Tungsten / steel connecting method for first wall of fusion reactor cladding

By using high-energy heat source in the fusion reactor to melt deposition of tungsten powder, a high-density tungsten armor is formed, which solves the problems of medium and high thermal stress and brittleness of tungsten/steel connections, and realizes the reliability and stability of tungsten/steel connections in the fusion reactor. , avoiding the impact of heterogeneous elements on the operation of fusion heaps.

CN119035736APending Publication Date: 2024-11-29HEFEI INSTITUTE OF PHYSICAL SCIENCE CHINESE ACADEMY OF SCIENCES
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411420446.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-12
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The prior art is difficult to achieve reliable tungsten/steel connections in fusion reactors, especially in the production of high thermal stress and brittle intermetallic compounds, and the introduced heterogeneous elements may affect the operation of the fusion reactor.

Method used

By finishing and preheating the surface of RAFM steel, melt deposition of tungsten powder is performed using high-energy heat sources such as lasers or electron beams, combined with remelting and scanning strategies, tungsten is deposited layer by layer to form a highly dense tungsten armor to eliminate heterogeneity Interface and reduce thermal stress.

Benefits of technology

It realizes reliable connection without the need to introduce different elements, significantly reduces the generation of interface stress and brittle phases, improves the performance of tungsten/steel connections and the defects of traditional technology, and meets the long-term steady-state operation needs of fusion reactors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119035736A_ABST
    Figure CN119035736A_ABST
Patent Text Reader

Abstract

The invention discloses a tungsten / steel connection method for a first wall of a fusion reactor cladding, which belongs to the technical field of dissimilar material connection and comprises the following steps: step 1, surface treatment of steel; step 2, fused deposition of tungsten; and step 3, carrying out post-treatment. According to the tungsten / steel connection process for the first wall of the fusion reactor cladding, heterogeneous elements are not introduced, dense tungsten is directly grown on the surface of RAFM steel through the additive manufacturing technology, and tungsten / steel connection is achieved. Through high-efficiency permeation of elements at a molten pool, component gradient transition is generated on a tungsten / steel connection interface, existence of a tungsten / steel heterogeneous interface is eliminated, and generation of an intermediate brittle phase is greatly reduced. Different additive manufacturing processes are adopted for achieving tungsten / steel connection according to the surfaces, with different sizes and morphologies, of RAFM steel, namely, the method is suitable for a curved-surface laser direct energy deposition technology and a planar electron beam powder bed cladding technology, partition printing is conducted, and complete connection of tungsten / steel is achieved step by step.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of dissimilar material connection, and in particular relates to a tungsten / steel connection method for a first wall of a fusion reactor blanket. Background Art

[0002] The first wall (FW) of the blanket is the core component of the fusion reactor device and is the component closest to the high-temperature plasma. It is used to protect peripheral components from the impact of high heat flux and high-energy particle flow. When the fusion device is in operation, the FW directly faces the plasma of hundreds of millions of degrees Celsius and is exposed to severe thermal loads, neutron energy impact, irradiation and other multiple effects. The service environment is the most severe. Therefore, the reliable manufacturing of FW is a key technology required for the construction of future fusion reactors. FW is composed of functional materials (tungsten) and structural materials (low-activated ferrite / martensitic steel, RAFM). The key problem at present is the reliable connection of heterogeneous tungsten / steel: (1) The significant mismatch in the thermophysical properties of tungsten and steel, especially the coefficient of thermal expansion (CTE), will produce high thermal stress at the connection interface; (2) When tungsten and steel are connected at the heterogeneous interface, brittle W is easily formed. x Fe y Intermetallic compounds. Large fusion experimental reactors, such as ITER and CRAFT, require large-area tungsten / steel bonding (tungsten-containing area greater than 1m 2 ) and narrow curved flow channels, which put forward higher requirements for the safety and reliability of FW in fusion environment, and require close fit and stability between tungsten and steel. Therefore, it is necessary to develop a tungsten / steel connection process with high engineering feasibility, high strength and high thermal fatigue performance.

