Preparation method and application of Al-Zn-Mg composite coating
Preparation of Al-Zn-Mg composite coating through cold spraying process solves the problems of high-temperature oxidation and corrosion resistance in thermal spraying process, forming a hard protective layer, significantly improving the corrosion resistance and service life of the coating, and is suitable for the ocean Steel protection in the environment.
Patent Information
- Application Number
- CN202410934482.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-11-29
AI Technical Summary
The existing metal protective coatings are susceptible to corrosion in marine environments, especially when the Al coating is damaged by Cl- in seawater, the corrosion resistance is reduced, and the high-temperature oxidation in the thermal spraying process is severely affected, affecting the coating performance.
The Al-Zn-Mg composite coating was prepared by cold spraying technology, and compressed air was used to use spherical Al powder, Zn powder and Mg powder in a ratio of 73 to 76 wt.% Al, 23 wt.% Zn, 1 to 4 wt.% Mg. Spraying, control spraying parameters such as gas pressure, temperature and movement speed, build an XY automation platform for shaping, and form a hard shell-like protective layer.
Effectively inhibit oxidation and phase transition, extend the service life of the coating, prevent pitting, improve the corrosion resistance of steel substrates, and provide long-term protection in seawater.
Smart Images

Figure CN119040870A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of material anticorrosion, and specifically relates to a preparation method of an Al-Zn-Mg composite coating and application thereof. Background Art
[0002] In the process of developing the ocean, humans have built a series of steel buildings, such as offshore drilling platforms, tidal power generation equipment, submarine pipelines, etc. These steel buildings are extremely susceptible to corrosion in the marine environment, causing economic losses and even safety accidents.
[0003] There are many ways to protect steel, and the most widely used one is metal protective coating. Thermal methods such as thermal spraying and hot dip plating are one of the important methods for preparing metal protective coatings, but these preparation methods require melting of raw materials such as metal wires during the working process. The metal protective coatings prepared by thermal methods are severely oxidized at high temperatures, and the coating composition is limited by the commercially available metal wires.
[0004] Due to its abundant reserves and obvious passivation effect, Al has become one of the preferred materials for metal protective coatings. However, the passivation film of Al coating will be destroyed by Cl in seawater. - The damage eventually develops into pitting. In order to improve the anode performance of Al, elements such as Zn and Mg are often added. Simply adding Zn can improve the performance of pure Al coating, but Zn has a higher electronegativity than Mg, so its sacrificial ability is weaker than Mg. In addition, Al-Zn coating relies too much on the sealing effect of corrosion products. In practical applications, once the corrosion products are destroyed, the corrosion resistance of the coating will be greatly reduced. Summary of the invention
[0005] The purpose of this section is to summarize some aspects of embodiments of the present invention and briefly introduce some preferred embodiments. Some simplifications or omissions may be made in this section and the specification abstract and the invention title of this application to avoid blurring the purpose of this section, the specification abstract and the invention title, and such simplifications or omissions cannot be used to limit the scope of the present invention.
[0006] In view of the above problems and / or the problems existing in the prior art, the present invention is proposed.
[0007] Therefore, the object of the present invention is to overcome the deficiencies in the prior art and provide a method for preparing an Al-Zn-Mg composite coating.
[0008] In order to solve the above technical problems, the present invention provides the following technical solutions: a method for preparing an Al-Zn-Mg composite coating, comprising:
[0009] The composite coating was prepared by using spherical Al powder, Zn powder and Mg as raw materials and treating the substrate by cold spraying process;
[0010] After shaping treatment, a cold-sprayed Al-Zn-Mg composite coating is obtained;
[0011] Wherein, based on the mass percentage of raw materials, the Al is 73-76wt.%, the Zn is 23wt.%, and the Mg is 1-4wt.%.
[0012] As a preferred embodiment of the preparation method described in the present invention, the cold spraying process parameters are as follows: the powder feeding gas is compressed air, the spraying angle is 90°, the gas pressure is 0.8-1.2 MPa, the powder feeding temperature is 400-500°C, the powder feeding amount is 40-60 g / min, the distance between the spray gun and the substrate is 10-12 mm, and the spray gun moving speed is 5-8 mm / s.
[0013] As a preferred embodiment of the preparation method of the present invention, the substrate is treated by:
[0014] Build an XY automation platform and check the operation of the spray robot to see if there is any shaking or jamming;
[0015] The base steel was pretreated and grease was removed by ultrasonic cleaning with acetone;
[0016] Use corundum for sandblasting to remove rust and increase the surface roughness of the substrate.
