Preparation method of modified polyamine polyfluorene block copolymer for new energy battery adhesive

Through the preparation of modified polybenamine polyfluorene block copolymer, the problem of low cycle life of conductive polymer electrode materials is solved, and the high-performance bonding strength and high-temperature resistance of new energy battery adhesives are achieved, which is suitable for large-scale Large-scale production.

CN119039571APending Publication Date: 2024-11-29SUZHOU RUITENGNING ENERGY TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411366584.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-29
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The conductive polymer electrode material has a low cycle life after multiple charges and discharges, and the ion transmission is slow, making it difficult to meet the high performance requirements of new energy battery adhesives.

Method used

The preparation method of modified polyamide polyfluorene block copolymer is adopted, and polyaniline is used to carry out polyaniline, 4-iodophenol, DCC, DMAP, Pd(PPh3)4, K2CO3 and 2-(7-bromo-9,9-dioctyl The reaction of the group-9-H-fluorene-2-)-4,4,5,5-tetramethyl-1,3,2-dioxoborane has excellent bonding strength, high temperature resistance and electrical conductivity polyamide polyfluorene block copolymer.

Benefits of technology

It improves the bonding strength and high temperature resistance of new energy battery adhesives, meets high performance requirements, and is simple and easy to operate, suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a preparation method of a modified polyamine polyfluorene block copolymer for a new energy battery adhesive. The preparation method comprises the following steps: S1, material preparation: preparing a raw material I of polyaniline, 4-iodophenol, DCC, DMAP, dichloromethane and methanol; the preparation method comprises the following steps: preparing a raw material II of toluene, Pd (PPh3) 4, K2CO3 and 2-(7-bromo-9, 9-dioctyl-9-H-fluorene-2-)-4, 4, 5, 5-tetramethyl-1, 3, 2-borane dioxide; s2, preparation of polyaniline iodobenzene: adding polyaniline, 4-iodophenol, DCC and DMAP into a 500mL four-neck flask, adding dichloromethane, dissolving, and stirring at room temperature; and S3, adding water after the reaction in the S2 is finished, stirring for 5 minutes to stop the reaction, and then filtering the reaction liquid. The polyaniline polyfluorene block copolymer modified by the method provided by the invention has excellent bonding strength, high temperature resistance and conductivity, can meet the high-performance requirements of new energy batteries on adhesives, and is simple in preparation method, easy to operate and suitable for large-scale production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of preparation of polyamine-polyfluorene block copolymers, and in particular to a method for preparing a modified polyamine-polyfluorene block copolymer for a new energy battery adhesive. Background Art

[0002] Supercapacitors have high specific capacitance, power density, energy density, excellent cycle stability, long cycle life and are green and environmentally friendly. Therefore, they are considered to be one of the most promising energy storage devices currently.

[0003] Electrode materials are the main components of supercapacitors and determine their performance. Currently, the electrode materials used for supercapacitors are mainly divided into three categories: carbon materials, metal oxides and hydrate materials, and conductive polymer materials.

[0003] Conductive polymers (polyaniline, polypyrrole, polythiophene, etc.) as supercapacitor electrode materials have the advantages of low cost, high capacity, short charge and discharge time, environmental friendliness and high safety. Their disadvantages are that after multiple charge and discharge cycles, the cycle life is not high and the ion transmission is slow.

[0004] Polyaniline in new energy battery adhesives is a kind of conductive polymer. After doping, it can have conductivity and electrochemical properties. It is an electrode material with excellent reversibility. However, compared with traditional polyaniline, modified polyaniline polyfluorene block copolymers have better adhesion, guidance and heat resistance. Therefore, we proposed a preparation method of modified polyaniline polyfluorene block copolymers for new energy battery adhesives. Summary of the invention

[0005] Based on the technical problems existing in the background technology, the present invention proposes a method for preparing a modified polyamine-polyfluorene block copolymer for new energy battery adhesive.