[0003] Due to the completely different melting temperatures of tungsten and steel, it is basically impossible to connect them by fusion welding. At present, the main tungsten / steel connection technology at home and abroad is solid phase welding, but both have significant application defects: (1) Plasma spraying: Due to the low thermal diffusion coefficient and conductivity of tungsten, the density of the obtained tungsten coating is poor, and this technology is still far from engineering application; (2) Brazing: Most brazing materials have poor wettability on tungsten, and the brazing materials that can be used for tungsten / steel connection mostly contain Ni, Nb and other easily transmutable active metal elements that are not allowed to exist in fusion reactors. At the same time, the operation of fusion reactors requires that the melting point of the brazing material cannot be too low. At present, there is still no connection brazing material that meets engineering applications. In addition, high melting point brazing materials require high welding temperatures, and the FW tungsten / steel interface to be connected is large, which is easy to cause brazing material loss. There are also disadvantages such as matrix coarsening, tungsten recrystallization catalysis, and high residual stress at the interface. (3) Solid phase diffusion welding: The requirements for the ideal intermediate layer material are high solubility in tungsten / steel, reduced generation of brittle phases (to improve the quality of connection), low activation and hydrogen embrittlement sensitivity (to avoid its significant impact on FW heat transfer, temperature field distribution, plasma operation, etc.), but so far, single-layer or multi-layer metals have been tested, including Ti, V, Zr, Ta, Nb, Ni, Cu, Ti / Ni, Ti / Ni / Ti, Ti / Cu, V / Ni, V / Cu, etc. These material systems cannot fully meet the above four requirements. In addition, vacuum hot pressing technology has low production efficiency, and a single start can only complete the connection of one workpiece, which is not suitable for mass production. However, the hot isostatic pressing (HIP) technology is costly and is limited by the workpiece loading space of the HIP equipment. It can only produce a small part of the fusion reactor FW, and it is inevitable to use welding and other processes to assemble it. The splicing process after multiple HIPs is cumbersome and complicated, and it still cannot get rid of the problem of tungsten / steel welding interface.

[0004] The tungsten / steel connection technologies that have been developed so far cannot meet the requirements of long-term steady-state, reliable and sustainable development during the actual operation of fusion reactors. The urgent task is to optimize the design and effectively develop a new tungsten / steel connection process for the first wall of the fusion reactor blanket, so as to prepare for the actual operation of the next-generation fusion reactor that is being built in my country. Summary of the invention

[0005] In order to solve the technical problems mentioned in the above background technology, the present invention proposes the following technical solutions: The present invention can achieve: 1) Eliminate the tungsten / steel heterogeneous interface in the first wall of the cladding, greatly reduce the interface stress and brittle W x Fe y Intermetallic compounds form a reliable connection interface. 2) Avoid introducing other elements to eliminate the effects of other elements other than tungsten steel on FW heat transfer, temperature field distribution, plasma operation, etc. 3) The tungsten coated on the first wall surface of the cladding is highly dense.

[0006] The technical solution adopted by the present invention is as follows:

[0007] A tungsten / steel connection method for a first wall of a fusion reactor blanket comprises the following steps:

[0008] Step 1, steel surface treatment: finish the surface of RAFM steel to a surface roughness of Ra≤0.4, and perform ultrasonic cleaning to ensure that the surface to be connected is free of contamination and impurities that may affect the connection state;

[0009] Step 2: Melt deposition of tungsten: preheat the RAFM steel substrate, melt the tungsten powder through a high-energy heat source, and deposit tungsten layer by layer on the RAFM steel surface by laser direct energy deposition or electron beam powder bed cladding, and achieve tungsten / steel connection with remelting and scanning strategies;

[0010] Step 3, post-processing: machining to remove excess surface, heat treatment to eliminate thermal stress, to improve the organization and enhance the overall performance.

