Aluminum alloy hub polishing and coating process
Through a multi-step process, the aluminum alloy wheel hub is polished and coated with specific abrasive particles and passivation liquid, solving the problem of low polishing accuracy in the automatic polishing process and achieving the formation of high finish and protective surfaces.
Patent Information
- Application Number
- CN202411275294.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-12
- Publication Date
- 2024-11-29
AI Technical Summary
The existing automatic precision polishing process has low polishing accuracy for aluminum alloy wheel hubs, and there are problems of polishing patterns and uneven brightness.
Using multi-step processes, including coarse washing, water-polishing grinding, mechanical polishing, rinsing, water-polishing and coating, the hub surface is gradually removed using conical abrasive particles containing resin components, porcelain grinding balls and chromium-free passivation liquid. blemishes and inhomogeneity form high finish and protective surfaces.
Through multi-step fine processing, the polishing accuracy and protection of the wheel hub are significantly improved, scratches and uneven brightness problems are eliminated, and the aesthetics and corrosion resistance of the wheel hub are improved.
Abstract
Description
Technical Field
[0001] The present application relates to the field of wheel hub polishing and coating technology, and in particular to an aluminum alloy wheel hub polishing and coating technology. Background Art
[0002] As one of the important parts of modern cars, wheels not only bear the weight and stress of the vehicle during driving, but are also an indispensable aesthetic element in the vehicle's exterior design. Common car wheels include steel wheels and aluminum alloy wheels. Steel wheels have high strength and are often used in large trucks; however, steel wheels are heavy and have a single appearance, which does not conform to today's low-carbon and fashionable concepts, and are gradually being replaced by aluminum alloy wheels.
[0003] In order to improve the corrosion resistance and glossiness of the wheel hub and protect it from the external environment, polishing coating technology came into being. Polishing the wheel hub can not only make the wheel hub surface more corrosion-resistant and wear-resistant, but also make the wheel hub surface smoother and improve the appearance of the wheel hub.
[0004] The polishing methods commonly used in the production process are mainly divided into manual polishing, mechanical polishing, electrolytic polishing and chemical polishing.
[0005] At present, the existing automatic fine polishing process usually uses a vibration polishing machine to perform vibration polishing on the aluminum alloy wheel hub. The inventor believes that the wheel hub surface treated by this polishing process has grinding lines and has the defect of low polishing accuracy. Summary of the invention
[0006] In order to alleviate the problem of low wheel hub polishing precision, the present application provides an aluminum alloy wheel hub polishing and coating process.
[0007] The present application provides an aluminum alloy wheel hub polishing and coating process, which adopts the following technical solutions: A polishing and coating process for an aluminum alloy wheel hub mainly comprises the following steps: S1. Rough cleaning: remove the aluminum chips and cutting fluid remaining on the wheel hub after machining the wheel hub; S2, water polishing: add conical abrasive particles containing resin components into the water polishing machine, grind the inside and outside of the wheel hub, and remove the machine tool marks on the wheel hub surface; S3, Mechanical polishing: Use the polishing machine cloth wheel to polish the spokes, rim and mounting plate of the wheel hub. First, use a hard polishing cloth combined with white coarse-grained abrasive paste to further polish the wheel hub surface, and then use a soft polishing cloth combined with fine-grained abrasive paste to polish the wheel hub to remove the cloth wheel mark left by the hard polishing cloth on the wheel hub surface; S4, flushing: perform ultrasonic degreasing cleaning and pure water spray cleaning on the polished wheel hub to remove the polishing paste remaining on the polished wheel hub; S5. Water polishing: Use porcelain grinding balls in a water polishing machine to water polish the entire wheel hub to eliminate scratches on the wheel hub surface and uneven brightness of the wheel hub that may appear during mechanical polishing; S6. Coating: Use electroplating equipment and chromium-free passivation liquid to electroplate a protective film on the surface of the wheel hub to prevent the wheel hub from oxidation.
