Heat-conducting double-faced adhesive tape and preparation method thereof

By preparing double-sided adhesives of modified carbon fiber and thermally conductive powder on the polyimide film, the problem of insufficient thermal conductivity of traditional double-sided adhesives is solved, high-performance thermal conductivity and electrical insulation are achieved, and initial adhesion is improved Force and peel strength.

CN119039892APending Publication Date: 2024-11-29SHENZHEN BORNSUN IND CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411114034.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Traditional double-sided adhesives have insufficient thermal conductivity in high-performance electronic devices, which leads to heat accumulation, threatens equipment safety, and has problems such as weak initial adhesion and insufficient peeling strength.

Method used

A glue and B glue are prepared with acrylic glue and silicone pressure-sensitive glue, and corona treatment is performed on polyimide (PI) film, and surface modified modified carbon fiber and thermally conductive powder are added to form a strong glue layer. and weak-sided adhesive layer, which improves thermal conductivity and adhesion through special treatment.

Benefits of technology

It realizes excellent thermal conductivity, good electrical insulation, strong initial adhesion and high peel strength of thermally conductive double-sided adhesive, meeting the needs of high-performance electronic equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004993123870000141
    Figure BDA0004993123870000141
  • Figure BDA0004993123870000151
    Figure BDA0004993123870000151
Patent Text Reader

Abstract

The invention discloses a heat-conducting double-faced adhesive tape and a preparation method thereof. The preparation method comprises the following steps: (1) uniformly stirring acrylic glue, a solvent, a tackifier, an antioxidant, a flatting agent, modified carbon fibers and heat-conducting powder, and then adding a curing agent to obtain a glue A; uniformly stirring silica gel pressure-sensitive glue, an anchoring agent, a solvent, a tackifier, a cross-linking agent, a flatting agent, modified carbon fibers and heat-conducting powder, and then adding a curing agent to obtain glue B; (2) carrying out corona treatment on the PI film; (3) coating the adhesive A on one surface of the PI film, and drying and curing to form a strong surface adhesive layer; (4) pasting a release film on the surface of the strong surface adhesive layer, and then rolling and curing; (5) coating the glue B on the other surface of the PI film, and drying and curing to form a weak surface glue layer; and (6) pasting a second release film on the surface of the weak-surface adhesive layer, and rolling to obtain the heat-conducting double-sided adhesive tape. The preparation method can be used for preparing the heat-conducting double-sided adhesive tape with better heat conduction capability, electrical insulation property, initial adhesive force and peel strength.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of double-sided adhesive tapes, and in particular relates to a heat-conductive double-sided adhesive tape and a preparation method thereof. Background Art

[0002] With the rapid development of technology and the rising expectations of consumers, the design of electronic devices is moving towards the cutting-edge trend of integrated rich functions, light weight, slim design and environmentally friendly intelligence. However, this series of evolutions has also spawned a series of new challenges, the most prominent of which is the strict requirements for thermal management and safety standards of electronic devices. In this context, traditional pressure-sensitive adhesives are widely popular because of their advantages of easy application, easy removal after pasting and no residue left.

[0003] As a common form of pressure-sensitive adhesive, traditional double-sided tape consists of two layers of adhesive and a layer of substrate sandwiched in between. This design enables it to effectively connect two different surfaces. Although traditional double-sided tape performs well in bonding performance, its insufficient thermal conductivity has become a major shortcoming. In highly integrated electronic components, heat generation increases significantly, and traditional double-sided tape cannot effectively guide and disperse this heat, which not only aggravates the heat accumulation inside the device, but also directly threatens the safety and service life of the device, and even causes serious consequences such as equipment failure, fire or explosion in extreme cases. In addition, existing double-sided tape products have some other problems, such as weak initial adhesion and insufficient strength when peeling. These problems further highlight the overall performance disadvantages of traditional double-sided tape in meeting the needs of high-performance electronic equipment.

[0004] Therefore, there is an urgent need for a thermally conductive double-sided adhesive and a preparation method thereof to solve the deficiencies of the prior art. Summary of the invention

[0005] In view of the above problems, the purpose of the present invention is to provide a thermally conductive double-sided adhesive and a preparation method thereof. The preparation method can be used to prepare a thermally conductive double-sided adhesive with excellent comprehensive performance to meet the needs of the industry. The thermally conductive double-sided adhesive not only exhibits excellent thermal conductivity, but also has good electrical insulation, strong initial adhesion and high peel strength.

[0006] To achieve the above objectives, the present invention provides a method for preparing a thermally conductive double-sided adhesive in a first aspect, the steps comprising:

[0007] (1) mixing acrylic glue, a first solvent, a first tackifier, an antioxidant, a first leveling agent, a first modified carbon fiber, and a first thermal conductive powder, stirring evenly, then adding a first curing agent, and stirring evenly to obtain glue A;

[0008] The silicone pressure-sensitive adhesive, the anchoring agent, the second solvent, the second tackifier, the cross-linking agent, the second leveling agent, the second modified carbon fiber, and the second thermal conductive powder are mixed, stirred evenly, and then the second curing agent is added, and stirred evenly to obtain glue B;

[0009] (2) corona treatment of the PI film;

[0010] (3) applying glue A on one surface of the PI film and drying and curing it to form a strong surface glue layer;

[0011] (4) applying the first release film to the surface of the strong adhesive layer, and then rolling and curing the film;

[0012] (5) Applying glue B to the other surface of the PI film and drying and curing it to form a weak surface glue layer;

[0013] (6) applying a second release film to the surface of the weak adhesive layer, and then rolling it up to obtain a thermally conductive double-sided adhesive;

[0014] The preparation of the first modified carbon fiber and the second modified carbon fiber includes: placing the carbon fiber in an aqueous solution containing a coupling agent and ethanol for pretreatment.