[0006] The present invention provides a method for preparing a modified polyamine-polyfluorene block copolymer for a new energy battery adhesive, comprising the following steps: S1: Material preparation: prepare raw material 1 of polyaniline, 4-iodophenol, DCC, DMAP, dichloromethane and methanol; Prepare raw material 2 of toluene, Pd(PPh3)4, K2CO3, and 2-(7-bromo-9,9-dioctyl-9-H-fluorene-2-)-4,4,5,5-tetramethyl-1,3,2-dioxaborane; S2: Preparation of polyaniline iodobenzene: Add polyaniline, 4-iodophenol, DCC, and DMAP into a 500 mL four-necked flask, add dichloromethane to dissolve, and stir at room temperature; S3: After the reaction of S2 is completed, water is added and stirred for 5 minutes to terminate the reaction. The reaction solution is then filtered and the filtrate is concentrated under reduced pressure to a relatively concentrated state without solid precipitation, and then reprecipitated in methanol to obtain polyaniline iodobenzene as a white solid product; S4: Preparation of polyphenylamine-polyfluorene block copolymer: Toluene, Pd(PPh3)4, and polyaniline iodobenzene were added to a 500 mL four-necked flask. After freezing and degassing for 3 times, 22% K2CO3 with nitrogen exchange for 30 min was added, and the mixture was heated and stirred. S5: The reaction in S4 is cooled to room temperature, 2-(7-bromo-9,9-dioctyl-9-H-fluorene-2-)-4,4,5,5-tetramethyl-1,3,2-dioxaborane is added to the reaction bottle, and after degassing 3 times, the temperature is raised and stirred to react; S6: After the reaction is completed, the mixture is cooled to room temperature, toluene is added thereto and mixed thoroughly, and then saturated brine is added to wash the mixture several times.

[0007] S7: The oil phase was collected, dried over MgSO4 and then filtered. The filtrate was concentrated to a relatively concentrated state without solid precipitation, and then reprecipitated in methanol to obtain a light yellow solid poly(benzamine)-poly(fluorene) block copolymer.

[0008] Preferably, the S2 room temperature is set to 15-25 degrees Celsius, and the stirring time is set to 23-25h.

[0009] Preferably, the DCC is N,N'-dicyclohexylcarbodiimide, and DCC is used to promote the reaction between polyaniline and 4-iodophenol to generate p-polyaniline iodobenzene.

[0010] Preferably, the heating temperature in S4 is set to 85° C.-95° C., and the stirring is set to 5-7 h.

[0011] Preferably, the temperature of the heating in S5 is 75° C.-85° C., and the stirring reaction time is set to 35-37 h.

[0012] Preferably, the number of washing with saturated salt water in S5 is set to 3-4 times.

[0013] Preferably, the Pd(PPh3)4, i.e., tetrakis(triphenylphosphine)palladium, is composed of a central palladium atom and four triphenylphosphine ligands; Preferably, the Pd(PPh3)4 is used as a catalyst to promote the reaction between polyaniline iodobenzene and 2-(7-bromo-9,9-dioctyl-9-H-fluorene-2-)-4,4,5,5-tetramethyl-1,3,2-dioxaborane, so that the reaction can be carried out efficiently under relatively mild conditions, thereby improving the reaction yield and product purity.

[0014] Beneficial effects of the present invention: The modified polyaniline-polyfluorene block copolymer prepared by the present invention has excellent bonding strength, high temperature resistance and electrical conductivity, and can meet the high performance requirements of new energy batteries for adhesives.

[0015] The preparation method of the invention is simple, easy to operate and suitable for large-scale production. DETAILED DESCRIPTION

[0016] The present invention will be further explained below in conjunction with specific embodiments. Example

[0017] This embodiment proposes a method for preparing a modified polyamine polyfluorene block copolymer for a new energy battery adhesive, comprising the following steps: S1: Material preparation: prepare raw material 1 of polyaniline, 4-iodophenol, DCC, DMAP, dichloromethane and methanol; Prepare raw material 2 of toluene, Pd(PPh3)4, K2CO3, and 2-(7-bromo-9,9-dioctyl-9-H-fluorene-2-)-4,4,5,5-tetramethyl-1,3,2-dioxaborane; S2: Preparation of polyaniline iodobenzene: Add polyaniline, 4-iodophenol, DCC, and DMAP into a 500 mL four-necked flask, add dichloromethane to dissolve, and stir at room temperature; S3: After the reaction of S2 is completed, water is added and stirred for 5 minutes to terminate the reaction. The reaction solution is then filtered and the filtrate is concentrated under reduced pressure to a relatively concentrated state without solid precipitation, and then reprecipitated in methanol to obtain polyaniline iodobenzene as a white solid product; S4: Preparation of polyphenylamine-polyfluorene block copolymer: Toluene, Pd(PPh3)4, and polyaniline iodobenzene were added to a 500 mL four-necked flask. After freezing and degassing for 3 times, 22% K2CO3 was added with nitrogen exchange for 30 min, and the temperature was raised and stirred. S5: The reaction in S4 is cooled to room temperature, 2-(7-bromo-9,9-dioctyl-9-H-fluorene-2-)-4,4,5,5-tetramethyl-1,3,2-dioxaborane is added to the reaction bottle, and after degassing 3 times, the temperature is raised and stirred to react; S6: After the reaction is completed, the mixture is cooled to room temperature, toluene is added thereto and mixed thoroughly, and then saturated brine is added to wash the mixture several times.

