Production method of high-purity silver nitrate

Through the collaborative process of composite decompression remover and nitric acid modified carbon materials, the problems of poor impurity removal and high cost in the production of high-purity silver nitrate in the existing technology are solved, and efficient and low-cost high-purity silver nitrate production are achieved. Meet the high purity needs of the photosensitive industry.

CN119038592APending Publication Date: 2024-11-29HUNAN YINHAI NEW MATERIAL TECHNOLOGY CO LTD

Patent Information

Application Number
CN202411250763.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-06
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The existing high-purity silver nitrate production methods have problems such as poor performance, high cost, long time and unsuitable for large-scale industrial production, especially in the photosensitive industry, which is difficult to meet the high purity needs.

Method used

The synergistic process of composite impurity removal agent and nitric acid modified carbon material is adopted to achieve efficient removal of metal impurity ions by silver oxide and aluminum nitrate or aluminum hydroxide as impurity removal agents, and nitric acid modified carbon material is used for adsorption.

Benefits of technology

It realizes efficient and low-cost continuous production, ensures high purity of silver nitrate, and has a metal ion content of less than 1ppm. It is suitable for industrial production and is environmentally friendly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005032180440000061
    Figure BDA0005032180440000061
Patent Text Reader

Abstract

The invention discloses a production method of high-purity silver nitrate, the method comprises the steps of silver washing, silver dissolving, impurity removal and evaporative crystallization, and impurity removal comprises the steps of impurity removal by adopting a composite impurity removal agent and secondary impurity removal by adopting a nitric acid modified carbon material. According to the method, the nitric acid modified carbon material adsorbent which is low in price and easy to obtain is adopted, efficient adsorption of impurity ions is achieved, the nitric acid modified carbon material adsorbent is cooperatively combined with the composite impurity removal agent, the problems that a single impurity removal agent or adsorbent is limited in use effect, high in cost and the like are solved, efficient and low-cost removal of the impurity ions is achieved, and the method can be used for continuously and efficiently producing high-purity silver nitrate products.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for producing high-purity silver nitrate, in particular to a method for producing high-purity silver nitrate by a composite impurity removal method using a composite impurity remover and an adsorbent. Background Art

[0002] Silver nitrate is a colorless, transparent, rhombic, flaky crystal that tastes bitter and is toxic. It is easily soluble in water and ammonia, slightly soluble in ethanol, poorly soluble in acetone and benzene, and almost insoluble in concentrated nitric acid. Silver nitrate aqueous solution is weakly acidic, with a pH of 5 to 6. Silver nitrate is a raw material for the production of various photosensitive materials, silver-plated products, pharmaceutical and antibacterial materials, silver oxide, silver powder, silver paste and other deep-processing products, especially high-purity photographic grade silver nitrate (see national standard YST476-2022 Silver nitrate for photography), which has a wide range of applications in various industries.

[0003] The traditional method of producing silver nitrate is to clean the silver ingot with deionized water and then react it with dilute nitric acid to make a crude silver nitrate solution, and then prepare silver nitrate crystals through processes such as impurity removal, evaporation concentration, crystallization, centrifugation, drying and packaging. The silver nitrate produced by this method has a high content of metal ions such as Fe, Cu, and Pb, which can no longer meet the needs of industry development, especially the photosensitive industry. Therefore, it is inevitable to develop and produce a high-purity silver nitrate that meets the new needs of the photosensitive industry.

[0004] Chinese patent document CN1386707A discloses a method for producing high-purity silver nitrate, which includes adding nitric acid to a heated silver nitrate solution and blowing gas into it before cooling and crystallizing. The silver nitrate produced by this method has a high content of metal impurity ions and is difficult to meet the needs of photosensitive materials.

[0005] Chinese patent document CN102040241A discloses a method for preparing high-purity silver nitrate by using magnesium carbonate as an impurity remover and then evaporating and crystallizing. This method does not remove impurities thoroughly and introduces new impurities, and the impurity ion content reaches more than 100 ppb.

[0006] Chinese patent document CN116692927A discloses a process for producing silver nitrate by using a chelating resin combined with ultrasound and triple-effect flash evaporation. This method is costly and energy intensive and is not suitable for large-scale industrial production.

