size of 1 nm to 6 nm and a concentration of 5×10 17 cm -3 ~2×10 18 cm -3 A second catalyst nanoparticle stream.

[0082] Next, the preheated carbon source mixed gas is introduced into the reaction chamber. The flow rate of the carbon source mixed gas is 21 m / s, the flow ratio of methane and hydrogen in the carbon source mixed gas is 1:15, and the carbon source mixed gas reacts with the second catalyst nanoparticles within 8 milliseconds, thereby realizing highly crystalline SWCNTs with controllable diameter.

[0083] The products generated in the reaction chamber are separated and collected by the collection unit 330, and are continuously collected through the transition chamber 333 to obtain the initial products.

[0084] It can be seen from Table 2 that the initial product yield obtained in Example 2 is 96 g / h, the TG residue in the product is 23.6wt%, and the product G / D ratio is 63.2, that is, the prepared product contains high-quality single-walled carbon nanotubes. According to the classic formula of Formula 1, the particle size distribution of the single-walled carbon nanotubes is concentrated in the range of 0.8nm~1.6nm.

[0085] Example 3 This embodiment is implemented by a device for macro-synthesis of single-walled carbon nanotubes in microplasma provided by the present invention. In this embodiment, ferrocene is used as a catalyst, thiophene is used as an inhibitor, argon is used as a carrier gas, hydrogen and oxygen with a volume ratio of 10:1 to 90:1 are used as a sheath mixed gas, and methane and hydrogen with a volume ratio of 1: (1 to 50) are used as a carbon source mixed gas.

[0086] A method for preparing a large amount of single-walled carbon nanotubes with controllable diameter comprises the following steps: Ferrocene and thiophene are placed in a conveyor 115 respectively, the molar ratio of iron to sulfur in ferrocene and thiophene is 20:1, and an inert gas is introduced to evacuate the entire device; the temperature of the carrier gas argon is preheated to 350°C by the catalyst carrier gas preheater 111 and the anticoagulant carrier gas preheater 112 respectively, and the temperature of the sheath mixed gas and the carbon source mixed gas is preheated to 900°C and 480°C by the sheath mixed gas preheater and the carbon source mixed gas preheater respectively, and the temperature of the reaction chamber in the high-temperature growth tube 211 is heated to 1550°C, forming a high-temperature reaction zone with a stable temperature field in the reaction chamber, and at the same time, starting the micro plasma generator, and setting the power of the micro plasma generator to 90W and the frequency to 480 MHz.

[0087] The preheated carrier gas argon is introduced into two conveyors 115 respectively, and the flow rate of the carrier gas argon is 5 L / min, so as to transport the ferrocene and thiophene in the two conveyors 115 to the evaporator 117 for evaporation, forming particles with a diameter of 1 nm to 600 nm and a volume concentration of 3×10 15 cm -3 ~9×10 18 cm -3 The catalyst precursor vapor is ionized by the micro plasma generator 120 to form a particle size of 1nm~8nm and a concentration of 7×10 16 cm -3 ~9×10 18 cm -3 the first catalyst nanoparticle flow ejected from the micro plasma generator 120 enters the reaction chamber in the high temperature growth tube 211 at a flow rate of 12 m / s.

[0088] The preheated sheath mixed gas is introduced into the reaction chamber from the outer space of the reaction chamber in the high-temperature growth tube 211. The flow rate of the sheath mixed gas is 35 m / s. In the reaction chamber, the first catalyst nanoparticle flow interacts with the sheath mixed gas. The catalyst nanoparticle flow is reduced or slightly oxidized by the sheath mixed gas. At the same time, the sheath mixed gas quickly diffuses to the center of the first catalyst nanoparticle flow to prevent further collision and aggregation of the catalyst nanoparticles, and forms a catalyst nanoparticle with a particle size of 1 nm to 6 nm and a concentration of 8×10 18 cm -3 ~9×10 20 cm -3 A second catalyst nanoparticle stream.

[0089] Next, the preheated carbon source mixed gas is introduced into the reaction chamber. The flow rate of the carbon source mixed gas is 36 m / s, the flow ratio of methane and hydrogen in the carbon source mixed gas is 1:20, and the carbon source mixed gas reacts with the second catalyst nanoparticles within 6 milliseconds, thereby realizing highly crystalline SWCNTs with controllable diameter.

