Machining method for large-diameter long-depth thin-wall high-temperature alloy casing of aero-engine
Through residual stress detection and scanning detection technology, the stress and dimension changes of the aircraft engine's large diameter long-drift thin-wall high-temperature alloy receiver are analyzed, and the processing parameters are adjusted, which solves the problems of deformation and stress concentration during the processing process, and realizes the integration of part size Improvement of gauges control and processing accuracy.
Patent Information
- Application Number
- CN202410835110.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-26
- Publication Date
- 2024-11-29
AI Technical Summary
Large diameter, long-drain, thin-walled high-temperature alloy receivers of aircraft engines are prone to deformation during processing, and the wall thickness is difficult to guarantee. Moreover, the concentrated stress during milling processing leads to deformation of parts, which is difficult to effectively solve the problem of the existing technology.
Residual stress detection equipment is used to detect the changes in stress before and after processing of parts, and combine scanning to detect the actual size, analyze the stress and dimensional changes, adjust the processing parameters to control deformation, and reduce the problem of stress concentration through multi-step processing and heat treatment.
Effectively control part deformation, ensure dimensional compliance, reduce the problems of large local processing volume and concentrated stress during subsequent processing, and improve processing accuracy and stability.
Smart Images

Figure CN119035973A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of engines, and in particular to a method for processing a large-caliber, long-depth, thin-walled, high-temperature alloy casing of an aero-engine. Background Art
[0002] The large-diameter, long-depth, thin-walled, high-temperature alloy casing of aircraft engines can be used for turbofan engines with greater thrust and high bypass ratio. The parts are larger in size and thinner in wall thickness than those of CJ-1000A. The structural features of the large-diameter, long-depth, thin-walled, high-temperature alloy casing are as follows: the parts are composed of a rotating large-diameter conical cylinder, an outer circumferential boss, and an inner circle hook. The size can reach φ1800mm (diameter of the large end of the conical cylinder) × φ1250mm (diameter of the small end of the conical cylinder) × 700mm, with multiple outer circumferential bosses, and a large-diameter ultra-thin wall part with a thickness of 1.8mm at the thinnest part of the boss wall (such as Figure 1 ).
[0003] Since the material is a high-temperature alloy (GH4738), the processing difficulties are high hardness and difficulty in processing; the part processing diameter is large, the wall thickness of the outer circumferential milling boss is ultra-thin, and there are many circumferential bosses. When milling the bosses, it is easy to generate large stress, which causes the part to deform; the wall thickness tolerance is difficult to guarantee. The problem of stress causing deformation of thin-walled parts is difficult to solve. Long-term aging is one method, and releasing stress through heat treatment is another method, but whether it is effective for the processing of thin-walled parts still troubles the industry.
[0004] CN201710347233.2 The present invention relates to a method and system for measuring stress at the edge of a bolt connection hole. The method comprises: pasting a strain gauge on the edge of a hole on the surface of a connected part, and measuring the strain after pasting; driving a bolt into the hole of the connected part, and measuring the strain again after driving; sleeve-mounting a measurement auxiliary pad on the bolt, wherein a groove is provided in the measurement auxiliary pad, and the strain gauge is accommodated in the groove during sleeve-mounting, so that the measurement auxiliary pad is pressed onto the connected part; installing a replacement nut on the bolt, and measuring the strain again after tightening. Summary of the invention
[0005] The purpose of the present invention is to propose a large-diameter, long-depth, thin-walled, high-temperature alloy casing processing implementation process for aircraft engines, using residual stress detection equipment to detect changes in residual stress before and after part processing, and then using the equipment to scan and detect the actual size of the part after processing, comparing the position of the stress change with the position of the scanned size change to see whether it corresponds, analyzing the stress and size detection results, so as to adjust more reasonable processing parameters, control the deformation of parts, ensure the size of parts, and reduce the problems of large local processing volume and stress concentration in subsequent processing.
[0006] The technical solution of the present invention is a method for processing a large-caliber, long-depth, thin-walled, high-temperature alloy casing of an aircraft engine. The casing workpiece blank to the finished product size is divided into 3-6 steps according to the contour structure machining to evenly remove the inner and outer circle excess. First, a residual stress detection device is used to detect the change in residual stress before and after the part processing, and then the equipment is used to scan and detect the actual size of the part after processing. The position of the stress change is compared with the position of the scanned size change to see whether it corresponds, and the stress and size detection results are analyzed, so as to adjust more reasonable processing parameters, control the deformation of the part, and ensure the size of the part.