[0007] Chinese patent document CN116462221A discloses a process for producing silver nitrate by using adsorption-ion exchange bifunctional resin and chelating resin for adsorption and impurity removal followed by efficient centrifugal separation. This method only uses adsorption as a means for impurity removal, has a single method, and requires the use of two resin materials for adsorption, which is costly and time-consuming, and is also not suitable for large-scale industrial production.

[0008] The above existing methods for preparing high-purity silver nitrate generally have the following problems:

[0009] 1. The effect of using a single impurity removal method or only crystallization is poor. Impurity ions accumulate during continuous production, and high-purity silver nitrate cannot be stably prepared;

[0010] 2. Although the treatment effect is improved by using resin adsorption to remove impurities, the treatment cost is high or the treatment time is long. The resin recovery is difficult and secondary pollution is likely to occur. It is not suitable for large-scale industrial production.

[0011] In view of this, it is necessary to develop a new production method of high-purity silver nitrate to solve the above problems. Summary of the invention

[0012] The technical problem to be solved by the present invention is to overcome the deficiencies of the prior art and provide a production method for high-purity silver nitrate which has simple process, can be continuously and efficiently produced, has good impurity removal effect, is suitable for industrial production and is environmentally friendly.

[0013] In order to solve the above technical problems, the present invention adopts the following technical solutions.

[0014] A method for producing high-purity silver nitrate comprises the following steps:

[0015] (1) Silver washing: The silver plate is washed with sodium hydroxide solution, washed with water once, washed with nitric acid solution, and washed with water twice to obtain a washed silver plate;

[0016] (2) Silver dissolution: Place the cleaned silver plate into a reaction kettle, add water and nitric acid solution, control the reaction temperature to 60°C to 80°C, and heat to drive out the acid after the reaction;

[0017] (3) Impurity removal: Add water to the solution obtained in step (2) to adjust the density to 1.7 g / cm 3 ~1.8g / cm 3 , then adding a composite impurity remover to adjust the pH value to 6-8, wherein the composite impurity remover is an impurity remover composed of silver oxide and aluminum nitrate or an impurity remover composed of silver oxide and aluminum hydroxide, stirring once and then standing, filtering to obtain a primary filtrate, adding nitric acid-modified carbon material to the primary filtrate, stirring twice and then standing for adsorption, filtering to obtain a secondary filtrate;

[0018] (4) Evaporation and crystallization: adding nitric acid solution to the secondary filtrate obtained in step (3) to adjust the pH value to 1-2, and concentrating by vacuum evaporation, cooling and crystallizing, filtering, and drying to obtain high-purity silver nitrate, wherein the high-purity silver nitrate is photographic grade silver nitrate.

[0019] In the above-mentioned method for producing high-purity silver nitrate, preferably, in step (3), the molar ratio of the silver oxide to aluminum nitrate is 6 to 10:1, or the molar ratio of the silver oxide to aluminum hydroxide is 6 to 10:1.

[0020] In the above-mentioned method for producing high-purity silver nitrate, preferably, in step (3), the nitric acid-modified carbon material includes one or more of nitric acid-modified activated carbon, nitric acid-modified graphene and nitric acid-modified carbon nanotubes; the preparation process of the nitric acid-modified carbon material is as follows: after washing and drying the carbon material, putting it into a 65wt% to 68wt% nitric acid solution, reacting at 60°C to 80°C for 2h to 3h, cooling, filtering, repeatedly washing with water to pH=7, and drying to obtain the nitric acid-modified carbon material.

[0021] In the above-mentioned method for producing high-purity silver nitrate, preferably, in step (3), the amount of nitric acid-modified carbon material added is 2 g / L to 8 g / L.

[0022] In the above-mentioned method for producing high-purity silver nitrate, preferably, in step (3), the first stirring time is 0.5h to 1h, the standing time is 0.5h to 1h, the second stirring time is 0.5h to 1h, and the standing adsorption time is 0.5h to 2h.

[0023] In the above-mentioned method for producing high-purity silver nitrate, preferably, in step (2), the mass fraction of nitric acid in the nitric acid solution is 65% to 68%, the volume ratio of the nitric acid solution to water is 22 to 25:1, and the heating time for driving out the acid is 2h to 3h.

[0024] In the above-mentioned method for producing high-purity silver nitrate, preferably, in step (2), after adding water, a portion of the nitric acid solution is first added, the reaction temperature is raised to 60° C. to 80° C., and then the remaining nitric acid solution is added dropwise.