[0090] The products generated in the reaction chamber are separated and collected by the collection unit 330, and are continuously collected through the transition chamber 333 to obtain the initial products.

[0091] It can be seen from Table 2 that the initial product yield of Example 3 is 166 g / h, the TG residue in the product is 8.6wt%, and the product G / D ratio is 75.7, that is, the prepared product contains high-quality single-walled carbon nanotubes. According to the classical formula of Formula 1, the particle size distribution of the single-walled carbon nanotubes is concentrated in the range of 0.8-1.6nm.

[0092] Example 4 This embodiment is implemented by a device for macro-synthesis of single-walled carbon nanotubes in microplasma provided by the present invention. In this embodiment, ferrocene is used as a catalyst, thiophene is used as an inhibitor, argon is used as a carrier gas, hydrogen and water vapor with a volume ratio of 10:1 to 90:1 are used as a sheath mixed gas, and methane and hydrogen with a volume ratio of 1: (1 to 50) are used as a carbon source mixed gas.

[0093] A method for preparing a large amount of single-walled carbon nanotubes with controllable diameter comprises the following steps: Ferrocene and thiophene are placed in a conveyor 115 respectively, the molar ratio of iron to sulfur in ferrocene and thiophene is 30:1, and an inert gas is introduced to evacuate the entire device; the temperature of the carrier gas argon is preheated to 450°C by the catalyst carrier gas preheater 111 and the anticoagulant carrier gas preheater 112 respectively, and the temperature of the sheath mixed gas and the carbon source mixed gas is preheated to 1100°C and 520°C by the sheath mixed gas preheater and the carbon source mixed gas preheater respectively, and the temperature of the reaction chamber in the high-temperature growth tube 211 is heated to 1550°C, forming a high-temperature reaction zone with a stable temperature field in the reaction chamber, and at the same time, starting the micro plasma generator, setting the power of the micro plasma generator to 120W and the frequency to 510 MHz.

[0094] The preheated carrier gas argon is introduced into two conveyors 115 respectively, and the flow rate of the carrier gas argon is 5 L / min, so as to transport the ferrocene and thiophene in the two conveyors 115 to the evaporator 117 for evaporation, forming particles with a diameter of 1 nm to 600 nm and a volume concentration of 3×10 15 cm -3 ~9×10 18 cm -3The catalyst precursor vapor is ionized by the micro plasma generator 120 to form a particle size of 1nm~7nm and a concentration of 2×10 17 cm -3 ~5×10 20 cm -3 the first catalyst nanoparticle flow ejected from the micro plasma generator 120 enters the reaction chamber in the high temperature growth tube 211 at a flow rate of 21 m / s.

[0095] The preheated sheath mixed gas is introduced into the reaction chamber from the outer space of the reaction chamber in the high-temperature growth tube 211. The flow rate of the sheath mixed gas is 55 m / s. In the reaction chamber, the first catalyst nanoparticle flow interacts with the sheath mixed gas. The catalyst nanoparticle flow is reduced or slightly oxidized by the sheath mixed gas. At the same time, the sheath mixed gas quickly diffuses to the center of the first catalyst nanoparticle flow, preventing the catalyst nanoparticles from further colliding and agglomerating, and forming a catalyst nanoparticle with a particle size of 1 nm to 6 nm and a concentration of 5×10 19 cm -3 ~9×10 22 cm -3 A second catalyst nanoparticle stream.

[0096] Next, the preheated carbon source mixed gas is introduced into the reaction chamber. The flow rate of the carbon source mixed gas is 46 m / s, the flow ratio of methane and hydrogen in the carbon source mixed gas is 1:35, and the carbon source mixed gas reacts with the second catalyst nanoparticles within 5 milliseconds, thereby realizing highly crystalline SWCNTs with controllable diameter.

[0097] The products generated in the reaction chamber are separated and collected by the collection unit 330, and are continuously collected through the transition chamber 333 to obtain the initial products.

[0098] It can be seen from Table 2 that the initial product yield of Example 4 is 148 g / h, the TG residue in the product is 9.7wt%, and the product G / D ratio is 82.5, that is, the prepared product contains high-quality single-walled carbon nanotubes. According to the classical formula of Formula 1, the particle size distribution of the single-walled carbon nanotubes is concentrated in the range of 0.8-1.6nm.