[0015] Compared with the prior art, the present invention first prepares A glue and B glue, then corona treatment is carried out on PI film, and then A glue and B glue are respectively coated on both sides of PI film and formed into heat-conducting double-sided adhesive through drying and curing. Wherein A glue and B glue both contain specially treated carbon fiber, specifically, by using coupling agent to carry out surface modification to carbon fiber, and the surface of carbon fiber is activated, which improves the compatibility and bonding force of carbon fiber and glue matrix, and strengthens the heat conduction path, so the first modified carbon fiber and the second modified carbon fiber can be added to A glue and B glue respectively to enhance its thermal conductivity without significantly reducing viscosity. At the same time, A glue and B glue also all include tackifier and leveling agent, the introduction of tackifier can effectively solve the problem of adhesive viscosity reduction caused by adding heat-conducting powder, and leveling agent helps glue to be evenly distributed to prevent the occurrence of local adhesion being too strong or too weak, so tackifier and leveling agent jointly ensure that double-sided adhesive has strong initial adhesion and high peel strength. In addition, the polyimide (PI) film has excellent electrical insulation properties and thermal stability, which ensures that even after the conductive carbon fiber is added, the electrical breakdown strength of the double-sided adhesive will not be greatly attenuated, thereby ensuring thermal conductivity while maintaining good electrical insulation performance. Therefore, the preparation method of the present invention can be used to prepare a thermally conductive double-sided adhesive with excellent thermal conductivity, good electrical insulation, strong initial adhesion and high peel strength to meet the needs of the industry.

[0016] Furthermore, in parts by mass, the raw materials for preparing glue A of the present invention include 50 to 100 parts of acrylic glue, 50 to 200 parts of a first solvent, 1 to 3 parts of a first tackifier, 0.1 to 0.8 parts of an antioxidant, 0.1 to 0.8 parts of a leveling agent, 600 to 800 parts of a first modified carbon fiber, 100 to 200 parts of a first thermally conductive powder, and 0.1 to 1.2 parts of a first curing agent; the raw materials for preparing glue B include 50 to 100 parts of silicone pressure-sensitive glue, 0.1 to 2 parts of an anchoring agent, 50 to 200 parts of a second solvent, 1 to 3 parts of a second tackifier, 0.1 to 1 parts of a cross-linking agent, 0.1 to 2 parts of a second leveling agent, 700 to 900 parts of a second modified carbon fiber, 100 to 200 parts of a second thermally conductive powder, and 0.1 to 1 parts of a second curing agent.

[0017] Furthermore, in step (1) of the present invention, the stirring speed is 30 to 100 rpm / min, and the stirring time is 30 to 100 min.

[0018] Furthermore, the inventors of the present invention discovered during the research and creation process that the content of each component in glue A and glue B will directly affect the final residual glue amount, initial adhesion and peel strength of the thermally conductive double-sided adhesive; specifically, the first curing agent of the present invention is preferably 0.5 parts; the cross-linking agent is preferably 0.3 parts; the first tackifier is preferably 2.1 parts; and the second tackifier is preferably 2.4 parts.

[0019] Furthermore, the first curing agent of the present invention is epoxy resin; and the cross-linking agent is at least one of hydrogen-containing silicone oil, benzoyl peroxide and di(2,4-dichlorobenzoyl) peroxide.

[0020] Furthermore, the first release film of the present invention is a silicone release film; and the second release film is a fluorine release film.

[0021] Furthermore, the first solvent of the present invention is ethyl acetate, and the second solvent is toluene.

[0022] Further, the thickness of the PI film of the present invention is 25 to 100 μm; the thickness of the strong surface adhesive layer and the weak surface adhesive layer are each independently 50 to 200 μm. Specifically, the thickness of the PI film may be, but is not limited to, 25 μm, 40 μm, 60 μm, 70 μm, 80 μm, 90 μm, and 100 μm. The thickness of the strong surface adhesive layer may be, but is not limited to, 50 μm, 70 μm, 90 μm, 120 μm, 150 μm, 180 μm, and 200 μm; the thickness of the weak surface adhesive layer may be, but is not limited to, 50 μm, 70 μm, 90 μm, 120 μm, 150 μm, 180 μm, and 200 μm. Preferably, the thickness of the PI film is 50 μm; the thickness of the strong surface adhesive layer is 125 μm; and the thickness of the weak surface adhesive layer is 125 μm.

[0023] Furthermore, the first thermally conductive powder and the second thermally conductive powder of the present invention are independently selected from at least one of aluminum hydroxide, boron nitride, aluminum nitride, zinc oxide, and aluminum oxide.

[0024] Furthermore, the acrylic glue of the present invention has a solid content of 43-47% and a viscosity of 1500-3500 cps; the silicone pressure-sensitive glue has a solid content of 58-62% and a viscosity of 18000-22000 cps.

[0025] Furthermore, the coupling agent of the present invention includes at least one of γ-aminopropyltriethoxysilane (KH550), γ-glycidyloxypropyltrimethoxysilane (KH560), γ-methacryloxypropyltrimethoxysilane (KH570), dodecyltrimethoxysilane, vinyltriethoxysilane, titanate coupling agent, and aluminate coupling agent.

[0026] Further, the preparation of the first modified carbon fiber and the second modified carbon fiber of the present invention includes: mixing the coupling agent, ethanol, and water in a weight ratio of 3 to 5:3 to 5:1 to 3, and hydrolyzing for 1.5 to 2.5 hours to obtain a modified liquid; mixing the modified liquid and the carbon fiber in a weight ratio of 7 to 9:1 to 3, stirring evenly, and then ultrasonically treating and drying to obtain the modified carbon fiber. Specifically, the frequency of the ultrasonic treatment can be 1800 to 2200 Hz, the ultrasonic treatment time can be 8 to 15 minutes, and the drying temperature is 120°C.

[0027] Furthermore, the antioxidant of the present invention is at least one of a phenolic antioxidant, a phosphite antioxidant, and an organic sulfide antioxidant.

[0028] Furthermore, the first leveling agent of the present invention is at least one of an acrylic leveling agent and a fluorine leveling agent; the second leveling agent is at least one of polydimethylsiloxane, polyether polyester modified organic siloxane, alkyl modified organic silicone, and oxane terminal modified organic silicone.

[0029] Furthermore, the corona power of the corona treatment of the present invention is 2.8-3.2 KV; corona treatment of the PI film can increase its surface energy, making it easier to bond with A glue and B glue.