[0025] In the above-mentioned method for producing high-purity silver nitrate, preferably, in step (4), the concentration of the nitric acid solution is 3wt% to 6wt%, the vacuum degree of the vacuum evaporation concentration is -65kPa to -90kPa, and the temperature of the vacuum evaporation concentration is 110°C to 130°C.

[0026] In the above-mentioned method for producing high-purity silver nitrate, preferably, in step (4), the cooling crystallization is carried out under stirring, the stirring rate is 60rpm-80rpm, the cooling crystallization time is 2h-4h, the drying temperature is 85°C-90°C, and the drying time is 5h-8h.

[0027] In the above-mentioned production method of high-purity silver nitrate, preferably, in step (1), the sodium hydroxide solution alkali washing is to put the silver plate into the sodium hydroxide solution for ultrasonic cleaning for 10min to 15min, take it out and drain it for 2min to 5min, and blow it dry with compressed air; the first water washing is to put the silver plate after the alkali washing into deionized water for ultrasonic cleaning for 10min to 15min, take it out and drain it for 2min to 5min, and blow it dry with compressed air; the nitric acid solution acid washing is to put the silver plate after the first water washing into the nitric acid solution for ultrasonic cleaning for 10min to 15min, take it out and drain it for 2min to 5min, and blow it dry with compressed air; the second water washing is to put the silver plate after the acid washing into deionized water for ultrasonic cleaning for 10min to 15min, take it out and drain it for 2min to 5min, and blow it dry with compressed air; the silver plate adopts the national standard No. 1 silver plate, the mass fraction of the sodium hydroxide solution is 5% to 8%, and the mass fraction of the nitric acid solution is 5% to 8%.

[0028] Compared with the prior art, the advantages of the present invention are:

[0029] The method of the present invention cooperates with a two-step impurity removal process, first using silver oxide and aluminum nitrate or aluminum hydroxide as a composite impurity remover to precipitate metal impurity ions, and then using cheap and readily available nitric acid-modified carbon materials as adsorbents to achieve efficient adsorption of impurity ions. The two work together to overcome the problem of limited effects of existing impurity removers. In the prior art, the adsorption capacity of ordinary activated carbon used in the activated carbon adsorption method is not high and the effect is limited. The present invention chemically modifies the activated carbon to enhance its adsorption performance. At the same time, the present invention has lower cost and is easier to manufacture and obtain than chelating resins and ion exchange resins, achieving efficient and low-cost removal of impurity ions. The method of the present invention can continuously and efficiently produce high-purity silver nitrate products, ensuring that the content of each metal ion in the final silver nitrate product is less than 1ppm. DETAILED DESCRIPTION

[0030] The present invention is further described below in conjunction with specific preferred embodiments, but the protection scope of the present invention is not limited thereby. The materials and instruments used in the following embodiments are all commercially available.

[0031] Example 1

[0032] A method for producing high-purity silver nitrate of the present invention comprises the following steps:

[0033] (1) Silver washing: Take 400 kg of national standard No. 1 silver plate and put it into a metal basket. Start the electric hoist and lift the metal basket into an alkali washing tank filled with sodium hydroxide solution. Ultrasonicate for 10 minutes, then lift it up to drain for 2 minutes and blow it dry with compressed air. Then lift the metal basket into the primary washing tank, acid washing tank and secondary washing tank respectively and perform the same operation (i.e. ultrasonicate for 10 minutes, then lift it up to drain for 2 minutes and blow it dry with compressed air). The alkali solution used in the alkali washing tank is a 5wt% sodium hydroxide solution, the acid solution used in the acid washing tank is a 5wt% dilute nitric acid solution, and the primary washing tank and the secondary washing tank are both filled with deionized water. After the secondary washing, use pH test paper to measure the surface water of the silver plate and control the pH value between 6 and 8.

[0034] (2) Silver dissolution: Slide the cleaned silver plate into the reactor mouth, add 15L of deionized water, first add 45L of 65wt% nitric acid solution, heat the reactor to 65°C, then control the dripping rate of the nitric acid solution to 130L / h (to prevent the generation of a large amount of yellow smoke and cause material impact), continue to add 300L of 65wt% nitric acid solution to react, after the acid is added (after the reaction), heat the reactor to 120°C for high-temperature acid removal for 2h, and when the solution color becomes significantly lighter and basically no bubbles are generated, the reaction is finished.