[0099] Example 5 This embodiment is implemented by a device for macro-synthesis of single-walled carbon nanotubes in microplasma provided by the present invention. In this embodiment, ferrocene is used as a catalyst, thiophene is used as an inhibitor, argon is used as a carrier gas, hydrogen and water vapor with a volume ratio of 10:1 to 90:1 are used as a sheath mixed gas, and methane and hydrogen with a volume ratio of 1: (1 to 50) are used as a carbon source mixed gas.

[0100] A method for preparing a large amount of single-walled carbon nanotubes with controllable diameter comprises the following steps: Ferrocene and thiophene are placed in a conveyor 115 respectively, the molar ratio of iron to sulfur in ferrocene and thiophene is 60:1, and an inert gas is introduced to evacuate the entire device; the temperature of the carrier gas argon is preheated to 500°C by the catalyst carrier gas preheater 111 and the anticoagulant carrier gas preheater 112 respectively, and the temperature of the sheath mixed gas and the carbon source mixed gas is preheated to 1200°C and 610°C by the sheath mixed gas preheater and the carbon source mixed gas preheater respectively, and the temperature of the reaction chamber in the high-temperature growth tube 211 is heated to 1550°C, forming a high-temperature reaction zone with a stable temperature field in the reaction chamber, and at the same time, starting the micro plasma generator, setting the power of the micro plasma generator to 150W and the frequency to 550 MHz.

[0101] The preheated carrier gas argon is introduced into two conveyors 115 respectively, and the flow rate of the carrier gas argon is 5 L / min, so as to transport the ferrocene and thiophene in the two conveyors 115 to the evaporator 117 for evaporation, and form particles with a diameter of 1 nm to 600 nm and a volume concentration of 9×10 16 cm -3 ~9×10 18 cm -3 The catalyst precursor vapor is ionized by the micro plasma generator 120 to form a particle size of 1nm~7nm and a concentration of 6×10 17 cm -3 ~9×10 20 cm -3 the first catalyst nanoparticle flow ejected from the micro plasma generator 120 enters the reaction chamber within the high temperature growth tube 211 at a flow rate of 18 m / s.

[0102] The preheated sheath mixed gas is introduced into the reaction chamber from the outer space of the reaction chamber in the high-temperature growth tube 211. The flow rate of the sheath mixed gas is 85 m / s. In the reaction chamber, the first catalyst nanoparticle flow interacts with the sheath mixed gas. The catalyst nanoparticle flow is reduced or slightly oxidized by the sheath mixed gas. At the same time, the sheath mixed gas quickly diffuses to the center of the first catalyst nanoparticle flow, preventing the catalyst nanoparticles from further colliding and agglomerating, and forming a catalyst nanoparticle with a particle size of 1 nm to 6 nm and a concentration of 9×10 20 cm -3 ~9×10 22 cm -3 A second catalyst nanoparticle stream.

[0103] Next, the preheated carbon source mixed gas is introduced into the reaction chamber. The flow rate of the carbon source mixed gas is 78 m / s, the flow ratio of methane and hydrogen in the carbon source mixed gas is 1:10, and the carbon source mixed gas reacts with the second catalyst nanoparticles within 3 milliseconds, thereby realizing highly crystalline SWCNTs with controllable diameter.

[0104] The products generated in the reaction chamber are separated and collected by the collection unit 330, and are continuously collected through the transition chamber 333 to obtain the initial products.

[0105] It can be seen from Table 2 that the yield of the initial product obtained in Example 5 is 175 g / h, and the TG residue in the product is 6.5wt%.

[0106] Comparative Example 1 The scheme of comparative example 1 is basically the same as that of embodiment 1, except that the temperatures of the carrier gas, sheath mixed gas, and carbon source mixed gas are all at room temperature.

[0107] It can be seen from Table 2 that the initial product yield of Comparative Example 1 is 33 g / h, which is significantly lower than that of Example 1. The TG residue in the product is 41.1wt%, which is also increased. The G / D ratio of the product is reduced to 28.3. According to the classical formula of Formula 1, the particle size distribution of single-walled carbon nanotubes is concentrated in the range of 1-3.2nm, which is more dispersed than that of Example 1.

[0108] Comparative Example 2 The scheme of Comparative Example 2 is basically the same as that of Example 2, except that: the flow rate of the sheath mixed gas is 2 m / s; the flow rate of the carbon source mixed gas is 2 m / s.