[0017] As a preferred embodiment of the preparation method of the present invention, wherein: in terms of element mass percentage, the Al is 76wt.%, the Zn is 23wt.%, and the Mg is 1wt.%.
[0018] As a preferred embodiment of the preparation method of the present invention, wherein: in terms of element mass percentage, the Al is 75wt.%, the Zn is 23wt.%, and the Mg is 2wt.%.
[0019] As a preferred embodiment of the preparation method of the present invention, wherein: in terms of element mass percentage, the Al is 74wt.%, the Zn is 23wt.%, and the Mg is 3wt.%.
[0020] As a preferred embodiment of the preparation method of the present invention, wherein: in terms of element mass percentage, the Al is 73wt.%, the Zn is 23wt.%, and the Mg is 4wt.%.
[0021] Another object of the present invention is to overcome the deficiencies in the prior art and provide a cold sprayed Al-Zn-Mg composite coating.
[0022] Another object of the present invention is to overcome the deficiencies in the prior art and provide a cold sprayed Al-Zn-Mg composite coating for use as an anti-corrosion coating.
[0023] Beneficial effects of the present invention:
[0024] (1) The cold spraying technology used in the present invention has a low working temperature when preparing the coating, which effectively inhibits the adverse effects such as oxidation, phase change, and grain growth.
[0025] (2) The Mg element added in the present invention can enhance the sacrificial effect of the coating and generate a hard shell-like protective layer, effectively extending the service life of the Al-Zn coating in practical applications; the cold-sprayed Al-Zn-Mg composite coating in the present invention can effectively solve the adverse effects of oxidation, phase change, grain growth, etc. caused by excessive temperature in methods such as thermal spraying, and effectively prevent the occurrence of pitting corrosion in seawater, ultimately achieving the purpose of effectively protecting the steel substrate for a long time. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the following briefly introduces the drawings required for describing the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative labor. Among them:
[0027] Figure 1 It is the cross-sectional BES diagram of the cold-sprayed Al-Zn-Mg composite coating in the comparative example and the embodiment of the present invention, wherein a and b are Al-23Zn-3Mg and Al-23Zn respectively.
[0028] Figure 2 It is the BES diagram of the Al-Zn-Mg composite coating in the comparative example and the embodiment of the present invention after being subjected to a salt spray test in a 5% NaCl solution for 480 hours, wherein a and b are Al-23Zn-3Mg and Al-23Zn respectively.
[0029] Figure 3 The electrochemical test results of the Al-Zn-Mg composite coatings in the comparative examples and embodiments of the present invention after being immersed in a 3.5% NaCl solution for 480 hours.
[0030] Figure 4 These are the hardness test results of the Al-Zn-Mg composite coatings in the comparative examples and embodiments of the present invention. DETAILED DESCRIPTION
[0031] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are described in detail below in conjunction with the embodiments of the specification.
[0032] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein, and those skilled in the art may make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.
[0033] Secondly, the term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the present invention. The term "in one embodiment" that appears in different places in this specification does not necessarily refer to the same embodiment, nor does it refer to a separate or selective embodiment that is mutually exclusive with other embodiments.
[0034] The XY automation platform in the embodiment of the present invention is provided by Guangzhou Diens Company, and includes an X-axis mechanical arm that moves left and right and a Y-axis mechanical arm that moves forward and backward, and can control the moving distance and moving speed more accurately.
[0035] Example 1
[0036] S1: Build an XY automation platform and check the operation of the spraying robot to see if there is any shaking or jamming;
[0037] S2: pre-treat the Q235 steel substrate and use acetone ultrasonic cleaning to remove oil stains;
[0038] S3: Use corundum for sandblasting to remove rust and increase the surface roughness of the substrate;
[0039] S4: Use spherical Al powder, Zn and Mg powder as raw materials, with a weight ratio of Al 76wt.%, Zn 23wt.%, Mg 1wt.%, mix well and put into a vacuum drying oven to dry for 2 hours.
[0040] S5: The powder feeding gas is compressed air, the spraying angle is 90°, the gas pressure is 0.8-1.2MPa, the powder feeding temperature is 400-500℃, the powder feeding amount is 40-60g / min, the distance between the spray gun and the substrate is 10-12mm, and the spray gun moving speed is 5-8mm / s. This parameter is used to prepare the cold spray composite coating;
[0041] S6: After shaping treatment and strict inspection and acceptance, the cold-sprayed Al-Zn-Mg composite coating is obtained.