[0008] By adopting the above technical scheme, before mechanical polishing, the wheel hub is first water-polished using conical abrasive particles containing resin components to remove knife marks and minor flaws on the wheel hub surface, and then the wheel hub is mechanically polished. After mechanical polishing, the entire wheel hub is water-polished again using ceramic grinding balls. Taking advantage of the characteristics of ceramic grinding balls with moderate hardness, low wear, and not easy to scratch the wheel hub surface, the wheel hub surface is finely polished under the action of water flow to eliminate scratches and uneven brightness that may be caused during mechanical polishing. After water polishing again, a protective film is electroplated on the wheel hub surface using a liquid prepared by electroplating equipment and chromium-free passivation liquid to prevent the wheel hub from oxidizing. Through multiple steps of fine processing, the wheel hub surface achieves extremely high smoothness and protection, alleviating the problem of low wheel hub polishing accuracy.
[0009] Optionally, in the S1 rough cleaning, the wheel hub is first placed in an ultrasonic cleaning machine for ultrasonic degreasing cleaning, and then the wheel hub is sprayed with pure water for cleaning.
[0010] By adopting the above technical solution, a combination of ultrasonic degreasing cleaning and pure water spray cleaning is used. Ultrasonic degreasing cleaning can penetrate into the tiny pores on the surface of the wheel hub and remove hard-to-reach oil stains and impurities; pure water spray cleaning ensures that the surface of the wheel hub is thoroughly rinsed clean without any residue.
[0011] Optionally, in the S1 rough washing, before the wheel hub is ultrasonically degreased, the ultrasonic cleaning machine is started to heat each station to 50 degrees Celsius, the conductivity of the cleaning water is less than 150us / cm before the cleaning agent is added, and the temperature of each station is maintained at 40-50 degrees Celsius during the cleaning process. The ultrasonic degreasing cleaning time is 30-40s, the cleaning agent concentration is 3%-5%, and the free alkali concentration is 2%-3%; the pure water spray cleaning time is 30-40s, and the PH of the spraying water is less than 7.5.
[0012] Optionally, in the S2 water polishing, the conical abrasive particles include conical abrasive particles with a diameter of 5 mm and conical abrasive particles with a diameter of 7 mm, the ratio of the conical abrasive particles with a diameter of 5 mm to the conical abrasive particles with a diameter of 7 mm is 3:7, and the water polishing time is 500-600s.
[0013] By adopting the above technical solution, conical abrasive particles with a diameter of 5 mm and conical abrasive particles with a diameter of 7 mm are mixed in a ratio of 3:7 and added to a water polishing machine to grind the wheel hub. The smaller particles can penetrate deeper into the tiny bumps on the surface of the wheel hub, which helps to remove finer machine tool marks and unevenness. The larger particles are more suitable for removing larger surface defects and deeper knife marks, while improving the grinding efficiency. The mixed use of the two particles helps to achieve more uniform and more effective surface treatment during the grinding process.
[0014] Optionally, in the S3 mechanical polishing, the rotation speed of the polishing machine cloth wheel is 1300r / min, the pressure applied by the polishing machine cloth wheel to the hub surface is 14-17mpa, the rotation speed of the hub is 50-100r / min, the hub rotates forward and reverse alternately during the polishing process, and the mechanical polishing time is 300-400s.
[0015] By adopting the above technical solution, the rotation speed of the polishing machine cloth wheel is set to 1300r / min, ensuring that the cloth wheel can generate sufficient linear speed and friction during the polishing process, thereby effectively removing tiny flaws and unevenness on the hub surface, while also avoiding overheating and excessive wear, and protecting the hub surface from damage; the hub rotates on its own during the polishing process, which can help disperse the heat and stress generated during the polishing process and reduce damage to the hub surface caused by overheating or excessive stress; by alternating forward and reverse rotation of the hub, it helps to eliminate polishing marks and stress concentration caused by unidirectional rotation, and can enable the polishing machine cloth wheel to form a more uniform polishing track on the hub surface, thereby improving the polishing effect and quality.