[0109] It can be seen from Table 2 that the initial product yield of Comparative Example 1 is 18 g / h, which is significantly lower than that of Example 2. The TG residue in the product is 50.8wt%, which has also increased. The G / D ratio of the product is reduced to 21.6. According to the classical formula of Formula 1, the particle size distribution of single-walled carbon nanotubes is concentrated in the range of 1-3.3nm, which is more dispersed than that of Example 2.

[0110] Comparative Example 3 The scheme of Comparative Example 3 is substantially the same as that of Example 3, except that the first catalyst nanoparticle flow ejected from the microplasma generator 120 interacts with the sheath mixed gas in the reaction chamber at a flow rate of 3 m / s.

[0111] It can be seen from Table 2 that the initial product yield of Comparative Example 3 is 45 g / h, which is significantly lower than that of Example 3. The TG residue in the product is 18.7wt%, which has also increased. The G / D ratio of the product is reduced to 33.8. According to the classical formula of Formula 1, the particle size distribution of single-walled carbon nanotubes is concentrated in the range of 1-3.1nm, which is more dispersed than that of Example 3.

[0112] Comparative Example 4 The scheme of Comparative Example 4 is substantially the same as that of Example 1, except that the reaction time of the carbon source mixed gas and the catalyst nanoparticles is 13 seconds.

[0113] It can be seen from Table 2 that the initial product yield of Comparative Example 4 is 34 g / h, which is significantly lower than that of Example 4. The TG residue in the product is 21.3wt%, which has also increased. The G / D ratio of the product is reduced to 45.1. According to the classical formula of Formula 1, the particle size distribution of the single-walled carbon nanotubes is concentrated in the range of 1-3.5nm, which is more dispersed than that of Example 4.

[0114] Comparative Example 5 The scheme of comparative example 5 is basically the same as that of example 1, except that the sheath mixed gas only contains reducing gas.

[0115] It can be seen from Table 2 that the initial product yield of Comparative Example 5 is 108 g / h, which is significantly lower than that of Example 5. The TG residue in the product is 29.8wt%, which has also increased. The G / D ratio of the product is reduced to 53.7. According to the classical formula of Formula 1, the particle size distribution of single-walled carbon nanotubes is concentrated in the range of 1-3.5nm, which is more dispersed than that of Example 5.

[0116] The single-walled carbon nanotubes obtained in Examples 1-5 and Comparative Examples 1-5 were tested respectively. The Raman spectroscopy, thermogravimetric characterization method, scanning electron microscopy and energy dispersive X-ray spectroscopy characterization method, transmission electron microscopy characterization method and ultraviolet-visible-near-infrared absorption spectroscopy characterization method standards of the single-walled carbon nanotube samples refer to GB / T 32871-2016, GB / T24490-2009, GB / T 32869-2016, GB / T 30534-2014 and GB_T 39114-2020, and the test scheme refers to Table 1.

[0117] Table 1 Test scheme for testing single-walled carbon nanotubes in the present invention ; The relationship between the diameter of single-walled carbon nanotubes and the frequency shift of the breathing mode is shown in Equation 1 ωRBM=A / d+B Formula 1 ωRBM is the respiratory mode frequency shift, in cm -1 ); d single-walled carbon nanotube diameter, in nanometers (nm); A constant, in nanometers per centimeter (cm -1 nm); B constant, unit is per centimeter (cm -1); Single-walled carbon nanotubes in different dielectric environments have slightly different A and B diameters. Although the A and B parameters of different samples are different, the difference in the diameter of the single-walled carbon nanotubes given is generally within the range of ±0.05nm. For single-walled carbon nanotube samples without surface treatment, it is recommended to use A=234 and B=10. The chiral index of single-walled carbon nanotubes is obtained by referring to the Kataura diagram. Microscopic particle size distribution measurement equipment: Differential Mobility Analyzer (DMA), which can detect the particle diameter distribution at different positions and conditions in the cavity.