[0030] Furthermore, the drying and curing temperatures in step (3) and step (5) of the present invention are independently 120-130° C.; the aging temperature in step (4) is 65-75° C., and the aging time is 22-26 hours.

[0031] Correspondingly, the second aspect of the present invention further provides a thermally conductive double-sided adhesive tape, which is prepared by the above-mentioned method for preparing the thermally conductive double-sided adhesive tape.

[0032] Compared with the prior art, the thermally conductive double-sided adhesive of the present invention is formed by coating A adhesive and B adhesive on both sides of the PI film respectively and then drying and curing. The strong adhesive layer and the weak adhesive layer of the thermally conductive double-sided adhesive both have excellent thermal conductivity, good electrical insulation, strong initial adhesion and high peel strength. Therefore, the strong adhesive layer of the thermally conductive double-sided adhesive can be used to bond hard surfaces such as metal or plastic, while the weak adhesive layer is used to bond softer or more sensitive materials, such as electronic components. DETAILED DESCRIPTION

[0033] In order to better illustrate the purpose, technical scheme and beneficial effects of the present invention, the present invention will be further described below in conjunction with specific embodiments. It should be noted that the following implementation method is a further explanation of the present invention and should not be used as a limitation of the present invention.

[0034] The sources of the raw materials are as follows:

[0035] Acrylic glue was purchased from Bang Curing Science PSA-1367 series acrylic pressure-sensitive adhesive;

[0036] The first tackifier and the second tackifier were purchased from SIC 6208 of Siluo Ke Chemical Company;

[0037] Antioxidants were purchased from Angel Synthetic Chemical Co., Ltd. B900 antioxidant;

[0038] The first leveling agent was purchased from Mo Neng Chemical Co., Ltd. UV1201;

[0039] Carbon fiber was purchased from Zhongli New Material Technology Co., Ltd. T700 carbon fiber powder;

[0040] Aluminum nitride was purchased from Jinyi New Materials Technology Co., Ltd. AN2;

[0041] Alumina was purchased from GD-S307A thermal conductor from Jinge New Materials Co., Ltd.;

[0042] The first curing agent was purchased from Bang Curing Science HD2055;

[0043] Silicone pressure-sensitive adhesive was purchased from Dinglisen New Materials Co., Ltd. DS-9860B;

[0044] The anchoring agent was purchased from Dinglisen New Materials Co., Ltd. DS-300;

[0045] The cross-linking agent was purchased from Dinglisen New Materials Co., Ltd. DS-008W;

[0046] The second curing agent was purchased from Dinglisen New Materials Co., Ltd. DS-1500 platinum curing agent;

[0047] The second leveling agent was purchased from Mo Neng Chemical Co., Ltd. 1030;

[0048] The preparation methods of the first modified carbon fiber and the second modified carbon fiber used in the embodiment and the comparative example are exactly the same. The preparation of the first modified carbon fiber includes:

[0049] (1) A coupling agent, ethanol and water were mixed in a weight ratio of 4:4:2, and then hydrolyzed for 2 hours to obtain a modified liquid; (2) The modified liquid and carbon fiber were mixed in a weight ratio of 8:2 and stirred at 1000 rpm / min for 30 minutes, and then ultrasonically treated at 2000 Hz for 10 minutes, and then dried at 120°C to obtain a first modified carbon fiber.

[0050] Example 1

[0051] This embodiment provides a method for preparing a thermally conductive double-sided adhesive, the steps comprising:

[0052] (1) 100 g of acrylic glue, 50 g of ethyl acetate, 2.1 g of a first tackifier, 0.8 g of an antioxidant, 0.2 g of a first leveling agent, 700 g of a first modified carbon fiber, and 100 g of aluminum nitride were mixed in a stirrer, stirred at 50 rpm / min for 60 min, then 0.5 g of a first curing agent was added, and stirred at 50 rpm / min for 30 min to obtain glue A;

[0053] 100 g of silicone pressure-sensitive adhesive, 0.2 g of anchoring agent, 50 g of toluene, 2.4 g of second tackifier, 0.3 g of cross-linking agent, 0.2 g of second leveling agent, 800 g of second modified carbon fiber, and 100 g of aluminum nitride were mixed, stirred at 50 rpm / min for 60 min, 0.1 g of second curing agent was added, and stirred at 50 rpm / min for 30 min to obtain glue B;

[0054] (2) A PI film with a thickness of 50 μm was subjected to corona treatment with a corona power of 3 KV;

[0055] (3) using a coating machine to apply glue A to one surface of the PI film, and then curing it at 120° C. to form a strong surface glue layer with a thickness of 125 μm;

[0056] (4) applying a silicone release film to the surface of the strong adhesive layer, then rolling it up and aging it at 70° C. for 24 h;

[0057] (5) coating the B adhesive on the other surface of the PI film, and then drying and curing at 130°C to form a weak adhesive layer with a thickness of 125 μm;

[0058] (6) A fluorine release film is pasted on the surface of the weak adhesive layer, and then rolled up to obtain a thermally conductive double-sided adhesive.

[0059] Example 2

[0060] This embodiment provides a method for preparing a thermally conductive double-sided adhesive, the steps comprising:

[0061] (1) 100 g of acrylic glue, 50 g of ethyl acetate, 2.1 g of a first tackifier, 0.8 g of an antioxidant, 0.2 g of a first leveling agent, 600 g of a first modified carbon fiber, and 100 g of aluminum nitride were mixed in a stirrer, stirred at 50 rpm / min for 60 min, 0.5 g of a first curing agent was added, and stirred at 50 rpm / min for 30 min to obtain glue A;

[0062] 100 g of silicone pressure-sensitive adhesive, 0.2 g of anchoring agent, 50 g of toluene, 2.4 g of second tackifier, 0.3 g of cross-linking agent, 0.2 g of second leveling agent, 700 g of second modified carbon fiber, and 100 g of aluminum nitride were mixed, stirred at 50 rpm / min for 60 min, 0.1 g of second curing agent was added, and stirred at 50 rpm / min for 30 min to obtain glue B;

[0063] (2) A PI film with a thickness of 50 μm was subjected to corona treatment with a corona power of 3 KV;

[0064] (3) using a coating machine to apply glue A to one surface of the PI film, and then curing it at 120° C. to form a strong surface glue layer with a thickness of 125 μm;

[0065] (4) applying a silicone release film to the surface of the strong adhesive layer, then rolling it up and aging it at 70° C. for 24 h;

[0066] (5) coating the B adhesive on the other surface of the PI film, and then drying and curing at 130°C to form a weak adhesive layer with a thickness of 125 μm;

[0067] (6) A fluorine release film is pasted on the surface of the weak adhesive layer, and then rolled up to obtain a thermally conductive double-sided adhesive.