[0007] Residual stress detection is carried out before parts processing, and compared with the residual stress detection after subsequent machining to remove the allowance (rough turning + rough milling + stress relief heat treatment), to understand the changes in stress after rough machining and the distribution of stress.
[0008] Residual stress analysis: mainly checks the deformation of parts. If the tolerance meets the part processing requirements, it means that the influence of stress value on parts is within the controllable range; if the tolerance exceeds the tolerance, it means that the processing parameters need to be changed to reduce stress. The results of the analysis and the control of the cutting amount of the present invention: by detecting the dimensional deformation of the parts to determine whether the stress distribution and stress value exceed the standard, if the deformation exceeds the tolerance range, it is necessary to adjust the corresponding processing parameters (check tool wear, reduce cutting amount and feed amount).
[0009] A20 residual stress detection I obtains the reference value of stress; →A30 rough turning - boring - rough milling shape →A70 residual stress detection 2, first comparison with the reference value of stress; →A80 dimension detection I, stress detection needs to be combined with dimension detection to determine the change of parts and control the cutting amount →A100 vacuum stress relief heat treatment →A110 residual stress detection 3, second comparison with the reference value of stress, →A120 dimension detection 2 stress detection needs to be combined with dimension detection to determine the change of parts and control the cutting amount →A130 turning base - expanding positioning hole - fine milling, all control the cutting amount; →A190 residual stress detection 4, third comparison with the reference value of stress, →A200 dimension detection 3, stress detection needs to be combined with dimension detection to determine the change of parts and control the cutting amount →A210 turning base - fine turning two ends; →A240 residual stress detection 5, fourth comparison with the reference value of stress, →A250 dimension detection 4, stress detection needs to be combined with dimension detection to determine the change of parts and control the cutting amount; drilling and milling all allowances.
[0010] The control of internal stress generated by cutting force is the change of cutting amount. When the stress value measured in the machining gap exceeds the first benchmark value by more than 30-100%, the cutting parameters are controlled by controlling the cutting amount per unit time. The cutting amount refers to the amount of metal cut per unit time. The cutting parameters are 40-70% of the normal value. When the benchmark value is more than 100-200%, the cutting parameters are controlled by controlling the cutting amount per unit time to 20-50% of the normal cutting amount per unit time (the cutting amount refers to the amount of metal cut per unit time).
[0011] Therefore, when fine milling the circumferential boss with 2mm left for the outer circle of the blank and 5mm left for the inner circle, the cutting amount should be controlled to reduce the internal stress caused by the cutting force during the milling process and control the deformation of the parts.
[0012] The first residual stress test is carried out on the incoming blank to obtain the reference value of stress. During the test, strain gauges are evenly pasted on the surface of the blank, and then strain measurement, that is, piezoelectric voltage measurement, is carried out. The pasted strain gauges are evenly distributed on the outer surface of the casing blank.
[0013] 4-8 strain gauges are distributed on each vertical section of the outer surface of the casing blank (Figure 2-3); the distribution of strain gauges on adjacent vertical sections is staggered. After the residual stress test, the dimension scanning test is carried out at the same time.
[0014] Beneficial effects: The present invention is suitable for workpieces with large turbine casings, thicker walls, and high processing difficulty: workpieces made of special materials are very easy to deform during machining (turning, milling, drilling, etc.), and the wall thickness is difficult to guarantee. Residual stress detection equipment is used to detect the change in residual stress before and after part processing, and then the equipment is used to scan and detect the actual size of the part after processing. The position of the stress change is compared with the position of the scanned size change to see if it corresponds, and the stress and size detection results are analyzed to adjust more reasonable processing parameters, control the deformation of parts, and ensure that the part size is compliant. Through detection and processing control, the problems of large local processing volume and stress concentration in subsequent processing are reduced. Residual stress detection is carried out before part processing, and compared with the residual stress detection after the subsequent removal of large allowances (rough turning + rough milling + stress relief heat treatment), the changes in stress after rough processing and the distribution of stress are understood.