[0118] Table 2 Product indicators in Examples 1-5 and Comparative Examples 1-5 ; The Raman spectra (excitation wavelength: 532 nm) of the single-walled carbon nanotubes obtained in Example 1 are respectively -1 , 1350 cm -1 and 200cm -1 At an amplitude of , it shows a sharp graphite peak (G band), an abnormally small disorder peak (D band) and a highly obvious radial breathing mode characteristic peak RBM. The ratio of the peak intensity of the G band to the peak intensity of the D band (G / D ratio) is 50.8, which is a conventional indicator of the degree of graphitization of SWCNTs. The higher the degree of graphitization means the higher the crystallinity. For SWCNTs, the G / D ratio is greater than 40. It can be said that the crystallinity of this sample is high. This relatively high value means that the crystallinity is quite high.

[0119] Figure 5 The SEM characterization of the preparation of Example 3 is shown by Figure 5 It can be learned that the impurity content in its product is relatively low. Figure 6 The Raman spectrum of the sample prepared in Example 5 is obtained by Figure 6 It can be seen that at 180 cm -1 There are obvious and sharp RBM characteristic absorption peaks on the left and right, that is, the product contains single-walled carbon nanotubes. Under the test condition of an excitation wavelength of 532nm, the product G / D ratio is calculated to be 107.2 using the classic formula of Formula 1, that is, the prepared product is high-quality single-walled carbon nanotubes.

[0120] Figure 7 The Raman spectrum RBM peak local map of the sample prepared in Example 5 is shown. Through statistical calculation of the breathing mode part (RBM peak) of the Raman spectrum, the diameters of the obtained SWCNTs are mainly concentrated in 1.13nm~1.54nm and 0.86nm~0.94nm.

[0121] from Figure 8 and Fig. 9It can be seen that the TEM characterization of the product prepared in Example 3 can intuitively show that the product contains SWCNTs with diameters of 1.30nm and 0.94nm, which can be mutually confirmed by the Raman characterization results of the product. The diameter distribution range is basically consistent with the diameter distribution calculated from the Raman spectrum. Further statistics are made through the TEM characterization results as follows Fig.10 As shown by Fig.10 It can be seen that the particle size of the catalyst nanoparticles in the second catalyst nanoparticle flow in Example 5 is concentrated in two peaks, with an average particle size of 1.5nm (distributed in 1.0-2.0nm) and 3.5nm (distributed in 3.2-4.0nm), and the diameter of the SWCNTs is mainly concentrated in 1.30nm (1.13nm~1.54nm), and 0.91nm (0.86nm~0.94nm).

[0122] The present invention successfully achieved the synthesis of nanoparticles with extremely high volume concentration (more than 2×10 16 cm -3 ) conditions, a stream of catalyst nanoparticles with an optimal size distribution not exceeding 6 nm was generated in a concentrated manner. This innovative breakthrough effectively overcomes the difficulties faced by highly crystalline single-walled carbon nanotubes in terms of narrow diameter distribution and yield, and opens up new paths for the development of related fields.

[0123] The present invention preheats the carrier gas, sheath mixed gas and carbon source mixed gas, which not only reduces the heating load of the reactor, but also avoids the increase of the concentration of catalyst nanoparticles. At the same time, the introduction of preheating gas also reduces unnecessary collisions between catalyst nanoparticles, thereby effectively inhibiting the excessive growth of catalyst nanoparticles and ensuring the uniformity and stability of the catalyst nanoparticles.

[0124] The present invention uses a preheated carrier gas, a continuously flowing micro plasma, a preheated sheath mixed gas curtain and a carbon source mixed gas curtain, and adopts a multi-step chemical vapor phase process to finely control the structure of the iron catalyst, and successfully achieves the nanoparticles with high volume concentration (more than 2×10 16 cm -3 ) conditions, a concentrated stream of iron nanoparticles with narrow size distribution of ~1.5 nm and ~3.5 nm was generated. Furthermore, using these catalyst nanoparticles, single-walled carbon nanotubes with high crystallinity and narrow diameter distribution (1.30 nm and 0.91 nm) can be synthesized, and macro-scale synthesis with a daily output of kilograms can be achieved. The present invention shows significant advantages in the macro-scale preparation of single-walled carbon nanotubes with controllable diameters, and has great commercial value and broad application prospects.