[0068] Example 3

[0069] This embodiment provides a method for preparing a thermally conductive double-sided adhesive, the steps comprising:

[0070] (1) 100 g of acrylic glue, 50 g of ethyl acetate, 2.1 g of a first tackifier, 0.8 g of an antioxidant, 0.2 g of a first leveling agent, 800 g of a first modified carbon fiber, and 100 g of aluminum nitride were mixed in a stirrer, stirred at 50 rpm / min for 60 min, then 0.5 g of a first curing agent was added, and stirred at 50 rpm / min for 30 min to obtain glue A;

[0071] 100 g of silicone pressure-sensitive adhesive, 0.2 g of anchoring agent, 50 g of toluene, 2.4 g of second tackifier, 0.3 g of cross-linking agent, 0.2 g of second leveling agent, 900 g of second modified carbon fiber, and 100 g of aluminum nitride were mixed, stirred at 50 rpm / min for 60 min, 0.1 g of second curing agent was added, and stirred at 50 rpm / min for 30 min to obtain glue B;

[0072] (2) A PI film with a thickness of 50 μm was subjected to corona treatment with a corona power of 3 KV;

[0073] (3) using a coating machine to apply glue A to one surface of the PI film, and then curing it at 120° C. to form a strong surface glue layer with a thickness of 125 μm;

[0074] (4) applying a silicone release film to the surface of the strong adhesive layer, then rolling it up and aging it at 70° C. for 24 h;

[0075] (5) coating the B adhesive on the other surface of the PI film, and then drying and curing at 130°C to form a weak adhesive layer with a thickness of 125 μm;

[0076] (6) A fluorine release film is pasted on the surface of the weak adhesive layer, and then rolled up to obtain a thermally conductive double-sided adhesive.

[0077] Example 4

[0078] This embodiment provides a method for preparing a thermally conductive double-sided adhesive, the steps comprising:

[0079] (1) 100 g of acrylic glue, 50 g of ethyl acetate, 2.1 g of a first tackifier, 0.8 g of an antioxidant, 0.2 g of a first leveling agent, 700 g of a first modified carbon fiber, and 100 g of aluminum nitride were mixed in a stirrer, stirred at 50 rpm / min for 60 min, 0.4 g of a first curing agent was added, and stirred at 50 rpm / min for 30 min to obtain glue A;

[0080] 100 g of silicone pressure-sensitive adhesive, 0.2 g of anchoring agent, 50 g of toluene, 2.4 g of second tackifier, 0.2 g of cross-linking agent, 0.2 g of second leveling agent, 800 g of second modified carbon fiber, and 100 g of aluminum nitride were mixed, stirred at 50 rpm / min for 60 min, 0.1 g of second curing agent was added, and stirred at 50 rpm / min for 30 min to obtain glue B;

[0081] (2) A PI film with a thickness of 50 μm was subjected to corona treatment with a corona power of 3 KV;

[0082] (3) using a coating machine to apply glue A to one surface of the PI film, and then curing it at 120° C. to form a strong surface glue layer with a thickness of 125 μm;

[0083] (4) applying a silicone release film to the surface of the strong adhesive layer, then rolling it up and aging it at 70° C. for 24 h;

[0084] (5) coating the B adhesive on the other surface of the PI film, and then drying and curing at 130°C to form a weak adhesive layer with a thickness of 125 μm;

[0085] (6) A fluorine release film is pasted on the surface of the weak adhesive layer, and then rolled up to obtain a thermally conductive double-sided adhesive.

[0086] Example 5

[0087] This embodiment provides a method for preparing a thermally conductive double-sided adhesive, the steps comprising:

[0088] (1) 100 g of acrylic glue, 50 g of ethyl acetate, 2.1 g of a first tackifier, 0.8 g of an antioxidant, 0.2 g of a first leveling agent, 700 g of a first modified carbon fiber, and 100 g of aluminum nitride were mixed in a stirrer, stirred at 50 rpm / min for 60 min, then 0.6 g of a first curing agent was added, and stirred at 50 rpm / min for 30 min to obtain glue A;

[0089] 100 g of silicone pressure-sensitive adhesive, 0.2 g of anchoring agent, 50 g of toluene, 2.4 g of second tackifier, 0.4 g of cross-linking agent, 0.2 g of second leveling agent, 800 g of second modified carbon fiber, and 100 g of aluminum nitride were mixed, stirred at 50 rpm / min for 60 min, 0.1 g of second curing agent was added, and stirred at 50 rpm / min for 30 min to obtain glue B;

[0090] (2) A PI film with a thickness of 50 μm was subjected to corona treatment with a corona power of 3 KV;

[0091] (3) using a coating machine to apply glue A to one surface of the PI film, and then curing it at 120° C. to form a strong surface glue layer with a thickness of 125 μm;

[0092] (4) applying a silicone release film to the surface of the strong adhesive layer, then rolling it up and aging it at 70° C. for 24 h;

[0093] (5) coating the B adhesive on the other surface of the PI film, and then drying and curing at 130°C to form a weak adhesive layer with a thickness of 125 μm;

[0094] (6) A fluorine release film is pasted on the surface of the weak adhesive layer, and then rolled up to obtain a thermally conductive double-sided adhesive.