[0015] The circumferential bosses (steps) of the workpiece are distributed in the axial direction, and a large number of pitch circles need to be milled. The internal stress generated by milling is large. The rigidity of the parts is enhanced, the internal stress generated by the cutting force during milling is reduced, and the deformation of the parts is controlled. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 It is a schematic cross-sectional view of the workpiece of the present invention; the numbers are the thickness values here;
[0017] FIG2 is a schematic diagram of residual stress detection points of the present invention; Figure 2A(where the numbers are stress measurement points), 2B are 4 different (residual stress) detection points and data distribution diagrams distributed at different axial positions and cross sections, and the residual stress remains in the same position at each stage.
[0018] Fig. 3 is a schematic diagram of dimension scanning detection; Figure 3A , 3B They are overall scanning (contour detection, using optical scanning A and digital-analog ratio analysis, compared with reference B, for accurate before-after comparison) and 8 different (residual stress) detection points and data distribution diagrams distributed on different sections.
[0019] Figure 4 Schematic diagram of circumferential distribution of bosses;
[0020] Figure 5 Schematic diagram of the cross-sectional width of the circumferential boss. The circumferential bosses (steps) are distributed in large numbers in the axial direction, and the number of pitch circles that need to be milled is large (such as Figure 4 , Figure 5 ). DETAILED DESCRIPTION
[0021] Processing implementation plan for large-diameter, long-depth, thin-walled, high-temperature alloy casings of aircraft engines: For example, the 200-type low-pressure turbine casing is larger in size and thinner in wall thickness than the 100-type low-pressure turbine casing, and is more difficult to process: the material is GH473, which is very easy to deform during processing, and the wall thickness is difficult to guarantee. First, the residual stress detection equipment is used to detect the change in residual stress before and after the parts are processed, and then the equipment is used to scan and detect the actual size of the parts after processing, and the position of the stress change is compared with the position of the scanned detection size change. The stress and size detection results are analyzed to adjust more reasonable processing parameters, control the deformation of the parts, and ensure the size of the parts; the residual stress detection points are shown in Figure 2, and the size scanning detection is shown in Figure 3. The size scanning uses optical scanning (non-contact) and three-coordinate measurement (contact), both of which are used for model comparison and analysis. Optical scanning to evaluate contour: an optical scanner is used to directly scan the part contour, generate the scanned size on the corresponding computer, fit the measured reference value with the reference on the theoretical model, set the part tolerance value, and the measurement result will reflect the size deviation in different colors; the advantage is that it will not limit the part size and can quickly get the result.
[0022] The three-coordinate measurement accuracy reaches 0.001mm. The optical scanning accuracy reaches 0.01mm.
[0023] There are many size allowances from the blank to the finished product. The allowances of the inner and outer circles are evenly removed according to the profiling structure to reduce the problems of large local processing volume and stress concentration in the subsequent processing process.
[0024] Residual stress detection is performed before parts processing, and compared with the residual stress detection after subsequent removal of large allowances (rough turning + rough milling + stress relief heat treatment), to understand the changes in stress after rough processing and the distribution of stress.
[0025] Since the circumferential bosses (steps) are distributed in large numbers in the axial direction, a large number of pitch circles need to be milled (such as Figure 4 , Figure 5 ), the internal stress generated by milling is large, and the wall thickness of the circumferential boss is 1.8 (+0.2-0) mm, so the circumferential boss is finely milled when 2 mm is left for the outer circle of the part and 5 mm is left for the inner circle, which can enhance the rigidity of the part, reduce the internal stress generated by the cutting force during the milling process, and control the deformation of the part (see the table below for tool selection and cutting parameters). It is mainly the change in cutting volume. When the stress value measured during the machining gap exceeds the first benchmark value by more than 30-100%, the cutting parameters are controlled by controlling the cutting volume per unit time to 40-70% of the normal cutting volume per unit time (the cutting volume refers to the amount of metal cut per unit time); when the benchmark value is above 100-200%, the cutting parameters are controlled by controlling the cutting volume per unit time to 20-50% of the normal cutting volume per unit time (the cutting volume refers to the amount of metal cut per unit time);
[0026] The first residual stress test (test I) is carried out on the incoming blank to obtain the reference value of stress. During the test, strain gauges are evenly pasted on the surface of the blank, and strain measurement (piezoelectric voltage measurement) is performed after pasting. The equipment specified in CN201710347233.2 is used for measurement.
[0027] After the inner and outer circle semi-finishing process (leaving 1mm allowance on one side), the residual stress detection and dimension detection processes are added to check the changes in the parts after the inner circle removal is 3mm and the outer circle removal is 1mm. According to the detected residual stress and dimensional changes, the influence of the processing parameters and tool selection on the parts during the semi-finishing process is understood. Based on these values, the stress and dimensional deformation caused by the finishing of the parts are estimated, and the processing parameters for the subsequent finishing of the parts are adjusted (for details of the processing parameters, see the process table of the implementation method).