[0042] S7: Solder the wires using a solder gun and encapsulate with resin to expose only the test surface.
[0043] S8: The encapsulated samples were immersed in a 3.5% NaCl solution for 480 h and electrochemical tests were performed.
[0044] S9: Two batches of samples were encapsulated using hot mounting powder, and only the test surface was exposed to a neutral salt spray test using a 5% NaCl solution.
[0045] Hardness test was performed using a microhardness tester.
[0046] Example 2
[0047] S1: Build an XY automation platform and check the operation of the spraying robot to see if there is any shaking or jamming;
[0048] S2: pre-treat the Q235 steel substrate and use acetone ultrasonic cleaning to remove oil stains;
[0049] S3: Use corundum for sandblasting to remove rust and increase the surface roughness of the substrate;
[0050] S4: Use spherical Al powder, Zn and Mg powder as raw materials, with a weight ratio of Al 75wt.%, Zn 23wt.%, Mg 2wt.%, mix well and put into a vacuum drying oven to dry for 2 hours.
[0051] S5: The powder feeding gas is compressed air, the spraying angle is 90°, the gas pressure is 0.8-1.2MPa, the powder feeding temperature is 400-500℃, the powder feeding amount is 40-60g / min, the distance between the spray gun and the substrate is 10-12mm, and the spray gun moving speed is 5-8mm / s. This parameter is used to prepare the cold spray composite coating;
[0052] S6: After shaping treatment and strict inspection and acceptance, the cold-sprayed Al-Zn-Mg composite coating is obtained.
[0053] S7: Solder the wires using a solder gun and encapsulate with resin to expose only the test surface.
[0054] S8: The encapsulated samples were immersed in a 3.5% NaCl solution for 480 h and electrochemical tests were performed.
[0055] S9: Two batches of samples were encapsulated using hot mounting powder, and only the test surface was exposed to a neutral salt spray test using a 5% NaCl solution.
[0056] Hardness test was performed using a microhardness tester.
[0057] Example 3
[0058] S1: Build an XY automation platform and check the operation of the spraying robot to see if there is any shaking or jamming;
[0059] S2: pre-treat the Q235 steel substrate and use acetone ultrasonic cleaning to remove oil stains;
[0060] S3: Use corundum for sandblasting to remove rust and increase the surface roughness of the substrate;
[0061] S4: Use spherical Al powder, Zn and Mg powder as raw materials, with a weight ratio of Al 74wt.%, Zn 23wt.%, Mg 3wt.%, mix well and put into a vacuum drying oven to dry for 2 hours.
[0062] S5: The powder feeding gas is compressed air, the spraying angle is 90°, the gas pressure is 0.8-1.2MPa, the powder feeding temperature is 400-500℃, the powder feeding amount is 40-60g / min, the distance between the spray gun and the substrate is 10-12mm, and the spray gun moving speed is 5-8mm / s. This parameter is used to prepare the cold spray composite coating;
[0063] S6: After shaping treatment and strict inspection and acceptance, the cold-sprayed Al-Zn-Mg composite coating is obtained.
[0064] S7: Solder the wires using a solder gun and encapsulate with resin to expose only the test surface.
[0065] S8: The encapsulated samples were immersed in a 3.5% NaCl solution for 480 h and electrochemical tests were performed.
[0066] S9: Two batches of samples were encapsulated using hot mounting powder, and only the test surface was exposed to a neutral salt spray test using a 5% NaCl solution.
[0067] Hardness test was performed using a microhardness tester.
[0068] Example 4
[0069] S1: Build an XY automation platform and check the operation of the spraying robot to see if there is any shaking or jamming;
[0070] S2: pre-treat the Q235 steel substrate and use acetone ultrasonic cleaning to remove oil stains;
[0071] S3: Use corundum for sandblasting to remove rust and increase the surface roughness of the substrate;
[0072] S4: Use spherical Al powder, Zn and Mg powder as raw materials, with a weight ratio of Al 73wt.%, Zn 23wt.%, Mg 4wt.%, mix well and put into a vacuum drying oven to dry for 2 hours.