[0018] S7: The oil phase was collected, dried over MgSO4 and then filtered. The filtrate was concentrated to a relatively concentrated state without solid precipitation, and then reprecipitated in methanol to obtain a light yellow solid poly(benzamine)-poly(fluorene) block copolymer.

[0019] In this embodiment, the room temperature of S2 is set to 15 degrees Celsius, and the stirring time is set to 23h. DCC is N,N'-dicyclohexylcarbodiimide. DCC is used to promote the reaction between polyaniline and 4-iodophenol to generate polyaniline iodobenzene. The heating temperature in S4 is set to 85°C, and the stirring is set to 5h. The heating temperature in S5 is 75°C, and the stirring reaction time is set to 35h. The number of saturated brine washings in S5 is set to 3 times. Pd(PPh3)4 is tetrakis(triphenylphosphine)palladium, which is composed of a central palladium atom and four triphenylphosphine ligands. Pd(PPh3)4 acts as a catalyst to promote the reaction between polyaniline iodobenzene and 2-(7-bromo-9,9-dioctyl-9-H-fluorene-2-)-4,4,5,5-tetramethyl-1,3,2-dioxaborane, so that the reaction can be carried out efficiently under relatively mild conditions, thereby improving the reaction yield and product purity. Example

[0020] This embodiment proposes a method for preparing a modified polyamine polyfluorene block copolymer for a new energy battery adhesive, comprising the following steps: S1: Material preparation: prepare raw material 1 of polyaniline, 4-iodophenol, DCC, DMAP, dichloromethane and methanol; Prepare raw material 2 of toluene, Pd(PPh3)4, K2CO3, and 2-(7-bromo-9,9-dioctyl-9-H-fluorene-2-)-4,4,5,5-tetramethyl-1,3,2-dioxaborane; S2: Preparation of polyaniline iodobenzene: Add polyaniline, 4-iodophenol, DCC, and DMAP into a 500 mL four-necked flask, add dichloromethane to dissolve, and stir at room temperature; S3: After the reaction of S2 is completed, water is added and stirred for 5 minutes to terminate the reaction. The reaction solution is then filtered and the filtrate is concentrated under reduced pressure to a relatively concentrated state without solid precipitation, and then reprecipitated in methanol to obtain polyaniline iodobenzene as a white solid product; S4: Preparation of polyphenylamine-polyfluorene block copolymer: Toluene, Pd(PPh3)4, and polyaniline iodobenzene were added to a 500 mL four-necked flask. After freezing and degassing for 3 times, 22% K2CO3 was added with nitrogen exchange for 30 min, and the temperature was raised and stirred. S5: The reaction in S4 is cooled to room temperature, 2-(7-bromo-9,9-dioctyl-9-H-fluorene-2-)-4,4,5,5-tetramethyl-1,3,2-dioxaborane is added to the reaction bottle, and after degassing 3 times, the temperature is raised and stirred to react; S6: After the reaction is completed, the mixture is cooled to room temperature, toluene is added thereto and mixed thoroughly, and then saturated brine is added to wash the mixture several times.

[0021] S7: The oil phase was collected, dried over MgSO4 and then filtered. The filtrate was concentrated to a relatively concentrated state without solid precipitation, and then reprecipitated in methanol to obtain a light yellow solid poly(benzamine-polyfluorene) block copolymer.

[0022] In this embodiment, the room temperature of S2 is set to 20 degrees Celsius, and the stirring time is set to 24h, DCC is N,N'-dicyclohexylcarbodiimide, and DCC is used to promote the reaction between polyaniline and 4-iodophenol to generate polyaniline iodobenzene, the heating temperature in S4 is set to 90°C, and the stirring is set to 6h, the heating temperature in S5 is 80°C, and the stirring reaction time is set to 36h, the number of saturated brine washings in S5 is set to 3 times, Pd(PPh3)4 is tetrakis(triphenylphosphine)palladium, which is composed of a central palladium atom and four triphenylphosphine ligands. Pd(PPh3)4 acts as a catalyst to promote the reaction between polyaniline iodobenzene and 2-(7-bromo-9,9-dioctyl-9-H-fluorene-2-)-4,4,5,5-tetramethyl-1,3,2-dioxaborane, so that the reaction can be carried out efficiently under relatively mild conditions, thereby improving the reaction yield and product purity. Example