[0011] In the above technical solution, in step 2, the preheating temperature is 600~1000℃.

[0012] In the above technical solution, in step 2, the high-energy heat source is a laser or an electron beam, in a pulsed or continuous manner.

[0013] In the above technical solution, in step 2, the feed rate of tungsten powder in the laser direct energy deposition is m = 5-30g / min, the laser power is 600~3000W, the spot diameter is 150~750μm, and the scanning speed is 50~600mm / min.

[0014] In the above technical solution, in step 2, the layer thickness of the electron beam powder bed cladding is 20~150μm, the electron beam power is 3~8kW, the electron beam spot diameter is 100~400μm, and the scanning speed is 100~300 mm / s.

[0015] In the above technical solution, in step 2, the laser direct energy deposition is applicable to RAFM steel curved substrates, and the electron beam powder bed cladding is applicable to RAFM steel flat substrates.

[0016] In the above technical solution, in step 2, the partitioning refers to first completing the tungsten / steel connection of a designated size area to reduce thermal stress.

[0017] In the above technical solution, in step 2, the remelting refers to the process of scanning the solidified deposited tungsten multiple times before re-coating the sample with new powder to eliminate columnar crystals and inhibit cracks.

[0018] In the above technical solution, in step 2, the scanning strategy refers to horizontal rotation and intersection of the scanning or deposition paths between adjacent printed tungsten layers along the construction direction to ensure complete remelting of the powder particles.

[0019] In the above technical solution, in step 2, the whole process is under vacuum conditions, and the vacuum degree is greater than 6×10 - 3 Pa, or a normal pressure protective atmosphere, wherein the normal pressure protective atmosphere comprises Ar, N 2 and H 2 Protective gas, etc.

[0020] The beneficial effects of the present invention are as follows:

[0021] 1. Compared with brazing and solid-phase diffusion welding technology, it can form a reliable connection without introducing undesirable heterogeneous elements (such as active / hydrogen storage elements contained in the brazing material and the intermediate layer), avoiding the known (changing the temperature field, easy transmutation activity, hydrogen storage, etc.) and unproven adverse effects on the function of the first wall and the operation of the fusion reactor, and meeting the actual operation requirements of the fusion reactor.

[0022] 2. Compared with plasma spraying technology, the tungsten armor produced is highly dense, has high molding accuracy, good control flexibility, and has a wider degree of freedom in terms of different shapes and composition gradients. Additive manufacturing simplifies structural design and can provide additional potential for the future first wall in terms of size, shape, and functional gradient transition requirements.

[0023] 3. Change the traditional tungsten / steel technology route of the first wall of the fusion reactor blanket, and innovatively transform the manufacturing concept into integral manufacturing. By directly printing tungsten on RAFM steel to achieve tungsten / steel connection, the existence of tungsten / steel heterogeneous interface can be eliminated, and the interface performance can be significantly improved: the elements of tungsten deposited under high-energy beam and the base material RAFM steel are mixed, and the content of elements such as Fe and Cr in the interface molten pool permeates each other, and the composition / functional gradient transition layer from the interface to the tungsten armor can be customized in the microstructure, effectively reducing the generation of unnecessary intermediate brittle phases. The overall manufacturing route is also consistent with the compact design and large module design concept of future blanket manufacturing, which can significantly reduce the number of blanket modules and reduce the gap between adjacent modules. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 The present invention is a schematic flow chart of a tungsten / steel connection method for the first wall of a fusion reactor blanket. DETAILED DESCRIPTION

[0025] In order to facilitate the understanding of the present invention, the present invention will be described more comprehensively and carefully in combination with preferred embodiments below, but the protection scope of the present invention is not limited to the following specific embodiments.