[0016] Optionally, the water polishing and fine polishing in step S5 includes two processes of initial polishing and final polishing. The initial polishing and final polishing respectively use ceramic grinding balls of different diameters to polish the wheel hub in a water polishing machine. The diameter of the ceramic grinding balls used in the initial polishing is larger than the diameter of the ceramic grinding balls used in the final polishing. During the initial polishing, the wheel hub rotates forward for 200-300 seconds and reversely for 200-300 seconds at a speed of 40-50r / min. During the final polishing, the wheel hub rotates forward for 100-200 seconds and reversely for 100-200 seconds at a speed of 40-50r / min.
[0017] By adopting the above technical solution, the initial polishing process removes large defects and unevenness, providing a good foundation for the final polishing. The final polishing process further refines the surface, eliminates tiny scratches and unevenness, and improves polishing efficiency.
[0018] Optionally, in the S6 coating, the concentration of the chromium-free passivation solution is between 5.5% and 7.5%, the pH value of the passivation solution is between 3.8 and 4.2, the water temperature is controlled between 30 and 40 degrees Celsius, and the coating time is 300 seconds.
[0019] By adopting the above technical scheme, the pH value of the passivation solution is controlled between 3.8 and 4.2. Within this pH value range, the chromium-free passivation solution can maintain good stability and activity, which is conducive to forming a dense and uniform passivation film on the surface of the wheel hub. At the same time, the appropriate pH value can also reduce the harmful gases and waste liquids generated during the passivation process, reducing pollution to the environment; in addition, the water temperature is controlled between 30 and 40 degrees Celsius. Within this temperature range, the effective ingredients in the chromium-free passivation solution can be fully dissolved and evenly distributed in the solution, which is conducive to forming a uniform and dense coating layer on the surface of the wheel hub; appropriate water temperature can also increase the coating rate, shorten the coating time, and improve production efficiency; too high water temperature may cause the effective ingredients in the passivation solution to decompose or volatilize, affecting the coating effect; too low water temperature may reduce the coating rate and increase production costs.
[0020] In summary, the present application includes at least one of the following beneficial technical effects: Before mechanical polishing, the wheel hub is first water-polished with conical abrasive particles containing resin components to remove knife marks and minor flaws on the wheel hub surface, and then the wheel hub is mechanically polished. After mechanical polishing, the entire wheel hub is water-polished again with ceramic grinding balls. The characteristics of ceramic grinding balls are moderate hardness, low wear, and not easy to scratch the wheel hub surface. The wheel hub surface is finely polished under the action of water flow to eliminate scratches and uneven brightness that may be caused during mechanical polishing. After water polishing again, a protective film is electroplated on the wheel hub surface using electroplating equipment and chromium-free passivation liquid to prevent the wheel hub from oxidizing. Through multiple steps of fine processing, the wheel hub surface reaches extremely high finish and protection, alleviating the problem of low wheel hub polishing accuracy. By mixing 5mm diameter conical abrasive particles and 7mm diameter conical abrasive particles in a ratio of 3:7 and adding them to the water polishing machine to grind the wheel hub, the smaller particles can penetrate deeper into the tiny bumps on the wheel hub surface, helping to remove finer machine tool knife marks and unevenness, while the larger particles are more suitable for removing larger surface defects and deeper knife marks, while improving grinding efficiency. The mixed use of the two particles helps to achieve more uniform and more effective surface treatment during the grinding process; By setting the speed of the polishing machine cloth wheel to 1300r / min, it is ensured that the cloth wheel can generate sufficient linear speed and friction during the polishing process, thereby effectively removing minor flaws and unevenness on the wheel hub surface, while also avoiding overheating and excessive wear, and protecting the wheel hub surface from damage. The wheel hub rotates on its own during the polishing process, which can help disperse the heat and stress generated during the polishing process and reduce damage to the wheel hub surface caused by overheating or excessive stress. By alternating forward and reverse rotation of the wheel hub, it helps to eliminate polishing marks and stress concentration caused by unidirectional rotation, and can enable the polishing machine cloth wheel to form a more uniform polishing track on the wheel hub surface, thereby improving the polishing effect and quality. DETAILED DESCRIPTION
[0021] In order to more clearly explain the overall concept of the present application, the present application is further described in detail below.