[0073] S5: The powder feeding gas is compressed air, the spraying angle is 90°, the gas pressure is 0.8-1.2MPa, the powder feeding temperature is 400-500℃, the powder feeding amount is 40-60g / min, the distance between the spray gun and the substrate is 10-12mm, and the spray gun moving speed is 5-8mm / s. This parameter is used to prepare the cold spray composite coating;
[0074] S6: After shaping treatment and strict inspection and acceptance, the cold-sprayed Al-Zn-Mg composite coating is obtained.
[0075] S7: Solder the wires using a solder gun and encapsulate with resin to expose only the test surface.
[0076] S8: The encapsulated samples were immersed in a 3.5% NaCl solution for 480 h and electrochemical tests were performed.
[0077] S9: Two batches of samples were encapsulated with hot mounting powder, and only the test surface was exposed to a neutral salt spray test using a 5% NaCl solution. A microhardness tester was used for hardness testing.
[0078] Comparative Example 1
[0079] S1: Build an XY automation platform and check the operation of the spraying robot to see if there is any shaking or jamming;
[0080] S2: pre-treat the Q235 steel substrate and use acetone ultrasonic cleaning to remove oil stains;
[0081] S3: Use corundum for sandblasting to remove rust and increase the surface roughness of the substrate;
[0082] S4: Use spherical Al powder and Zn powder as raw materials, with a weight ratio of Al 77wt.%, Zn 23wt.%, mix well and put into a vacuum drying oven to dry for 2 hours.
[0083] S5: The powder feeding gas is compressed air, the spraying angle is 90°, the gas pressure is 0.8-1.2MPa, the powder feeding temperature is 400-500℃, the powder feeding amount is 40-60g / min, the distance between the spray gun and the substrate is 10-12mm, and the spray gun moving speed is 5-8mm / s. This parameter is used to prepare the cold spray composite coating;
[0084] S6: After shaping treatment and strict inspection and acceptance, the cold sprayed Al-Zn coating is obtained.
[0085] S7: Solder the wires using a solder gun and encapsulate with resin to expose only the test surface.
[0086] S8: The encapsulated samples were immersed in a 3.5% NaCl solution for 480 h and electrochemical tests were performed.
[0087] S9: Two batches of samples were encapsulated using hot mounting powder, and only the test surface was exposed to a neutral salt spray test using a 5% NaCl solution.
[0088] Hardness test was performed using a microhardness tester.
[0089] Cross-sectional BES diagram of cold sprayed Al-Zn-Mg composite coating Figure 1 .
[0090] Comparative Example 2
[0091] S1: Build an XY automation platform and check the operation of the spraying robot to see if there is any shaking or jamming;
[0092] S2: pre-treat the Q235 steel substrate and use acetone ultrasonic cleaning to remove oil stains;
[0093] S3: Use corundum for sandblasting to remove rust and increase the surface roughness of the substrate;
[0094] S4: Use spherical Al powder, Zn and Mg powder as raw materials, with a weight ratio of Al 72wt.%, Zn 23wt.%, Mg 5wt.%, mix well and put into a vacuum drying oven to dry for 2 hours.
[0095] S5: The powder feeding gas is compressed air, the spraying angle is 90°, the gas pressure is 0.8-1.2MPa, the powder feeding temperature is 400-500℃, the powder feeding amount is 40-60g / min, the distance between the spray gun and the substrate is 10-12mm, and the spray gun moving speed is 5-8mm / s. This parameter is used to prepare the cold spray composite coating;
[0096] S6: After shaping treatment and strict inspection and acceptance, the cold-sprayed Al-Zn-Mg composite coating is obtained.
[0097] S7: Solder the wires using a solder gun and encapsulate with resin to expose only the test surface.
[0098] S8: The encapsulated samples were immersed in a 3.5% NaCl solution for 480 h and electrochemical tests were performed.
[0099] S9: Two batches of samples were encapsulated using hot mounting powder, and only the test surface was exposed to a neutral salt spray test using a 5% NaCl solution.
[0100] Hardness test was performed using a microhardness tester.
[0101] One hot-mounted sample in step S9 of the embodiment and the comparative example was taken, and hardness test was performed using a microhardness tester. The results are shown in Tables 1 and Figure 4 shown.
[0102] Table 1
[0103]
[0104] It can be seen that the hardness of the cold sprayed Al-Zn-Mg composite coating increases with the increase of Mg content.
[0105] The hot-mounted samples in step S9 of the embodiment and the comparative example were placed in a salt spray chamber to conduct a neutral salt spray test.