[0035] (3) Impurity removal: The above reaction solution was passed into an impurity removal kettle and diluted with deionized water to 1.7-1.8 g / cm 3 On the one hand, water can be used to wash the inner wall of the kettle to reduce the residual silver nitrate solution on the inner wall. On the other hand, the concentration of the silver nitrate reaction solution is high, and it is easy to precipitate after stopping heating, causing great loss during filtration. Adding water to dilute can prevent precipitation. Add 7kg of composite impurity remover to adjust the pH to 6. The composite impurity remover is composed of silver oxide and aluminum nitrate. The molar ratio of silver oxide to aluminum nitrate is 7:1. Stir once for 0.5h, let stand for 0.5h, filter, and obtain a primary filtrate. Add 3kg of nitric acid-modified graphene to the primary filtrate, so that the amount of nitric acid-modified carbon material added is 6g / L. Stir twice for 0.5h, let stand for 0.5h for adsorption, filter, and obtain a secondary filtrate.

[0036] In this embodiment, the preparation process of nitric acid-modified graphene is as follows: after washing and drying the graphene, it is put into a 65wt% nitric acid solution, reacted at 70°C for 2h, cooled, filtered, repeatedly rinsed with water to pH=7, and dried to obtain nitric acid-modified graphene.

[0037] (4) Evaporation and crystallization: 5 wt % dilute nitric acid was added to the secondary filtrate to adjust the pH value to 2, and the filtrate was sent to an evaporation and concentration kettle. The vacuum degree was adjusted to -80 kPa, and the temperature was raised to 130° C. The evaporation and concentration were carried out under vacuum with stirring. After the evaporation liquid was evaporated with stirring until a crystal film appeared, the evaporation was continued for 0.5 h. The evaporation liquid was introduced into a crystallization kettle while it was hot. The crystallization kettle was turned on and stirred at a rate of 60 rpm. Cooling water was introduced into the jacket of the crystallization kettle. The crystallization was cooled and crystallized for 2 h. After the crystallization was completed, the silver nitrate crystals were filtered to obtain the silver nitrate crystals. The silver nitrate crystals were transferred into an oven and dried at 90° C. for 6 h to obtain high-purity silver nitrate that met the national standard for photographic grade.

[0038] Experimental Example 2

[0039] A method for producing high-purity silver nitrate of the present invention comprises the following steps:

[0040] (1) Silver washing: Take 840 kg of national standard No. 1 silver plate and put it into a metal basket. Start the electric hoist and lift the metal basket into an alkali washing tank filled with sodium hydroxide solution. Ultrasonicate for 15 minutes, then lift it up to drain for 2 minutes and blow it dry with compressed air. Then lift the metal basket into the primary washing tank, acid washing tank and secondary washing tank respectively and perform the same operation (i.e. ultrasonicate for 15 minutes, then lift it up to drain for 2 minutes and blow it dry with compressed air). The alkali solution used in the alkali washing tank is a 5wt% sodium hydroxide solution, the acid solution used in the acid washing tank is a 5wt% dilute nitric acid solution, and the primary washing tank and the secondary washing tank are both filled with deionized water. After the secondary washing, use pH test paper to measure the surface water of the silver plate and control the pH value to between 6 and 8.

[0041] (2) Silver dissolution: Slide the cleaned silver plate into the reactor from the mouth, add 30L of deionized water, add 90L of 65wt% nitric acid solution, heat the reactor to 70°C, control the nitric acid solution dripping speed to 130L / h, continue to add 615L of 65wt% nitric acid solution to react, after the acid addition is completed, raise the temperature of the reactor to 120°C for high-temperature acid removal for 2.5h. When the color of the solution becomes significantly lighter and almost no bubbles are generated, the reaction is completed.