[0023] This embodiment proposes a method for preparing a modified polyamine polyfluorene block copolymer for a new energy battery adhesive, comprising the following steps: S1: Material preparation: prepare raw material 1 of polyaniline, 4-iodophenol, DCC, DMAP, dichloromethane and methanol; Prepare raw material 2 of toluene, Pd(PPh3)4, K2CO3, and 2-(7-bromo-9,9-dioctyl-9-H-fluorene-2-)-4,4,5,5-tetramethyl-1,3,2-dioxaborane; S2: Preparation of polyaniline iodobenzene: Add polyaniline, 4-iodophenol, DCC, and DMAP into a 500 mL four-necked flask, add dichloromethane to dissolve, and stir at room temperature; S3: After the reaction of S2 is completed, water is added and stirred for 5 minutes to terminate the reaction. The reaction solution is then filtered and the filtrate is concentrated under reduced pressure to a relatively concentrated state without solid precipitation, and then reprecipitated in methanol to obtain polyaniline iodobenzene as a white solid product; S4: Preparation of polyphenylamine-polyfluorene block copolymer: Toluene, Pd(PPh3)4, and polyaniline iodobenzene were added to a 500 mL four-necked flask. After freezing and degassing for 3 times, 22% K2CO3 was added with nitrogen exchange for 30 min, and the temperature was raised and stirred. S5: The reaction in S4 is cooled to room temperature, 2-(7-bromo-9,9-dioctyl-9-H-fluorene-2-)-4,4,5,5-tetramethyl-1,3,2-dioxaborane is added to the reaction bottle, and after degassing 3 times, the temperature is raised and stirred to react; S6: After the reaction is completed, the mixture is cooled to room temperature, toluene is added thereto and mixed thoroughly, and then saturated brine is added to wash the mixture several times.

[0024] S7: The oil phase was collected, dried over MgSO4 and then filtered. The filtrate was concentrated to a relatively concentrated state without solid precipitation, and then reprecipitated in methanol to obtain a light yellow solid poly(benzamine)-poly(fluorene) block copolymer.

[0025] In this embodiment, the room temperature of S2 is set to 25 degrees Celsius, and the stirring time is set to 25 hours. DCC is N,N'-dicyclohexylcarbodiimide. DCC is used to promote the reaction between polyaniline and 4-iodophenol to generate polyaniline iodobenzene. The heating temperature in S4 is set to 95°C, and the stirring is set to 7 hours. The heating temperature in S5 is 85°C, and the stirring reaction time is set to 37 hours. The number of saturated brine washings in S5 is set to 4 times. Pd(PPh3)4 is tetrakis(triphenylphosphine)palladium, which is composed of a central palladium atom and four triphenylphosphine ligands. Pd(PPh3)4 acts as a catalyst to promote the reaction between polyaniline iodobenzene and 2-(7-bromo-9,9-dioctyl-9-H-fluorene-2-)-4,4,5,5-tetramethyl-1,3,2-dioxaborane, so that the reaction can be carried out efficiently under relatively mild conditions, thereby improving the reaction yield and product purity. Example

[0026] This embodiment proposes a method for preparing a modified polyamine polyfluorene block copolymer for a new energy battery adhesive, comprising the following steps: The preparation method of polyaniline iodobenzene is as follows: polyaniline (12.1 g, molecular weight of about 726), 4-iodophenol (20 g), DCC (18.8 g), and DMAP (11.1 g) are added to a 500 mL four-necked flask, and dichloromethane (250 mL) is added to dissolve and stirred at room temperature for 24 hours. After the reaction is completed, 1 ml of water is added and stirred for 5 minutes to terminate the reaction. The reaction solution is filtered, and the filtrate is concentrated under reduced pressure to a relatively concentrated state without solid precipitation, and then reprecipitated in methanol (2000 mL) to obtain 17.8 white solid product (B), with a yield of about 82.3%; The preparation method of polybenzamine polyfluorene block copolymer is as follows: toluene (100mL), Pd(PPh3)4 (0.185g), and 1.3g of polyaniline iodobenzene are added to a 500mL four-necked flask. After freezing and degassing for 3 times, 22% K2CO3 (150mL) that has been nitrogen exchanged for 30 minutes is added thereto, and the temperature is raised to 90oC and stirred for 6 hours. The reaction is cooled to room temperature, and 2-(7-bromo-9,9-dioctyl-9-H-fluorene-2-)-4,4,5,5-tetramethyl-1,3,2-dioxaborane (9g) is added to the reaction bottle, and after degassing for 3 times, the temperature is raised to 80oC and stirred for 36 hours. After the reaction is completed, it is cooled to room temperature, 300mL of toluene is added thereto and mixed thoroughly, and washed three times with 300mL of saturated brine. The oil phase was collected, dried over MgSO4 and filtered. The filtrate was concentrated to a relatively concentrated state without solid precipitation, and reprecipitated in methanol to obtain 7.1 g of a light yellow solid with a yield of 69.6%.