[0028] Processing route for large-caliber, long-depth, thin-walled, high-temperature alloy casings:
[0029] A10 incoming material inspection → A20 residual stress detection I to obtain the stress reference value; → A30 rough turning of the shape (5mm allowance on one side) → A40 rough turning of the outer circle (2mm allowance on one side) → A50 drilling and boring of positioning holes → A60 rough milling of the circumferential shape (2mm allowance on one side) → A70 residual stress detection 2, first comparison with the stress reference value; → A80 dimension detection I → A90 corrosion inspection → A100 vacuum stress relief heat treatment → A110 residual stress detection 3, second comparison with the stress reference value (this stress detection is to check the changes before and after the stress relief heat treatment of the parts and whether the size affects the machining cutting amount) → A120 dimension detection 2 → A130 turning one end reference → A140 turning the other end reference → A150 expanding the positioning hole → A160 fine milling of the circumferential shape → A170 semi-finishing turning of one end → A180 semi-finishing turning of the other end, A130 -180 all control the cutting amount; →A190 residual stress detection 4, compared with the stress reference value for the third time, →A200 dimension detection 3, stress detection needs to be combined with dimension detection to determine the change of parts and determine the machining cutting amount →A210 turning the base →A220 fine turning one end →A230 fine turning the other end, A210-230 all control the cutting amount; →A240 residual stress detection 5, compared with the stress reference value for the fourth time, →A250 dimension detection 4, stress detection needs to be combined with dimension detection to determine the change of parts and determine the machining cutting amount; →A260 drilling and milling one end hole →A270 drilling and milling the other end hole →A280 drilling and milling circumferential holes, grooves and boss surfaces →A290 milling inner circular grooves and holes →A300 electric pulse holes →A310 clamp repair →A320 dimension detection 5 →A330 fluorescent inspection →A340 marking →A350 final inspection. The residual stress is detected before the parts are processed, and compared with the residual stress detection after the subsequent machining to remove the excess, the change of stress after rough machining and the distribution of stress are analyzed.
[0030] Analysis and adjustment of processing parameters are mainly to control the cutting amount per unit time: by detecting the deformation of the parts, if the tolerance meets the requirements of the parts processing, it means that the influence of the stress value on the parts is within the controllable range, and the original cutting amount per unit time is used; if the stress value and tolerance are out of tolerance, it means that the processing parameters need to be changed to reduce the stress and reduce the cutting amount per unit time. The results of the analysis and the control of the cutting amount of the present invention: by detecting the dimensional deformation of the parts to determine whether the stress distribution and stress value exceed the standard, if the deformation is large and exceeds the tolerance range, the corresponding processing parameters need to be adjusted (of course, check the tool wear, reduce the cutting amount and feed amount).
[0031] Table 1: Basic parameters of turning (cutting amount)
[0032]
[0033] Table 2: Basic parameters of milling (cutting amount)
[0034]
[0035] The present invention uses specific embodiments to illustrate the principles and implementation methods of the present invention. The description of the above embodiments is only used to help understand the device of the present invention and its core concept. At the same time, for those skilled in the art, according to the concept of the present invention, there will be changes in the specific implementation methods and application scope. In summary, the content of this specification should not be understood as limiting the present invention.
Claims
1. A method for machining a large-caliber, long-depth, thin-walled, high-temperature alloy casing of an aircraft engine. Its characteristics are: The size of the receiver workpiece from the blank to the finished product is divided into 3-6 steps according to the contoured structure machining to evenly remove the inner and outer circle excess. First, the residual stress detection equipment is used to detect the change of residual stress before and after the part processing, and then the equipment is used to scan and detect the actual size of the part after processing. The position of the stress change is compared with the position of the scanned size change to see if it corresponds. The stress and size detection results are analyzed to adjust more reasonable processing parameters, control the deformation of the parts, and ensure the size of the parts.