[0042] (3) Impurity removal: The reaction solution obtained in step (2) above was passed into an impurity removal kettle and diluted with deionized water to 1.7-1.8 g / cm 3 , add 14kg of composite impurity remover to adjust the pH value to 6, the composite impurity remover is composed of silver oxide and aluminum hydroxide, the molar ratio of silver oxide to aluminum hydroxide is 7:1, stir once for 0.5h, let stand for 0.5h, filter to obtain a primary filtrate, add 5kg of nitric acid-modified graphene to the primary filtrate, that is, the addition amount of nitric acid-modified graphene is 7g / L, stir twice for 0.5h, let stand for adsorption for 0.5h, filter to obtain a secondary filtrate;

[0043] (4) Evaporation and crystallization: 5 wt % dilute nitric acid was added to the secondary filtrate to adjust the pH to 2, and the filtrate was sent to an evaporation and concentration kettle. The vacuum degree was adjusted to -80 kPa, and the temperature was raised to 120° C. The evaporation and concentration were carried out under vacuum with stirring. After the evaporation liquid was evaporated with stirring until a crystal film appeared, the evaporation was continued for 0.5 h. The evaporation liquid was introduced into a crystallization kettle while it was hot. The crystallization kettle was turned on and stirred at a rate of 60 rpm. Cooling water was introduced into the jacket of the crystallization kettle. The crystallization was cooled and crystallized for 2 h. After the crystallization was completed, the silver nitrate crystals were filtered to obtain the silver nitrate crystals. The silver nitrate crystals were transferred into an oven and dried at 90° C. for 6 h to obtain high-purity silver nitrate that met the national standard for photographic grade.

[0044] Comparative Example 1

[0045] A method for producing silver nitrate is basically the same as that of Example 2, except that in step (3), no nitric acid-modified graphene is added to the primary filtrate, and the next step (4) is directly performed.

[0046] Comparative Example 2

[0047] A method for producing silver nitrate is basically the same as that of Example 2, except that in step (3), the composite impurity remover is replaced by silver oxide.

[0048] The specific process of step (3) is as follows: the reaction solution obtained in step (2) is passed into a de-impurity kettle and diluted with deionized water to 1.7-1.8 g / cm 3 , add 14 kg of silver oxide, stir for 0.5 h once, let stand for 0.5 h, filter to obtain a primary filtrate, add 5 kg of nitric acid-modified graphene to the primary filtrate, stir for a second time for 0.5 h, let stand for 0.5 h, filter to obtain a secondary filtrate.

[0049] Comparative Example 3

[0050] A method for producing silver nitrate is basically the same as Example 2, except that in step (3), the composite impurity remover is replaced by silver oxide, and nitric acid is not added to modify graphene.

[0051] The specific process of step (3) is as follows: the reaction solution obtained in step (2) is passed into a de-impurity kettle and diluted with deionized water to 1.7-1.8 g / cm 3 , add 14 kg of silver oxide, stir for 0.5 h, let stand for 0.5 h, and filter to obtain the filtrate.

[0052] The silver nitrate prepared in Examples 1-2 and Comparative Examples 1-3 was tested for purity, and the data obtained were shown in Table 1 below. As can be seen from Table 1, the silver nitrate produced by the method of the present invention can significantly reduce the content of Fe, Cu, and Pb metal impurities, reaching the national standard of photographic grade silver nitrate.

[0053] Table 1 Silver nitrate purity test results of Examples 1-2 and Comparative Examples 1-3

[0054]

[0055] The above is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as above in the preferred embodiment, it is not used to limit the present invention. Any technician familiar with the art can make many possible changes and modifications to the technical solution of the present invention by using the methods and technical contents disclosed above without departing from the spirit and technical solution of the present invention, or modify it into an equivalent embodiment of equivalent changes. Therefore, any simple modification, equivalent replacement, equivalent change and modification made to the above embodiments according to the technical essence of the present invention without departing from the content of the technical solution of the present invention, still fall within the scope of protection of the technical solution of the present invention.

Claims

1. A method for producing high-purity silver nitrate, characterized in that: The following steps are involved: (1) Silver washing: The silver plate is washed with sodium hydroxide solution, washed with water once, washed with nitric acid solution, and washed with water twice to obtain a washed silver plate; (2) Silver dissolution: Place the cleaned silver plate into a reaction kettle, add water and nitric acid solution, control the reaction temperature to 60°C to 80°C, and heat to drive out the acid after the reaction; (3) Impurity removal: Add water to the solution obtained in step (2) to adjust the density to 1.7 g / cm 3 ~1.8g / cm 3 , then adding a composite impurity remover to adjust the pH value to 6-8, wherein the composite impurity remover is an impurity remover composed of silver oxide and aluminum nitrate or an impurity remover composed of silver oxide and aluminum hydroxide, stirring once and then standing, filtering to obtain a primary filtrate, adding nitric acid-modified carbon material to the primary filtrate, stirring twice and then standing for adsorption, filtering to obtain a secondary filtrate; (4) Evaporation and crystallization: adding nitric acid solution to the secondary filtrate obtained in step (3) to adjust the pH value to 1-2, and concentrating by vacuum evaporation, cooling and crystallizing, filtering, and drying to obtain high-purity silver nitrate, wherein the high-purity silver nitrate is photographic grade silver nitrate.