[0027] The modified polyaniline-polyfluorene block copolymer prepared by the present invention has excellent bonding strength, high temperature resistance and electrical conductivity, can meet the high performance requirements of new energy batteries for adhesives, and the preparation method is simple, easy to operate, and suitable for large-scale production.

[0028] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A method for preparing a modified polyamine-polyfluorene block copolymer for new energy battery adhesive, characterized in that: The following steps are involved: S1: Material preparation: prepare raw material 1 of polyaniline, 4-iodophenol, DCC, DMAP, dichloromethane and methanol; Prepare raw material 2 of toluene, Pd(PPh3)4, K2CO3, and 2-(7-bromo-9,9-dioctyl-9-H-fluorene-2-)-4,4,5,5-tetramethyl-1,3,2-dioxaborane; S2: Preparation of polyaniline iodobenzene: Add polyaniline, 4-iodophenol, DCC, and DMAP into a 500 mL four-necked flask, add dichloromethane to dissolve, and stir at room temperature; S3: After the reaction of S2 is completed, water is added and stirred for 5 minutes to terminate the reaction. The reaction solution is then filtered and the filtrate is concentrated under reduced pressure to a relatively concentrated state without solid precipitation, and then reprecipitated in methanol to obtain polyaniline iodobenzene as a white solid product; S4: Preparation of polyphenylamine-polyfluorene block copolymer: Toluene, Pd(PPh3)4, and polyaniline iodobenzene were added to a 500 mL four-necked flask. After freezing and degassing for 3 times, 22% K2CO3 with nitrogen exchange for 30 min was added, and the mixture was heated and stirred. S5: The reaction in S4 is cooled to room temperature, 2-(7-bromo-9,9-dioctyl-9-H-fluorene-2-)-4,4,5,5-tetramethyl-1,3,2-dioxaborane is added to the reaction bottle, and after degassing 3 times, the temperature is raised and stirred to react; S6: After the reaction is completed and cooled to room temperature, toluene is added and mixed thoroughly, and then saturated brine is added to wash several times; S7: The oil phase was collected, dried over MgSO4 and then filtered. The filtrate was concentrated to a relatively concentrated state without solid precipitation, and then reprecipitated in methanol to obtain a light yellow solid poly(benzamine)-poly(fluorene) block copolymer.

2. The method for preparing a modified polyamine-polyfluorene block copolymer for a new energy battery adhesive according to claim 1, characterized in that: The S2 room temperature is set to 15-25 degrees Celsius, and the stirring time is set to 23-25h.

3. The method for preparing a modified polyamine-polyfluorene block copolymer for a new energy battery adhesive according to claim 1, characterized in that: The DCC is N,N'-dicyclohexylcarbodiimide, and DCC is used to promote the reaction between polyaniline and 4-iodophenol to generate p-polyaniline iodobenzene.

4. The method for preparing a modified polyamine-polyfluorene block copolymer for a new energy battery adhesive according to claim 1, characterized in that: The heating temperature in S4 is set to 85° C.-95° C., and the stirring is set to 5-7 h.

5. The method for preparing a modified polyamine-polyfluorene block copolymer for a new energy battery adhesive according to claim 1, characterized in that: The temperature of the heating in S5 is 75° C.-85° C., and the stirring reaction time is set to 35-37 h.

6. The method for preparing a modified polyamine-polyfluorene block copolymer for a new energy battery adhesive according to claim 1, characterized in that: The number of washing with saturated salt water in S5 is set to 3-4 times.

7. The method for preparing a modified polyamine-polyfluorene block copolymer for a new energy battery adhesive according to claim 1, characterized in that: The Pd(PPh3)4 is tetrakis(triphenylphosphine)palladium, which is composed of a central palladium atom and four triphenylphosphine ligands.

8. The method for preparing a modified polyamine-polyfluorene block copolymer for a new energy battery adhesive according to claim 1, characterized in that: The Pd(PPh3)4 acts as a catalyst to promote the reaction between polyaniline iodobenzene and 2-(7-bromo-9,9-dioctyl-9-H-fluorene-2-)-4,4,5,5-tetramethyl-1,3,2-dioxaborane, so that the reaction can be carried out efficiently under relatively mild conditions, thereby improving the reaction yield and product purity.