[0125] It should be understood that the above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with the technology to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing catalyst nanoparticles with high volume concentration and narrow diameter distribution, characterized in that: include: Introducing a catalyst and an anticoagulant into an evaporator, and mixing and evaporating the catalyst and the anticoagulant in the evaporator to form a catalyst precursor vapor; Introducing the catalyst precursor vapor into a micro plasma reactor to ionize it to form a first catalyst nanoparticle flow, and delivering the first catalyst nanoparticle flow into a reaction chamber having a second temperature at a first flow rate; A sheath mixed gas is input into the reaction chamber, and the sheath mixed gas surrounds the first catalyst nanoparticle flow and maintains a second flow rate, the catalyst nanoparticles in the first catalyst nanoparticle flow are reduced or oxidized by the sheath mixed gas, and the sheath mixed gas quickly diffuses to the central area of ​​the first catalyst nanoparticle flow and prevents collision and aggregation between the catalyst nanoparticles, thereby obtaining a second catalyst nanoparticle flow, wherein the particle size distribution range of the catalyst nanoparticles contained in the second catalyst nanoparticle flow is smaller than the particle size distribution range of the catalyst nanoparticles contained in the first catalyst nanoparticle flow.

2. The method for preparing catalyst nanoparticles with high volume concentration and narrow diameter distribution according to claim 1, characterized in that: Specifically include: The catalyst and the anticoagulant are introduced into the evaporator respectively by using a carrier gas having a first temperature, wherein the first temperature is 100° C. to 500° C.; and / or the flow rate of the carrier gas is 0.05 L / min to 15 L / min; and / or the carrier gas comprises an inert gas; And / or, the first flow velocity is greater than 5 m / s; And / or, the first flow velocity is 5 m / s to 12 m / s; And / or, the second temperature is 800° C. to 1800° C.; And / or, the catalyst precursor vapor volume concentration is 3×10 15 cm -3 ~9×10 18 cm -3 ; And / or, the particle size of the catalyst precursor particles contained in the catalyst precursor vapor is 1 nm to 600 nm; And / or, the method for preparing catalyst nanoparticles with high volume concentration and narrow diameter distribution specifically comprises: Firstly, preheating the sheath mixed gas to a third temperature, and then inputting the sheath mixed gas into the reaction chamber; And / or, the third temperature is 300° C. to 1200° C.; And / or, the second flow velocity is 3 m / s~90 m / s.

3. The method for preparing catalyst nanoparticles with high volume concentration and narrow diameter distribution according to claim 1, characterized in that: The catalyst nanoparticles in the first catalyst nanoparticle flow have a particle size of 1 nm to 12 nm and a concentration of not less than 2×10 16 cm -3 The particle size of the catalyst nanoparticles in the second catalyst nanoparticle flow is 1 nm to 6 nm, and the concentration is not less than 2×10 16 cm -3 ; and / or, the concentration of the catalyst nanoparticles in the first catalyst nanoparticle flow is 2×10 16 cm -3 ~9×10 20 cm -3 , the concentration of the catalyst nanoparticles in the second catalyst nanoparticle flow is 2×10 16 cm -3 ~9×10 22 cm -3 ; And / or, the particle sizes of the catalyst nanoparticles in the second catalyst nanoparticle flow are concentrated in the range of 1 nm to 2 nm, and 3.2 nm to 4 nm.

4. The method for preparing catalyst nanoparticles with high volume concentration and narrow diameter distribution according to claim 1, characterized in that: The catalyst includes an organic substance containing iron, the anticoagulant includes a compound or a mixture containing sulfur, and the sheath mixed gas includes a reducing gas and water vapor or oxygen; and / or, the molar ratio of the iron element in the catalyst to the sulfur element in the flocculant is 2:1 to 60:1; and / or, the catalyst comprises ferrocene; And / or, the anticoagulant includes at least one of thiophene, dimethyl sulfoxide, sulfur powder, hydrogen sulfide, sulfur dioxide, or a combination of two or more thereof; and / or, the reducing gas in the sheath mixed gas includes at least one of hydrogen, carbon monoxide and ammonia; And / or, the volume ratio of the reducing gas to the water vapor or the oxygen is 10:1 to 90:

1.

5. A method for macro-scale synthesis of single-walled carbon nanotubes with controllable diameter, characterized in that: include: Under the second temperature condition, the catalyst nanoparticles have a particle size of 1 nm to 6 nm and a concentration of not less than 2×10 16 cm -3 The catalyst nanoparticle flow and the carbon source mixed gas are mixed and reacted within 1 millisecond to 10 milliseconds to obtain single-walled carbon nanotubes with controllable diameter; and / or, the concentration of the catalyst nanoparticles in the catalyst nanoparticle flow is 2×10 16 cm -3 ~9×10 22 cm -3 .