2. The production method of high-purity silver nitrate according to claim 1, wherein In step (3), the molar ratio of the silver oxide to aluminum nitrate is 6 to 10:1, or the molar ratio of the silver oxide to aluminum hydroxide is 6 to 10:

1.

3. The production method of high-purity silver nitrate according to claim 1, wherein In step (3), the nitric acid-modified carbon material includes one or more of nitric acid-modified activated carbon, nitric acid-modified graphene and nitric acid-modified carbon nanotubes; the preparation process of the nitric acid-modified carbon material is as follows: after washing and drying the carbon material, putting it into a 65wt% to 68wt% nitric acid solution, reacting at 60°C to 80°C for 2h to 3h, cooling, filtering, repeatedly rinsing with water to pH = 7, and drying to obtain the nitric acid-modified carbon material.

4. The production method of high-purity silver nitrate according to claim 1, wherein In step (3), the amount of nitric acid-modified carbon material added is 2 g / L to 8 g / L.

5. The method for producing high-purity silver nitrate according to any one of claims 1 to 4, characterized in that: In step (3), the first stirring time is 0.5h to 1h, the standing time is 0.5h to 1h, the second stirring time is 0.5h to 1h, and the standing adsorption time is 0.5h to 2h.

6. The method for producing high-purity silver nitrate according to any one of claims 1 to 4, characterized in that: In step (2), the mass fraction of nitric acid in the nitric acid solution is 65% to 68%, the volume ratio of the nitric acid solution to water is 22 to 25:1, and the heating time for removing the acid is 2h to 3h.

7. The method for producing high-purity silver nitrate according to any one of claims 1 to 4, characterized in that: In step (2), after adding water, first add part of the nitric acid solution, raise the reaction temperature to 60° C. to 80° C., and then dropwise add the remaining nitric acid solution.

8. The method for producing high-purity silver nitrate according to any one of claims 1 to 4, characterized in that: In step (4), the concentration of the nitric acid solution is 3wt% to 6wt%, the vacuum degree of the vacuum evaporation concentration is -65kPa to -90kPa, and the temperature of the vacuum evaporation concentration is 110°C to 130°C.

9. The method for producing high-purity silver nitrate according to any one of claims 1 to 4, characterized in that: In step (4), the cooling crystallization is carried out under stirring, the stirring rate is 60rpm-80rpm, the cooling crystallization time is 2h-4h, the drying temperature is 85°C-90°C, and the drying time is 5h-8h.

10. The method for producing high-purity silver nitrate according to any one of claims 1 to 4, characterized in that: In step (1), the sodium hydroxide solution alkali washing is to put the silver plate into the sodium hydroxide solution for ultrasonic cleaning for 10min to 15min, take it out and drain it for 2min to 5min, and blow it dry with compressed air; the first water washing is to put the silver plate after the alkali washing into deionized water for ultrasonic cleaning for 10min to 15min, take it out and drain it for 2min to 5min, and blow it dry with compressed air; the nitric acid solution acid washing is to put the silver plate after the first water washing into the nitric acid solution for ultrasonic cleaning for 10min to 15min, take it out and drain it for 2min to 5min, and blow it dry with compressed air; the second water washing is to put the silver plate after the acid washing into deionized water for ultrasonic cleaning for 10min to 15min, take it out and drain it for 2min to 5min, and blow it dry with compressed air; the silver plate adopts the national standard No. 1 silver plate, the mass fraction of the sodium hydroxide solution is 5% to 8%, and the mass fraction of the nitric acid solution is 5% to 8%.

Citation Information

Patent Citations

  • Production method of photography-level silver nitrate

    CN102040241A

  • Production process of high-purity silver nitrate, high-purity silver nitrate and application of high-purity silver nitrate

    CN116462221A

  • Preparation method of high-purity silver nitrate

    CN116692927A

  • Process for preparing high-purity silver nitrate crystal

    CN1386707A

Cited By

  • Production method of high-purity silver nitrate

    CN120774453A

  • Purification preparation method of high-purity silver nitrate

    CN122301249A