2. The method for machining a large-caliber, long-depth, thin-walled, high-temperature alloy casing of an aircraft engine according to claim 1, Its characteristics are: Specific steps: A20 residual stress detection I to obtain the stress benchmark value; → A30 rough turning - drilling and boring - rough milling shape → A70 residual stress detection 2, first comparison with the stress benchmark value; → A80 dimension detection I, stress detection needs to be combined with dimension detection to determine the change of parts and control the cutting amount → A100 vacuum stress relief heat treatment → A110 residual stress detection 3, second comparison with the stress benchmark value, → A120 dimension detection 2 stress detection needs to be combined with dimension detection to determine the change of parts and control the cutting amount → A130 turning benchmark - expanding positioning holes - fine milling, all control the cutting amount; → A190 residual stress detection 4, third comparison with the stress benchmark value, → A200 dimension detection 3, stress detection needs to be combined with dimension detection to determine the change of parts and control the cutting amount → A210 turning benchmark - fine turning two ends; → A240 residual stress detection 5, fourth comparison with the stress benchmark value, → A250 dimension detection 4, stress detection needs to be combined with dimension detection to determine the change of parts and control the cutting amount; drilling and milling.
3. The method for machining a large-caliber, long-depth, thin-walled, high-temperature alloy casing of an aircraft engine according to claim 2, Its characteristics are: Residual stress detection is carried out before each machining of parts, and compared with the residual stress detection after subsequent machining to remove the excess, the change of stress after rough machining and the distribution of stress are analyzed; stress control is carried out by changing the cutting amount. When the stress value measured in the machining gap exceeds the first benchmark value by more than 30-100%, the cutting amount is controlled to 40-70% of the normal value; when the benchmark value is above 100-200%, the cutting parameters are controlled by controlling the cutting amount per unit time to 20-50% of the normal cutting amount.
4. The method for machining a large-caliber, long-depth, thin-walled, high-temperature alloy casing of an aircraft engine according to claim 2 or 3, Its characteristics are: When fine milling the circumferential boss while leaving 2mm for the outer circle of the blank and 5mm for the inner circle, control the cutting amount, reduce the internal stress caused by the cutting force during the milling process, and control the deformation of the parts.
5. The method for machining a large-caliber, long-depth, thin-walled, high-temperature alloy casing of an aircraft engine according to claim 1 or 2, Its characteristics are: The first residual stress test is carried out on the incoming blank to obtain the reference value of stress. During the test, strain gauges are evenly pasted on the surface of the blank, and then strain measurement, that is, piezoelectric voltage measurement, is carried out. The pasted strain gauges are evenly distributed on the outer surface of the casing blank.
6. The method for machining a large-caliber, long-depth, thin-walled, high-temperature alloy casing of an aircraft engine according to claim 1 or 2, Its characteristics are: 4 to 8 strain gauges are evenly distributed on each vertical section of the outer surface of the receiver blank; the distribution of strain gauges on adjacent vertical sections is staggered.
7. The method for machining a large-caliber, long-depth, thin-walled, high-temperature alloy casing of an aircraft engine according to claim 1 or 2, Its characteristics are: Dimension scanning inspection is carried out simultaneously after residual stress detection.
8. The method for machining a large-caliber, long-depth, thin-walled, high-temperature alloy casing of an aircraft engine according to claim 2, Its characteristic is that the residual stress Analysis: Check the deformation of the parts. If the tolerance meets the requirements of part processing, it means that the influence of the stress value on the parts is within the controllable range; if the tolerance exceeds the tolerance, it means that the processing parameters need to be changed to reduce the stress; Analysis and adjustment of processing parameters, control of the cutting amount per unit time: By detecting the deformation of the parts, if the tolerance meets the requirements of part processing, it means that the influence of the stress value on the parts is within the controllable range, and the original cutting amount per unit time is used; if the stress value and tolerance exceed the tolerance, it means that the processing parameters need to be changed to reduce the stress and reduce the cutting amount per unit time; The results of the analysis and the control of the cutting amount of the present invention: By detecting the dimensional deformation of the parts, it is possible to determine whether the stress distribution and stress value exceed the standard. If the deformation is large and exceeds the tolerance range, the corresponding processing parameters need to be adjusted.
Citation Information
Patent Citations
Method for measuring marine diesel engine fuselage surface stress distribution law
CN110736577A
Precision machining method for long-wheelbase variable-diameter complex thin-wall structural part
CN113500359A
Integral machining method for ultra-thin wall easy-to-deform aluminum alloy multi-petal shunt ring of aero-engine
CN116803596A
Cited By
Machining method for driving ring of gas compressor
CN120644924A
Workpiece measuring method and non-contact measuring platform
CN120720987A