6. The method for macro-synthesis of single-walled carbon nanotubes with controllable diameter according to claim 5, characterized in that: The catalyst nanoparticle stream is a second catalyst nanoparticle stream formed by the method for preparing catalyst nanoparticles with high volume concentration and narrow diameter distribution according to any one of claims 1 to 4; And / or, the method for macro-synthesizing single-walled carbon nanotubes with controllable diameter specifically comprises: The catalyst nanoparticle stream is formed by using the method for preparing catalyst nanoparticles with high volume concentration and narrow diameter distribution as described in any one of claims 1 to 4; Introducing a carbon source mixed gas having a fourth temperature into the reaction chamber, maintaining the carbon source mixed gas at a third flow rate, and allowing the carbon source mixed gas and the catalyst nanoparticle flow to mix and react within 1 millisecond to 10 milliseconds; And / or, the method for macro-synthesizing single-walled carbon nanotubes with controllable diameter specifically comprises: The carbon source mixed gas is firstly preheated to a fourth temperature, and then the carbon source mixed gas is introduced into the reaction chamber.

7. The method for macro-synthesis of single-walled carbon nanotubes with controllable diameter according to claim 6, characterized in that: The fourth temperature is 230°C to 650°C; And / or, the third flow velocity is 3 m / s to 90 m / s; And / or, the carbon source mixed gas includes a carbon source gas and a reducing gas; and / or, the volume ratio of the carbon source gas to the reducing gas is 1:(1-50); and / or, the flow ratio of the carbon source gas contained in the carbon source mixed gas to the reducing gas contained in the sheath mixed gas is 1:(2-35); and / or, the carbon source gas comprises at least one of natural gas, methane, ethane, propane, butane, pentane, hexane, ethylene, propylene, ethanol, anthracene or anthracene oil vapor; And / or, the reducing gas contained in the carbon source mixed gas includes at least one of hydrogen, carbon monoxide and ammonia.

8. A single-walled carbon nanotube, characterized in that: The single-walled carbon nanotubes are prepared by the method for macro-synthesis of single-walled carbon nanotubes with controllable diameters as described in any one of claims 4 to 7; and / or, the G / D ratio of the single-walled carbon nanotubes exceeds 50; And / or, the diameters of the single-walled carbon nanotubes are mainly concentrated in the range of 1.13 nm to 1.54 nm and 0.86 nm to 0.94 nm.

9. A device for preparing catalyst nanoparticles with high volume concentration and narrow diameter distribution, characterized in that: include: A catalyst supply mechanism, an anticoagulant supply mechanism, an evaporator, a microplasma generator, a sheath mixed gas supply mechanism and a reaction mechanism, wherein the catalyst supply mechanism and the anticoagulant supply mechanism are connected to the evaporator respectively, the evaporator is connected to the microplasma generator, the reaction mechanism comprises a reaction chamber, a heating mechanism, a catalyst nanoparticle flow injection port and a sheath mixed gas air curtain injection port communicated with the reaction chamber, the sheath mixed gas air curtain injection port is arranged around the catalyst nanoparticle flow injection port, the microplasma generator is connected to the catalyst nanoparticle flow injection port, the sheath mixed gas supply mechanism is connected to the sheath mixed gas air curtain injection port, and the heating mechanism is used to maintain the ambient temperature in the reaction chamber at a second temperature; The catalyst supply mechanism is used to preheat the catalyst and introduce the catalyst into the evaporator, the anticoagulant supply mechanism is used to preheat the catalyst and introduce the anticoagulant into the evaporator, the evaporator is used to evaporate and mix the introduced catalyst and anticoagulant to form a catalyst precursor vapor, the microplasma generator is used to decompose the catalyst precursor vapor to form a first catalyst nanoparticle flow, and introduce the first catalyst nanoparticle flow into the reaction chamber, the sheath mixed gas supply mechanism is used to preheat the sheath mixed gas and introduce the sheath mixed gas into the reaction chamber, the sheath mixed gas is distributed around the catalyst nanoparticle flow, and the sheath mixed gas can reduce or oxidize the catalyst nanoparticle flow, and the sheath mixed gas can quickly diffuse to the central area of ​​the catalyst nanoparticle flow and prevent collision and aggregation between catalyst nanoparticles; And / or, the catalyst supply mechanism includes a catalyst carrier gas preheater and a catalyst conveyor, the catalyst carrier gas preheater and the catalyst conveyor are connected in sequence, and the catalyst conveyor is connected to the evaporator; the anticoagulant supply mechanism includes an anticoagulant carrier gas preheater and an anticoagulant conveyor, the anticoagulant carrier gas preheater and the anticoagulant conveyor are connected in sequence, and the anticoagulant conveyor is connected to the evaporator.