[0095] Example 6

[0096] This embodiment provides a method for preparing a thermally conductive double-sided adhesive, the steps comprising:

[0097] (1) 100 g of acrylic glue, 50 g of ethyl acetate, 1.4 g of a first tackifier, 0.8 g of an antioxidant, 0.2 g of a first leveling agent, 700 g of a first modified carbon fiber, and 100 g of aluminum nitride were mixed in a stirrer, stirred at 50 rpm / min for 60 min, then 0.5 g of a first curing agent was added, and stirred at 50 rpm / min for 30 min to obtain glue A;

[0098] 100 g of silicone pressure-sensitive adhesive, 0.2 g of anchoring agent, 50 g of toluene, 1.6 g of second tackifier, 0.3 g of cross-linking agent, 0.2 g of second leveling agent, 800 g of second modified carbon fiber, and 100 g of aluminum nitride were mixed, stirred at 50 rpm / min for 60 min, 0.1 g of second curing agent was added, and stirred at 50 rpm / min for 30 min to obtain glue B;

[0099] (2) A PI film with a thickness of 50 μm was subjected to corona treatment with a corona power of 3 KV;

[0100] (3) using a coating machine to apply glue A to one surface of the PI film, and then curing it at 120° C. to form a strong surface glue layer with a thickness of 125 μm;

[0101] (4) applying a silicone release film to the surface of the strong adhesive layer, then rolling it up and aging it at 70° C. for 24 h;

[0102] (5) coating the B adhesive on the other surface of the PI film, and then drying and curing at 130°C to form a weak adhesive layer with a thickness of 125 μm;

[0103] (6) A fluorine release film is pasted on the surface of the weak adhesive layer, and then rolled up to obtain a thermally conductive double-sided adhesive.

[0104] Example 7

[0105] This embodiment provides a method for preparing a thermally conductive double-sided adhesive, the steps comprising:

[0106] (1) 100 g of acrylic glue, 50 g of ethyl acetate, 2.8 g of a first tackifier, 0.8 g of an antioxidant, 0.2 g of a first leveling agent, 700 g of a first modified carbon fiber, and 100 g of aluminum nitride were mixed in a stirrer, stirred at 50 rpm / min for 60 min, 0.5 g of a first curing agent was added, and stirred at 50 rpm / min for 30 min to obtain glue A;

[0107] 100 g of silicone pressure-sensitive adhesive, 0.2 g of anchoring agent, 50 g of toluene, 3.2 g of second tackifier, 0.3 g of cross-linking agent, 0.2 g of second leveling agent, 800 g of second modified carbon fiber, and 100 g of aluminum nitride were mixed, stirred at 50 rpm / min for 60 min, 0.1 g of second curing agent was added, and stirred at 50 rpm / min for 30 min to obtain glue B;

[0108] (2) A PI film with a thickness of 50 μm was subjected to corona treatment with a corona power of 3 KV;

[0109] (3) using a coating machine to apply glue A to one surface of the PI film, and then curing it at 120° C. to form a strong surface glue layer with a thickness of 125 μm;

[0110] (4) applying a silicone release film to the surface of the strong adhesive layer, then rolling it up and aging it at 70° C. for 24 h;

[0111] (5) coating the B adhesive on the other surface of the PI film, and then drying and curing at 130°C to form a weak adhesive layer with a thickness of 125 μm;

[0112] (6) A fluorine release film is pasted on the surface of the weak adhesive layer, and then rolled up to obtain a thermally conductive double-sided adhesive.

[0113] Example 8

[0114] This embodiment provides a method for preparing a thermally conductive double-sided adhesive, the steps comprising:

[0115] (1) 60 g of acrylic glue, 60 g of ethyl acetate, 2.1 g of a first tackifier, 0.4 g of an antioxidant, 0.5 g of a first leveling agent, 700 g of a first modified carbon fiber, and 120 g of aluminum nitride were mixed in a stirrer, stirred at 70 rpm / min for 80 min, then 0.5 g of a first curing agent was added, and stirred at 80 rpm / min for 36 min to obtain glue A;

[0116] 70 g of silicone pressure-sensitive adhesive, 0.4 g of anchoring agent, 70 g of toluene, 2.4 g of second tackifier, 0.3 g of cross-linking agent, 0.4 g of second leveling agent, 800 g of second modified carbon fiber, and 110 g of aluminum nitride were mixed, stirred at 60 rpm / min for 70 min, 0.2 g of second curing agent was added, and stirred at 90 rpm / min for 40 min to obtain glue B;

[0117] (2) A PI film with a thickness of 60 μm was subjected to corona treatment with a corona power of 3.2 KV;

[0118] (3) using a coating machine to apply glue A to one surface of the PI film, and then curing it at 125° C. to form a strong surface glue layer with a thickness of 120 μm;

[0119] (4) applying a silicone release film to the surface of the strong adhesive layer, then rolling it up and aging it at 70° C. for 24 h;

[0120] (5) coating the B adhesive on the other surface of the PI film, and then drying and curing at 132°C to form a weak adhesive layer with a thickness of 120 μm;

[0121] (6) A fluorine release film is pasted on the surface of the weak adhesive layer, and then rolled up to obtain a thermally conductive double-sided adhesive.

[0122] Comparative Example 1

[0123] This comparative example provides a method for preparing a thermally conductive double-sided adhesive, the steps comprising:

[0124] (1) 100 g of acrylic glue, 50 g of ethyl acetate, 0.8 g of antioxidant, 0.2 g of first leveling agent, 700 g of first modified carbon fiber, and 100 g of aluminum nitride were mixed in a stirrer, stirred at 50 rpm / min for 60 min, then 0.5 g of first curing agent was added, and stirred at 50 rpm / min for 30 min to obtain glue A;

[0125] 100 g of silicone pressure-sensitive adhesive, 0.2 g of anchoring agent, 50 g of toluene, 0.3 g of cross-linking agent, 0.2 g of second leveling agent, 800 g of second modified carbon fiber, and 100 g of aluminum nitride were mixed, stirred at 50 rpm / min for 60 min, 0.1 g of second curing agent was added, and stirred at 50 rpm / min for 30 min to obtain glue B;

[0126] (2) A PI film with a thickness of 50 μm was subjected to corona treatment with a corona power of 3 KV;

[0127] (3) using a coating machine to apply glue A to one surface of the PI film, and then curing it at 120° C. to form a strong surface glue layer with a thickness of 125 μm;

[0128] (4) applying a silicone release film to the surface of the strong adhesive layer, then rolling it up and aging it at 70° C. for 24 h;

[0129] (5) coating the B adhesive on the other surface of the PI film, and then drying and curing at 130°C to form a weak adhesive layer with a thickness of 125 μm;

[0130] (6) A fluorine release film is pasted on the surface of the weak adhesive layer, and then rolled up to obtain a thermally conductive double-sided adhesive.