[0106] Among them, the salt spray test is based on GB / T 2423.17-2008. Specifically, the neutral salt spray test is carried out in a YC-60 salt spray tester. All coating surfaces maintain an angle of 30° with the horizontal plane. The samples are taken out after 480 hours to observe the corrosion morphology. The working temperature of the salt spray box is maintained at 35°C, and the spray solution is 5% NaCl solution with a pH value of 6.5-7.2.
[0107] The results are as follows Figure 2 As shown, it can be seen that the coating with Mg added will generate a shell-like protective layer to prevent the salt spray from further corroding the coating, and the resulting BES diagram of the corrosion product is more uniform than that of the ordinary Al-Zn coating.
[0108] The samples immersed in step S8 in the embodiment and the comparative example were subjected to electrochemical impedance test.
[0109] Among them, the electrochemical test was carried out using a Princeton P4000A electrochemical workstation, equipped with a circulating water device, the temperature was controlled at 25±1°C, the corrosive electrolyte was a 3.5% NaCl aqueous solution, and it was carried out under a conventional three-electrode system. The immersion time was 480h, and the potentiodynamic polarization test was performed with a scanning frequency of 5mV / s and a scanning range of ±0.5Vvs.SHE.
[0110] The results are shown in Table 2 and Figure 3 As shown, it can be seen that among the various embodiments and comparative examples, the coating prepared in Example 3 has the highest self-corrosion potential and the lowest self-corrosion current density, so it has the smallest corrosion tendency, the slowest corrosion rate, and the best corrosion resistance.
[0111] Table 2
[0112]
[0113] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solutions of the present invention can be modified or replaced by equivalents without departing from the spirit and scope of the technical solutions of the present invention, which should all be included in the scope of the present invention.
Claims
1. A method for preparing an Al-Zn-Mg composite coating, Features: include, The composite coating was prepared by using spherical Al powder, Zn powder and Mg as raw materials and treating the substrate by cold spraying process; After shaping treatment, a cold-sprayed Al-Zn-Mg composite coating is obtained; Wherein, based on the mass percentage of raw materials, the Al is 73-76wt.%, the Zn is 23wt.%, and the Mg is 1-4wt.%.
2. The preparation method according to claim 1, Features: The cold spraying process parameters are as follows: the powder feeding gas is compressed air, the spraying angle is 90°, the gas pressure is 0.8-1.2 MPa, the powder feeding temperature is 400-500°C, the powder feeding amount is 40-60 g / min, the distance between the spray gun and the substrate is 10-12 mm, and the spray gun moving speed is 5-8 mm / s.
3. The preparation method according to claim 1 or 2, Features: The substrate, and the processing method thereof comprises: Build an XY automation platform and check the operation of the spray robot to see if there is any shaking or jamming; The base steel was pretreated and grease was removed by ultrasonic cleaning with acetone; Use corundum for sandblasting to remove rust and increase the surface roughness of the substrate.
4. The preparation method according to claim 1, Features: In terms of element mass percentage, the Al is 76 wt.%, the Zn is 23 wt.%, and the Mg is 1 wt.%.
5. The preparation method according to claim 1, Features: In terms of element mass percentage, the Al is 75 wt.%, the Zn is 23 wt.%, and the Mg is 2 wt.%.
6. The preparation method according to claim 1, Features: In terms of element mass percentage, the Al is 74 wt.%, the Zn is 23 wt.%, and the Mg is 3 wt.%.
7. The preparation method according to claim 1, Features: In terms of element mass percentage, the Al is 73 wt.%, the Zn is 23 wt.%, and the Mg is 4 wt.%.
8. A cold sprayed Al-Zn-Mg composite coating obtained by the preparation method according to any one of claims 1 to 7.
9. Use of the cold sprayed Al-Zn-Mg composite coating as claimed in claim 8 as an anti-corrosion coating.
Citation Information
Patent Citations
Steel structure part surface protective coating and preparation method thereof
CN105624665A
Spraying powder for cold spraying of magnesium alloy wheel and spraying process and evaluation method thereof
CN114318324A
Thermal spraying Zn-Al-Mg alloy coating and preparation method thereof
CN114774832A
Zn-Al-Mg Alloy Coating Steel Sheet Having SuperiorCorrosion Resistance And Plating Workability
KR1020030054469A
Method of forming improved zinc-aluminum coating on ferrous surfaces
US3393089A