[0022] In the following description, many specific details are set forth to facilitate a full understanding of the present application. However, the present application may also be implemented in other ways different from those described herein. Therefore, the protection scope of the present application is not limited by the specific embodiments disclosed below. It should be noted that the embodiments of the present application and the features in each embodiment may be combined with each other without conflict.
[0023] In this application, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection, an electrical connection, or a communication; it can be a direct connection, or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to specific circumstances.
[0024] The embodiment of the present application discloses a polishing and coating process for an aluminum alloy wheel hub. The polishing and coating process for an aluminum alloy wheel hub mainly comprises the following steps: S1. Rough cleaning: Start the ultrasonic cleaning machine to heat each station to 50 degrees Celsius, put the wheel hub into the ultrasonic cleaning machine for ultrasonic degreasing cleaning, and keep the temperature of each station at 40-50 degrees Celsius during the cleaning process, 45 degrees Celsius in this embodiment, the conductivity of the cleaning water before adding the cleaning agent is less than 150us / cm, the ultrasonic degreasing cleaning time is 30-40s, 30s in this embodiment, the cleaning agent concentration is 3%-5%, 5% in this embodiment, and the free alkali concentration is 2%-3%, 3% in this embodiment; then the wheel hub is sprayed with pure water, the pH of the spraying water is less than 7.5, and the cleaning time is 30-40s, 40s in this embodiment, so as to remove the aluminum chips and cutting fluid remaining on the wheel hub after the machine tool processing.
[0025] By combining ultrasonic degreasing cleaning with pure water spray cleaning, ultrasonic degreasing cleaning can penetrate into the tiny pores on the wheel hub surface to remove hard-to-reach oil stains and impurities; pure water spray cleaning ensures that the wheel hub surface is thoroughly rinsed clean without any residue.
[0026] S2. Water polishing: Conical abrasive particles containing resin components are added into the water polishing machine. The conical abrasive particles include conical abrasive particles with a diameter of 5 mm and conical abrasive particles with a diameter of 7 mm. The ratio of the conical abrasive particles with a diameter of 5 mm to the conical abrasive particles with a diameter of 7 mm is 3:7. The inside and outside of the wheel hub are polished. The water polishing time is 500-600 seconds, 500 seconds in this embodiment, to remove the machine tool marks on the surface of the wheel hub.
[0027] By mixing 5mm diameter conical abrasive particles and 7mm diameter conical abrasive particles in a ratio of 3:7 and adding them to a water polishing machine to grind the wheel hub, the smaller particles can penetrate deeper into the tiny bumps on the wheel hub surface, helping to remove finer machine tool tool marks and unevenness, while the larger particles are more suitable for removing larger surface defects and deeper tool marks, while improving grinding efficiency. The mixed use of the two particles helps to achieve more uniform and more effective surface treatment during the grinding process.
[0028] S3. Mechanical polishing: polish the spokes, rim and mounting plate of the wheel hub using a polishing machine cloth wheel. First, use a hard polishing cloth combined with white coarse-grained abrasive paste to further polish the surface of the wheel hub, and then use a soft polishing cloth combined with fine-grained abrasive paste to polish the wheel hub to eliminate the cloth wheel mark left by the hard polishing cloth on the surface of the wheel hub. The rotation speed of the polishing machine cloth wheel is 1300r / min, and the pressure applied by the polishing machine cloth wheel to the surface of the wheel hub is 14-17mpa, which is 14mpa in this embodiment. The rotation speed of the wheel hub is 50-100r / min, which is 50r / min in this embodiment. The wheel hub rotates forward and reverse alternately during the polishing process. The mechanical polishing time is 300-400s, which is 400s in this embodiment.
[0029] By setting the speed of the polishing machine cloth wheel to 1300r / min, it is ensured that the cloth wheel can generate sufficient linear speed and friction during the polishing process, thereby effectively removing tiny flaws and unevenness on the wheel hub surface, while avoiding overheating and excessive wear, and protecting the wheel hub surface from damage; the wheel hub rotates on its own during the polishing process, which can help disperse the heat and stress generated during the polishing process and reduce damage to the wheel hub surface caused by overheating or excessive stress; by alternating forward and reverse rotation of the wheel hub, it helps to eliminate polishing marks and stress concentration caused by unidirectional rotation, and can make the polishing machine cloth wheel form a more uniform polishing track on the wheel hub surface, thereby improving the polishing effect and quality.