[0131] Comparative Example 2

[0132] This comparative example provides a method for preparing a thermally conductive double-sided adhesive, the steps comprising:

[0133] (1) 100 g of acrylic glue, 50 g of ethyl acetate, 2.1 g of a first tackifier, 0.8 g of an antioxidant, 700 g of a first modified carbon fiber, and 100 g of aluminum nitride were mixed in a stirrer, stirred at 50 rpm / min for 60 min, then 0.5 g of a first curing agent was added, and stirred at 50 rpm / min for 30 min to obtain glue A;

[0134] 100 g of silicone pressure-sensitive adhesive, 0.2 g of anchoring agent, 50 g of toluene, 2.4 g of second tackifier, 0.3 g of cross-linking agent, 800 g of second modified carbon fiber, and 100 g of aluminum nitride were mixed, stirred at 50 rpm / min for 60 min, 0.1 g of second curing agent was added, and stirred at 50 rpm / min for 30 min to obtain glue B;

[0135] (2) A PI film with a thickness of 50 μm was subjected to corona treatment with a corona power of 3 KV;

[0136] (3) using a coating machine to apply glue A to one surface of the PI film, and then curing it at 120° C. to form a strong surface glue layer with a thickness of 125 μm;

[0137] (4) applying a silicone release film to the surface of the strong adhesive layer, then rolling it up and aging it at 70° C. for 24 h;

[0138] (5) coating the B adhesive on the other surface of the PI film, and then drying and curing at 130°C to form a weak adhesive layer with a thickness of 125 μm;

[0139] (6) A fluorine release film is pasted on the surface of the weak adhesive layer, and then rolled up to obtain a thermally conductive double-sided adhesive.

[0140] Comparative Example 3

[0141] This comparative example provides a method for preparing a thermally conductive double-sided adhesive, the steps comprising:

[0142] (1) 100 g of acrylic glue, 50 g of ethyl acetate, 2.1 g of a first tackifier, 0.8 g of an antioxidant, 0.2 g of a first leveling agent, 700 g of a first modified carbon fiber, and 100 g of aluminum nitride were mixed in a stirrer, stirred at 50 rpm / min for 60 min, then 0.5 g of a first curing agent was added, and stirred at 50 rpm / min for 30 min to obtain glue A;

[0143] 100 g of silicone pressure-sensitive adhesive, 0.2 g of anchoring agent, 50 g of toluene, 2.4 g of second tackifier, 0.3 g of cross-linking agent, 0.2 g of second leveling agent, 800 g of second modified carbon fiber, and 100 g of aluminum nitride were mixed, stirred at 50 rpm / min for 60 min, 0.1 g of second curing agent was added, and stirred at 50 rpm / min for 30 min to obtain glue B;

[0144] (2) using a coating machine to coat glue A on a silicone oil release film with a thickness of 75 μm, and then curing it at 120° C. to form a strong surface glue layer with a thickness of 125 μm;

[0145] (3) A 50 μm thick silicone release film is applied to the surface of the strong adhesive layer, and the 50 μm thick silicone release film is removed after rolling up, and the film is aged at 70° C. for 24 h;

[0146] (4) using a coating machine to coat the B glue on a fluorine release film with a thickness of 75 μm, and then curing it at 120° C. to form a weak surface glue layer with a thickness of 125 μm;

[0147] (5) A 50 μm thick fluorine release film is applied to the surface of the weak adhesive layer, and the 50 μm thick silicone release film is removed after rolling up;

[0148] (6) The strong surface adhesive layer obtained after step (3) and the weak surface adhesive layer obtained after step (5) are bonded together to obtain a substrate-free thermally conductive double-sided adhesive.

[0149] Comparative Example 4

[0150] This comparative example provides a method for preparing a thermally conductive double-sided adhesive, the steps comprising:

[0151] (1) 100 g of acrylic glue, 50 g of ethyl acetate, 2.1 g of a first tackifier, 0.2 g of a first leveling agent, 700 g of aluminum oxide, and 100 g of aluminum nitride were mixed in a stirrer, stirred at 50 rpm / min for 60 min, then 0.5 g of a first curing agent was added, and stirred at 50 rpm / min for 30 min to obtain glue A;

[0152] 100 g of silicone pressure-sensitive adhesive, 50 g of toluene, 2.4 g of the second tackifier, 0.3 g of a cross-linking agent, 0.2 g of a second leveling agent, 800 g of alumina, and 100 g of aluminum nitride were mixed, stirred at 50 rpm / min for 60 min, 0.1 g of a second curing agent was added, and stirred at 50 rpm / min for 30 min to obtain glue B;

[0153] (2) A PI film with a thickness of 50 μm was subjected to corona treatment with a corona power of 3 KV;

[0154] (3) using a coating machine to apply glue A to one surface of the PI film, and then curing it at 120° C. to form a strong surface glue layer with a thickness of 125 μm;

[0155] (4) applying a silicone release film to the surface of the strong adhesive layer, then rolling it up and aging it at 70° C. for 24 h;

[0156] (5) coating the B adhesive on the other surface of the PI film, and then drying and curing at 130°C to form a weak adhesive layer with a thickness of 125 μm;

[0157] (6) A fluorine release film is pasted on the surface of the weak adhesive layer, and then rolled up to obtain a thermally conductive double-sided adhesive.