[0026] Embodiment 1:

[0027] like Figure 1 As shown, this embodiment realizes tungsten / steel connection by laser directed energy deposition on the RAFM steel curved surface:

[0028] (1) Surface treatment of steel: Polish the upper surface of RAFM steel to a roughness of Ra ≤ 0.4 to remove the surface oxide film and impurities, and then clean it thoroughly with alcohol and dry it;

[0029] (2) Molten deposition of tungsten: The RAFM steel substrate was preheated to 900°C. To prevent oxidation, argon was used as powder feeding gas and protective gas. Coaxial powder feeding was adopted, and the powder feeding rate (m = 20 g / min) was adjusted. The laser parameters were: power P = 2500 W, scanning speed v = 300 mm / min, and beam spot diameter 300 μm. The laser emitted from the nozzle melted the tungsten powder instantly and quickly solidified it on the surface of the RAFM steel substrate. The tungsten / steel connection was achieved through the mixed dilution of liquid tungsten and steel. Single-layer partitioned (30×30 mm unit) deposition was carried out. With the motion system, the curved surface was divided into multiple zones, and gradually spread until the tungsten / steel connection was achieved on the entire RAFM steel substrate surface. During the solidification process, the temperature was kept warm and the temperature was slowly reduced to room temperature. After the single layer was melted, the powder feeder moved upward. Before the next layer began to be deposited, the laser deposition path between adjacent layers was rotated 90°. The deposited tungsten was scanned and remelted multiple times, and then the subsequent tungsten powder was melted and deposited. Argon is used as powder feeding gas and protective gas throughout the whole process to prevent tungsten powder from oxidation.

[0030] (3) Post-processing: Machining to remove excess uneven surfaces, and heat treatment of the deposited tungsten to eliminate thermal stress and improve the structure.

[0031] The tungsten / steel connection obtained by this implementation method has a significant Fe, Cr, and W composition gradient transition from the vicinity of the substrate along the structural direction, eliminating the existence of heterogeneous interfaces. Without introducing dissimilar materials, the brittle intermediate phase and interface stress problems that are widely present in the interface of traditional brazing and solid phase diffusion technology are greatly reduced, and the interface performance of tungsten / steel connection is significantly improved. In addition, this implementation method uses additive manufacturing to print tungsten when connecting tungsten / steel, which can provide a wide range of geometric freedom and composition freedom for the design of the subsequent first wall tungsten armor, simplify the structural design, and achieve the unification of functional structure.

[0032] Embodiment 2:

[0033] like Figure 1 As shown, in this embodiment, tungsten / steel connection is achieved on the RAFM steel plane by electron beam powder bed cladding:

[0034] (1) Surface treatment of steel: The upper surface of the RAFM steel was polished to a roughness of Ra ≤ 0.4, the surface oxide film and impurities were removed, and the steel was cleaned with ultrasound and acetone and then placed in an electron gun vacuum chamber;

[0035] (2) Molten deposition of tungsten: Preheat the RAFM steel substrate to 650°C, evenly spread a layer of 100μm tungsten powder on the surface, adjust the electron beam parameters to: 5 kW power, 300μm beam spot, 200mm / s scanning speed, perform partition scanning and cladding on the tungsten powder, so that the powder particles are evenly heated and melted to form a cladding layer with the RAFM steel, and the tungsten / steel connection is achieved through the mixed dilution of liquid tungsten and steel. The single-time construction partition size is 60×60mm, and multiple zones are gradually spread until the tungsten / steel is completely connected on the surface of the RAFM substrate. After the single-layer connection is completed, the electron beam scanning path is rotated 67°, and the deposited tungsten is scanned and remelted multiple times before re-coating with fresh powder, and then the subsequent tungsten powder is melted and deposited. The vacuum degree of the whole process is better than 6×10 -3 Pa, to prevent oxidation and other problems;

[0036] (3) Post-processing: Low-temperature annealing of FW is performed to eliminate thermal stress and improve the structure.