[0030] S4. Rinse: Perform ultrasonic degreasing cleaning and pure water spray cleaning on the polished wheel hub to remove the polishing paste remaining on the polished wheel hub.
[0031] S5. Water polishing and fine polishing: Use porcelain grinding balls in the water polishing machine to water polish the entire wheel hub, including the initial polishing and final polishing. The initial polishing and final polishing use porcelain grinding balls of different diameters to polish the wheel hub in the water polishing machine. The diameter of the porcelain grinding balls used in the initial polishing is larger than that of the porcelain grinding balls used in the final polishing. During the initial polishing process, the wheel hub rotates forward for 200-300 seconds and reverse for 200-300 seconds at a speed of 40-50r / min. During the final polishing process, the wheel hub rotates forward for 100-200 seconds. , reverse 100-200s, the speed is 40-50r / min. In this embodiment, a ceramic grinding ball with a diameter of 3mm is used for the initial polishing. During the initial polishing, the wheel hub rotates forward for 200s, reverses for 200s, and the speed is 40r / min. A ceramic grinding ball with a diameter of 1mm is used for the final polishing. During the final polishing, the wheel hub rotates forward for 200s, reverses for 200s, and the speed is 40r / min, thereby eliminating scratches on the surface of the wheel hub and uneven brightness of the wheel hub during mechanical polishing.
[0032] The initial polishing process removes large defects and unevenness, providing a good foundation for the final polishing process. The final polishing process further refines the surface, eliminates tiny scratches and unevenness, and improves polishing efficiency.
[0033] S6. Coating: A protective film is electroplated on the surface of the wheel hub using electroplating equipment and a liquid prepared from a chromium-free passivation liquid to prevent oxidation of the wheel hub. The concentration of the chromium-free passivation liquid is between 5.5% and 7.5%, and is 5.5% in this embodiment. The pH value of the passivation liquid is between 3.8 and 4.2, and is 4.2 in this embodiment. The water temperature is controlled between 30 and 40 degrees Celsius, and is 40 degrees Celsius in this embodiment. The coating time is 300 seconds.
[0034] By controlling the pH value of the passivation solution between 3.8 and 4.2, within this pH range, the chromium-free passivation solution can maintain good stability and activity, which is conducive to forming a dense and uniform passivation film on the surface of the wheel hub. At the same time, the appropriate pH value can also reduce the harmful gases and waste liquids generated during the passivation process, reducing pollution to the environment; in addition, the water temperature is controlled between 30 and 40 degrees Celsius. Within this temperature range, the effective ingredients in the chromium-free passivation solution can be fully dissolved and evenly distributed in the solution, which is conducive to forming a uniform and dense coating layer on the surface of the wheel hub; appropriate water temperature can also increase the coating rate, shorten the coating time, and improve production efficiency; too high water temperature may cause the effective ingredients in the passivation solution to decompose or volatilize, affecting the coating effect; too low water temperature may reduce the coating rate and increase production costs.
[0035] Anything not described in this application can be achieved by adopting or drawing on existing technologies.
[0036] The various embodiments in this specification are described in a progressive manner, and the same or similar parts between the various embodiments can be referenced to each other, and each embodiment focuses on the differences from other embodiments.
[0037] The above are all preferred embodiments of the present application, and the protection scope of the present application is not limited thereto. Therefore, any equivalent changes made according to the structure, shape, and principle of the present application should be included in the protection scope of the present application.