[0158] Comparative Example 5

[0159] This comparative example provides a method for preparing a thermally conductive double-sided adhesive, the steps comprising:

[0160] (1) 100 g of acrylic glue, 50 g of ethyl acetate, 2.1 g of a first tackifier, 0.8 g of an antioxidant, and 0.2 g of a first leveling agent were mixed in a stirrer, stirred at 50 rpm / min for 60 min, and then 0.5 g of a first curing agent was added, and stirred at 50 rpm / min for 30 min to obtain glue A;

[0161] 100 g of silicone pressure-sensitive adhesive, 0.2 g of anchoring agent, 50 g of toluene, 2.4 g of second tackifier, 0.3 g of cross-linking agent, and 0.2 g of second leveling agent were mixed, stirred at 50 rpm / min for 60 min, 0.1 g of second curing agent was added, and stirred at 50 rpm / min for 30 min to obtain glue B;

[0162] (2) A PI film with a thickness of 50 μm was subjected to corona treatment with a corona power of 3 KV;

[0163] (3) using a coating machine to apply glue A to one surface of the PI film, and then curing it at 120° C. to form a strong surface glue layer with a thickness of 125 μm;

[0164] (4) applying a silicone release film to the surface of the strong adhesive layer, then rolling it up and aging it at 70° C. for 24 h;

[0165] (5) coating the B adhesive on the other surface of the PI film, and then drying and curing at 130°C to form a weak adhesive layer with a thickness of 125 μm;

[0166] (6) A fluorine release film is pasted on the surface of the weak adhesive layer, and then rolled up to obtain a thermally conductive double-sided adhesive.

[0167] Comparative Example 6

[0168] This comparative example provides a method for preparing a thermally conductive double-sided adhesive, the steps comprising:

[0169] (1) 100 g of acrylic glue, 50 g of ethyl acetate, 2.1 g of a first tackifier, 0.8 g of an antioxidant, 0.2 g of a first leveling agent, 700 g of carbon fiber, and 100 g of aluminum nitride were mixed in a stirrer, stirred at 50 rpm / min for 60 min, then 0.5 g of a first curing agent was added, and stirred at 50 rpm / min for 30 min to obtain glue A;

[0170] 100 g of silicone pressure-sensitive adhesive, 0.2 g of anchoring agent, 50 g of toluene, 2.4 g of second tackifier, 0.3 g of cross-linking agent, 0.2 g of second leveling agent, 800 g of carbon fiber, and 100 g of aluminum nitride were mixed, stirred at 50 rpm / min for 60 min, 0.1 g of second curing agent was added, and stirred at 50 rpm / min for 30 min to obtain glue B;

[0171] (2) A PI film with a thickness of 50 μm was subjected to corona treatment with a corona power of 3 KV;

[0172] (3) using a coating machine to apply glue A to one surface of the PI film, and then curing it at 120° C. to form a strong surface glue layer with a thickness of 125 μm;

[0173] (4) applying a silicone release film to the surface of the strong adhesive layer, then rolling it up and aging it at 70° C. for 24 h;

[0174] (5) coating the B adhesive on the other surface of the PI film, and then drying and curing at 130°C to form a weak adhesive layer with a thickness of 125 μm;

[0175] (6) A fluorine release film is pasted on the surface of the weak adhesive layer, and then rolled up to obtain a thermally conductive double-sided adhesive.

[0176] The thermal conductivity, breakdown voltage, peel force, and ring-shaped initial adhesion of the thermally conductive double-sided adhesives prepared in Examples 1 to 8 and Comparative Examples 1 to 6 were tested, and the test results are shown in Table 1; the thermal conductivity test refers to the ISO22007-2 standard, the breakdown voltage refers to the ASTM D149 test standard, the peel force refers to the GB / T2792-1981 test standard, and the ring-shaped initial adhesion refers to the GB / T31125-2014 test standard.

[0177] The thermally conductive double-sided adhesives prepared in Examples 1 to 8 and Comparative Examples 1 to 6 were adhered to a steel plate, and the steel plate with the samples was placed in an oven with a preset temperature of 70° C. and kept for 7 days. After the test, the adhesive was removed from the steel plate and the surface of the steel plate was carefully inspected to see if there was any residual colloidal substance. The results are shown in Table 1.

[0178] Table 1 Test results of thermally conductive double-sided adhesive

[0179]

[0180]

[0181] As can be seen from Table 1, the thermally conductive double-sided adhesives of Examples 1 to 3 have a strong adhesive layer and a weak adhesive layer, and both the strong adhesive layer and the weak adhesive layer have excellent thermal conductivity, good electrical insulation, strong initial adhesion and high peel strength. Therefore, the strong adhesive layer of the thermally conductive double-sided adhesive can be used to bond hard surfaces such as metal or plastic, while the weak adhesive layer is used to bond softer or more sensitive materials, such as electronic components. In addition, the thermally conductive double-sided adhesive of the present invention has no residual adhesive after peeling, and can be reworked without affecting the cleanliness of electronic products.

[0182] Comparing Example 1 with Examples 4 to 5, it can be seen that the content of the first curing agent in the A glue directly affects the final residual adhesive amount of the thermally conductive double-sided adhesive, that is, when the content of the first curing agent is greater than 0.5 parts, the colloid will over-react during the curing process, producing more by-products, such as small molecular volatiles, which will cause the internal structure of the colloid to be loose, thereby leaving more residues when peeling; when the content of the first curing agent is less than 0.5 parts, the colloid cannot be completely cured, resulting in poor physical properties, such as insufficient viscosity, hardness and elasticity, which will also leave more residual adhesive when peeling. Therefore, the first curing agent of the present invention is preferably 0.5 parts.

[0183] By comparing Example 1 with Examples 4 to 5, it can be seen that the content of the cross-linking agent in glue B will also directly affect the final amount of residual glue in the thermally conductive double-sided adhesive, that is, when the cross-linking agent content is greater than 0.3 parts, the colloid will be prompted to form an overly dense three-dimensional network structure, which may make the colloid too hard and lack appropriate elasticity, resulting in the colloid being easily broken during peeling and increasing the amount of residual glue; when the cross-linking agent content is less than 0.3 parts, the network structure of the colloid will be unstable, resulting in the colloid being easily worn or decomposed during use, and residual glue will also be left during peeling; therefore, the cross-linking agent of the present invention is preferably 0.3 parts.

[0184] Comparing Example 1 with Examples 6 to 7, it can be seen that in the formula of A and B glue, the content of the tackifier has a direct and important impact on the final performance of the thermally conductive double-sided adhesive, especially the amount of residual glue, peel force and ring initial adhesion. Specifically, when the content of the first tackifier is less than 2.1 parts and the content of the second tackifier is less than 2.4 parts, the colloid cannot quickly establish sufficient adhesion when contacting the surface, which may lead to insufficient bonding strength; and when the content of the first tackifier is greater than 2.1 parts and the content of the second tackifier is greater than 2.4 parts, the surface of the colloid will be too sticky, and it will be difficult to cleanly detach from the bonded surface when peeling, leaving more residual glue. Therefore, the first tackifier of the present invention is preferably 2.1 parts, and the second tackifier is preferably 2.4 parts.