[0037] This implementation method achieves good thermal stability of the tungsten / steel connection interface, greatly reduces the interface stress, and does not generate brittle phases. Compared with the traditional brazing and solid phase diffusion technology that introduces heterogeneous elements to cause activation and hydrogen-induced powdering, the connection interface of this solution does not introduce other elements, and well maintains the design performance of the first wall. In addition, the electron beam can be quickly manipulated in the entire construction area, locally controlling the thermal conditions of the material, which is conducive to controlling the microstructure and stress state.

[0038] The present invention does not elaborate on some of the common technologies of those skilled in the art. The above-described embodiments are only descriptions of preferred implementations of the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementations described. Without departing from the design spirit of the present invention, various modifications and improvements made by ordinary technicians in this field to the technical solution of the present invention should fall within the scope of protection determined by the claims of the present invention.

Claims

1. A tungsten / steel connection method for the first wall of a fusion reactor blanket, characterized in that: The following steps are involved: Step 1, steel surface treatment: finish the surface of RAFM steel to a surface roughness of Ra≤0.4, and perform ultrasonic cleaning to ensure that the surface to be connected is free of contamination and impurities that may affect the connection state; Step 2: Melt deposition of tungsten: preheat the RAFM steel substrate, melt the tungsten powder through a high-energy heat source, and deposit tungsten layer by layer on the RAFM steel surface by laser direct energy deposition or electron beam powder bed cladding, and achieve tungsten / steel connection with remelting and scanning strategies; Step 3, post-processing: machining to remove excess surface, heat treatment to eliminate thermal stress, improve the organization, and enhance overall performance.

2. The tungsten / steel connection method for the first wall of a fusion reactor blanket according to claim 1, characterized in that: In step 2, the preheating temperature is 600-1000°C.

3. The tungsten / steel connection method for the first wall of a fusion reactor blanket according to claim 1, characterized in that: In step 2, the high energy heat source is a laser or an electron beam, in a pulsed or continuous manner.

4. The tungsten / steel connection method for the first wall of a fusion reactor blanket according to claim 1, characterized in that: In step 2, the feed rate of tungsten powder in the laser direct energy deposition is m = 5-30g / min, the laser power is 600~3000W, the spot diameter is 150~750μm, and the scanning speed is 50~600mm / min.

5. The tungsten / steel connection method for the first wall of a fusion reactor blanket according to claim 1, characterized in that: In step 2, the layer thickness of the electron beam powder bed cladding is 20-150 μm, the electron beam power is 3-8 kW, the electron beam spot diameter is 100-400 μm, and the scanning speed is 100-300 mm / s.

6. The tungsten / steel connection method for the first wall of a fusion reactor blanket according to claim 4, characterized in that: In step 2, the laser direct energy deposition is applicable to RAFM steel curved substrates, and the electron beam powder bed cladding is applicable to RAFM steel flat substrates.

7. The tungsten / steel connection method for the first wall of a fusion reactor blanket according to claim 1, characterized in that: In step 2, the partitioning means completing the tungsten / steel connection of a designated size area first to reduce thermal stress.

8. The tungsten / steel connection method for the first wall of a fusion reactor blanket according to claim 1, characterized in that: In step 2, the remelting process refers to the process of scanning the solidified deposited tungsten multiple times before recoating the sample with new powder to eliminate columnar grains and suppress cracks.

9. The tungsten / steel connection method for the first wall of a fusion reactor blanket according to claim 1, characterized in that: In step 2, the scanning strategy refers to horizontal rotation and intersection of scanning or deposition paths between adjacent printed tungsten layers along the build direction to ensure complete remelting of the powder particles.

10. The tungsten / steel connection method for the first wall of a fusion reactor blanket according to claim 1, characterized in that: In step 2, the entire process is under vacuum conditions, and the vacuum degree is greater than 6×10 -3 Pa, or normal pressure protective atmosphere, the normal pressure protective atmosphere is Ar, N2 or H2 protective gas.