Claims
1. A polishing and coating process for an aluminum alloy wheel hub, characterized in that: The main steps include: S1. Rough cleaning: remove the aluminum chips and cutting fluid remaining on the wheel hub after machining the wheel hub; S2, water polishing: add conical abrasive particles containing resin components into the water polishing machine, grind the inside and outside of the wheel hub, and remove the machine tool marks on the wheel hub surface; S3, Mechanical polishing: Use the polishing machine cloth wheel to polish the spokes, rim and mounting plate of the wheel hub. First, use a hard polishing cloth combined with white coarse-grained abrasive paste to further polish the wheel hub surface, and then use a soft polishing cloth combined with fine-grained abrasive paste to polish the wheel hub to remove the cloth wheel mark left by the hard polishing cloth on the wheel hub surface; S4, flushing: perform ultrasonic degreasing cleaning and pure water spray cleaning on the polished wheel hub to remove the polishing paste remaining on the polished wheel hub; S5. Water polishing: Use porcelain grinding balls in a water polishing machine to water polish the entire wheel hub to eliminate scratches on the wheel hub surface and uneven brightness of the wheel hub that may appear during mechanical polishing; S6. Coating: Use electroplating equipment and chromium-free passivation liquid to electroplate a protective film on the surface of the wheel hub to prevent the wheel hub from oxidation.
2. The aluminum alloy wheel hub polishing and coating process according to claim 1, characterized in that: In the S1 rough cleaning, the wheel hub is first placed in an ultrasonic cleaning machine for ultrasonic degreasing cleaning, and then the wheel hub is sprayed with pure water for cleaning.
3. The aluminum alloy wheel hub polishing and coating process according to claim 1, characterized in that: In the S1 rough washing, before the wheel hub is ultrasonically degreased, the ultrasonic cleaning machine is started to heat each station to 50 degrees Celsius. The conductivity of the cleaning water is less than 150us / cm before the cleaning agent is added. During the cleaning process, the temperature of each station is maintained at 40-50 degrees Celsius. The ultrasonic degreasing cleaning time is 30-40s, the cleaning agent concentration is 3%-5%, and the free alkali concentration is 2%-3%; the pure water spray cleaning time is 30-40s, and the PH of the spraying water is less than 7.
5.
4. The aluminum alloy wheel hub polishing and coating process according to claim 1, characterized in that: In the S2 water polishing, the conical abrasive particles include conical abrasive particles with a diameter of 5 mm and conical abrasive particles with a diameter of 7 mm, the ratio of the conical abrasive particles with a diameter of 5 mm to the conical abrasive particles with a diameter of 7 mm is 3:7, and the water polishing time is 500-600s.
5. The aluminum alloy wheel hub polishing and coating process according to claim 1, characterized in that: In the S3 mechanical polishing, the rotation speed of the polishing machine cloth wheel is 1300r / min, the pressure applied by the polishing machine cloth wheel to the hub surface is 14-17mpa, the rotation speed of the hub is 50-100r / min, the hub rotates forward and reverse alternately during the polishing process, and the mechanical polishing time is 300-400s.
6. The aluminum alloy wheel hub polishing and coating process according to claim 1, characterized in that: The step S5 of water polishing and fine polishing includes two processes, namely, initial polishing and final polishing. The wheel hub is polished in a water polishing machine using ceramic grinding balls of different diameters for the initial polishing and the final polishing respectively. The diameter of the ceramic grinding balls used for the initial polishing is larger than the diameter of the ceramic grinding balls used for the final polishing. During the initial polishing, the wheel hub rotates forward for 200-300 seconds and reversely for 200-300 seconds at a speed of 40-50 r / min. During the final polishing, the wheel hub rotates forward for 100-200 seconds and reversely for 100-200 seconds at a speed of 40-50 r / min.
7. The aluminum alloy wheel hub polishing and coating process according to claim 1, characterized in that: In the S6 coating, the concentration of the chromium-free passivation solution is between 5.5% and 7.5%, the pH value of the passivation solution is between 3.8 and 4.2, the water temperature is controlled between 30 and 40 degrees Celsius, and the coating time is 300 seconds.
Citation Information
Patent Citations
Aluminum alloy hub polishing process
CN105538051A
Hub surface pretreatment process
CN108866556A
Hub polishing process
CN110877283A
Aluminum alloy wheel hub surface treatment method
CN111496581A
Automobile hub surface treatment method
CN112522751A