10. A device for macro-synthesis of single-walled carbon nanotubes with controllable diameter, characterized in that: include: A catalyst nanoparticle preparation unit comprises a catalyst supply mechanism, an anticoagulant supply mechanism, an evaporator, and a microplasma generator, wherein the catalyst supply mechanism and the anticoagulant supply mechanism are respectively connected to the evaporator, and the evaporator is connected to the microplasma generator. The catalyst supply mechanism is used to preheat the catalyst and introduce the catalyst into the evaporator, the anticoagulant supply mechanism is used to preheat the catalyst and introduce the anticoagulant into the evaporator, the evaporator is used to evaporate and mix the introduced catalyst and anticoagulant to form catalyst precursor vapor, and the microplasma generator is used to decompose the catalyst precursor vapor to form a first catalyst nanoparticle flow, and introduce the first catalyst nanoparticle flow into a reaction chamber; The reaction unit comprises a carbon source mixed gas supply mechanism, a sheath mixed gas supply mechanism and a reaction mechanism, wherein the reaction mechanism comprises a reaction chamber, a heating mechanism and a catalyst nanoparticle flow injection port, a sheath mixed gas air curtain injection port and a carbon source mixed gas injection port which are connected to the reaction chamber, wherein the sheath mixed gas air curtain injection port is arranged around the catalyst nanoparticle flow injection port, the micro plasma generator is connected to the catalyst nanoparticle flow injection port, the sheath mixed gas supply mechanism is connected to the sheath mixed gas air curtain injection port, the carbon source mixed gas supply mechanism is connected to the carbon source mixed gas injection port, and the heating mechanism The structure is used to maintain the ambient temperature in the reaction chamber at a second temperature, the sheath mixed gas supply mechanism is used to preheat the sheath mixed gas and introduce the sheath mixed gas into the reaction chamber, the carbon source mixed gas supply mechanism is used to preheat the carbon source mixed gas and introduce the carbon source mixed gas into the reaction chamber, the sheath mixed gas is distributed around the catalyst nanoparticle flow, and the sheath mixed gas can reduce or oxidize the catalyst nanoparticle flow, and the sheath mixed gas can quickly diffuse to the central area of ​​the catalyst nanoparticle flow and prevent collision and aggregation between catalyst nanoparticles; And / or, the catalyst supply mechanism includes a catalyst carrier gas preheater and a catalyst conveyor, the catalyst carrier gas preheater and the catalyst conveyor are connected in sequence, the catalyst conveyor is connected to the evaporator, and the anticoagulant supply mechanism includes an anticoagulant carrier gas preheater and an anticoagulant conveyor, the anticoagulant carrier gas preheater and the anticoagulant conveyor are connected in sequence, and the anticoagulant conveyor is connected to the evaporator; And / or, the apparatus for macro-synthesis of single-walled carbon nanotubes with controllable diameter further comprises: a product collection unit, which is connected to the reaction chamber and is used for performing gas-solid separation on the generated single-walled carbon nanotubes and realizing continuous collection.

Citation Information

Patent Citations

  • Carbon nanotube preparation device and method

    CN110217777A

  • Device and method for preparing single-walled carbon nanotubes

    CN114053985A

  • Device and method for preparing single-walled carbon nanotubes through extensible floating catalytic cracking

    CN114162804A

  • Systems and methods of making carbon nanotubes

    US12098074B1

Cited By

  • Reaction device for catalyzing generation of single-walled nanotubes and application of reaction device

    CN119524735A

  • Single-walled carbon nanotube and preparation method and device thereof

    CN120774413A

  • Single-walled carbon nanotube and method and apparatus for preparing the same

    CN120774413B

  • In-situ preparation method of high-purity single-walled carbon nanotube based on field-assisted growth

    CN122501855A