[0185] By comparing Example 1 with Comparative Examples 1 to 2, it can be seen that removing the tackifier or leveling agent from the formula of A and B glue will affect the initial adhesion and peel strength of the colloid. This is because the introduction of the tackifier can effectively solve the problem of decreased viscosity of the adhesive caused by the addition of thermal conductive powder, and the leveling agent helps to evenly distribute the glue to prevent the local adhesion from being too strong or too weak. This also shows that the tackifier and the leveling agent of the present invention work together to ensure that the double-sided adhesive has a strong initial adhesion and a high peel strength.

[0186] By comparing Example 1 with Comparative Example 3, it can be seen that the use of PI film with excellent electrical insulation properties and thermal stability as the substrate ensures that the electrical breakdown strength of the double-sided adhesive will not be significantly attenuated even after the conductive carbon fiber is added, thereby ensuring thermal conductivity while maintaining good electrical insulation properties.

[0187] Comparing Example 1 with Comparative Examples 4 to 6, it can be seen that replacing the modified carbon fiber with alumina thermal conductive powder or removing the modified carbon fiber or replacing the modified carbon fiber with unmodified carbon fiber will seriously affect the thermal conductivity and viscosity of the double-sided adhesive. This shows that by using a coupling agent to modify the surface of the carbon fiber, the surface of the carbon fiber is activated, which improves the compatibility and bonding force between the carbon fiber and the glue matrix and enhances the thermal conductivity path. Therefore, the first modified carbon fiber and the second modified carbon fiber can be added to the A glue and the B glue respectively without significantly reducing the viscosity to enhance their thermal conductivity.

[0188] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention is described in detail with reference to the preferred embodiments, it is not limited to those listed in the embodiments. Those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A method for preparing a thermally conductive double-sided adhesive, characterized in that the steps include: (1) mixing acrylic glue, a first solvent, a first tackifier, an antioxidant, a first leveling agent, a first modified carbon fiber, and a first thermal conductive powder, stirring evenly, then adding a first curing agent, and stirring evenly to obtain glue A; The silicone pressure-sensitive adhesive, the anchoring agent, the second solvent, the second tackifier, the cross-linking agent, the second leveling agent, the second modified carbon fiber, and the second thermal conductive powder are mixed, stirred evenly, and then the second curing agent is added, and stirred evenly to obtain glue B; (2) corona treatment of the PI film; (3) coating the A glue on one surface of the PI film, and drying and curing it to form a strong surface glue layer; (4) applying the first release film to the surface of the strong adhesive layer, and then rolling and curing the film; (5) coating the B glue on the other surface of the PI film, and drying and curing it to form a weak surface glue layer; (6) A second release film is attached to the surface of the weak adhesive layer, and then rolled up to obtain a thermally conductive double-sided adhesive; wherein the preparation of the first modified carbon fiber and the second modified carbon fiber includes: placing the carbon fiber in an aqueous solution containing a coupling agent and ethanol for pretreatment.

2. The method for preparing the thermally conductive double-sided adhesive according to claim 1, characterized in that: In terms of mass, the raw materials for preparing the A glue include 50 to 100 parts of acrylic glue, 50 to 200 parts of a first solvent, 1 to 3 parts of a first tackifier, 0.1 to 0.8 parts of an antioxidant, 0.1 to 0.8 parts of a leveling agent, 600 to 800 parts of a first modified carbon fiber, 100 to 200 parts of a first thermally conductive powder, and 0.1 to 1.2 parts of a first curing agent; the raw materials for preparing the B glue include 50 to 100 parts of silicone pressure-sensitive glue, 0.1 to 2 parts of an anchoring agent, 50 to 200 parts of a second solvent, 1 to 3 parts of a second tackifier, 0.1 to 1 parts of a cross-linking agent, 0.1 to 2 parts of a second leveling agent, 700 to 900 parts of a second modified carbon fiber, 100 to 200 parts of a second thermally conductive powder, and 0.1 to 1 parts of a second curing agent.

3. The method for preparing the thermally conductive double-sided adhesive according to claim 1, characterized in that: The first curing agent is 0.5 parts; the cross-linking agent is 0.3 parts; the first tackifier is 2.1 parts; and the second tackifier is 2.4 parts.

4. The method for preparing the thermally conductive double-sided adhesive according to claim 1, characterized in that: The first curing agent is epoxy resin; the cross-linking agent is at least one of hydrogen-containing silicone oil, benzoyl peroxide and di(2,4-dichlorobenzoyl) peroxide.

5. The method for preparing the thermally conductive double-sided adhesive according to claim 1, characterized in that: The first release film is a silicone release film, and the second release film is a fluorine release film.

6. The method for preparing the thermally conductive double-sided adhesive according to claim 1, characterized in that: The first solvent is ethyl acetate, and the second solvent is toluene.

7. The method for preparing the thermally conductive double-sided adhesive according to claim 1, characterized in that: The thickness of the PI film is 25 to 100 μm; the thickness of the strong surface adhesive layer and the weak surface adhesive layer are each independently 50 to 200 μm.

8. The method for preparing the thermally conductive double-sided adhesive according to claim 1, characterized in that: The first thermally conductive powder and the second thermally conductive powder are each independently selected from at least one of aluminum hydroxide, boron nitride, aluminum nitride, zinc oxide, and aluminum oxide.

9. The method for preparing the thermally conductive double-sided adhesive according to claim 1, characterized in that: The acrylic glue has a solid content of 43-47% and a viscosity of 1500-3500 cps; the silicone pressure-sensitive glue has a solid content of 58-62% and a viscosity of 18000-22000 cps.

10. A thermally conductive double-sided adhesive, characterized in that: The thermally conductive double-sided adhesive is prepared by the preparation method according to any one of claims 1 to 9.