Perovskite nano crystal and preparation method thereof

By designing the flow channel system and metal pipelines, the problem of low mass production efficiency of perovskite nanocrystals was solved, and stable mass production of perovskite nanocrystals with high quantum efficiency was achieved, which can be applied to multiple technical fields.

CN119041028APending Publication Date: 2024-11-29ETERNAL SPECIALTY MATERIALS ZHUHAI CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310616184.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-29
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Existing technologies make it difficult to stably mass-produce perovskite nanocrystals with high quantum efficiency, especially red perovskite nanocrystals. Furthermore, batch synthesis methods are susceptible to human interference and are not conducive to mass production.

Method used

A flow channel system was used, with metal pipes (such as stainless steel pipes) as reactor pipelines. After preheating the cesium and lead precursor solutions, the mixture was converged in a micro mixer and reacted in the reactor. The reaction conditions were controlled to prepare perovskite nanocrystals.

Benefits of technology

The quantum efficiency of perovskite nanocrystals has been improved to over 80%, preferably over 90%, making them suitable for fields such as color conversion display technology, energy materials, smart sensing, and biomedical imaging.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119041028A_ABST
    Figure CN119041028A_ABST
Patent Text Reader

Abstract

The invention provides a perovskite nano crystal and a preparation method thereof, and the method for preparing the perovskite nano crystal is a method for preparing the perovskite nano crystal through a runner system, and comprises the following steps: providing a cesium precursor solution and a lead precursor solution; respectively preheating the cesium precursor solution and the lead precursor solution; and converging the pre-heated cesium precursor and the pre-heated lead precursor, and conveying the converged mixture to a reactor for reaction to obtain the perovskite nano crystal, wherein the reactor comprises a metal tube. The perovskite nano crystal provided by the invention has quantum efficiency of at least about 80%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a perovskite nanocrystal and a preparation method thereof, and in particular to a method for continuously mass-producing perovskite nanocrystals using a flow channel system and the resulting product.

[0002] Prior Art

[0003] With the development of technology, electronic products have become more diversified. Not only do they pursue thinness and lightness, but the public's requirements for the resolution of electronic devices have also increased. Micro light-emitting diodes (micro-LEDs) with chip sizes less than 50μm have attracted attention from all walks of life due to their excellent brightness, lifespan, efficiency and resolution. To produce full-color micro-LEDs, different red, green and blue wafers can be used to manufacture RGB micro-LEDs, but the problem of mass transfer and the complexity of the process greatly increase the difficulty of manufacturing. Another solution is to use blue micro-LEDs to excite color conversion layers, such as quantum dots, phosphors, etc. The process is relatively simple, only a single drive circuit is required, and it is easier to adjust the efficiency between different colors. Compared with the use of RGB micro-LEDs, the use of monochrome micro-LEDs with color conversion layers has lower energy consumption and better efficiency.

[0004] The most common color conversion layers today are phosphors and quantum dots. Phosphors have the characteristics of high stability, wide absorption range and large half-width. They have been developed for many years and have mature market applications. However, their size is generally hundreds of microns, which limits their application in micro-LEDs. Quantum dots are nanometers in size, and perovskite quantum dots have the characteristics of high absorption coefficient, high quantum efficiency and narrow half-width, which greatly increases their application in micro-LEDs.

[0005] Common methods for synthesizing perovskite quantum dots include reverse microemulsion method, self-assembly method, antisolvent vapor-assisted crystallization method and hot-injection method. [1-3] The above method belongs to batch synthesis, which has a simple process and is easy to operate, but it is difficult to accurately control the conditions of each synthesis, resulting in the synthesis process being easily interfered by human factors and low experimental repeatability. In addition, the batch synthesis method is not conducive to mass production.

[0006] Phillips et al. (2014) [4]Proposed to synthesize perovskite nanocrystals through microfluidic system to improve reaction control and product quality. Lignos et al. [5] The perovskite nanocrystals of CsPbBr3 were synthesized by a microfluidic system, and the ratio of halogens was changed by the microfluidic system to adjust the emission wavelength between 410nm and 700nm. However, the quantum efficiency of the perovskite nanocrystals synthesized by the microfluidic system still has room for improvement.

[0007] Although existing literature indicates that perovskite nanocrystal products can be synthesized through a microfluidic system, there is currently a lack of methods on the market that can stably mass-produce perovskite nanocrystals with high quantum efficiency, especially methods that can stably mass-produce red perovskite nanocrystals with quantum efficiencies of 80% or even more than 90%.

[0008] Therefore, there is a need in the art for a perovskite nanocrystal that can be practically mass-produced and has good quality (such as high quantum efficiency). Summary of the invention

[0009] The present invention provides a method for preparing perovskite nanocrystals, comprising:

[0010] Providing cesium precursor solution and lead precursor solution;

[0011] Preheating the cesium precursor solution and the lead precursor solution respectively; and

[0012] The preheated cesium precursor and the preheated lead precursor are combined and transported to a reactor for reaction to obtain perovskite nanocrystals.

[0013] The reactor comprises a metal tube.

[0014] The present invention further provides a perovskite nanocrystal prepared by the above method and having a quantum efficiency of at least about 80%.

[0015] The inventors unexpectedly discovered that using metal tubes (such as stainless steel tubes) instead of Teflon tubes as pipelines of the flow system, especially reactor pipelines, helps to improve the reaction efficiency and the quality of the reaction products, and can make the quantum efficiency of the obtained perovskite nanocrystals as high as about 80% or more, preferably about 90% or more, so that the obtained perovskite nanocrystals can be more advantageously applied to various fields, such as color conversion display technology, energy materials, smart sensors, biomedical imaging and other fields. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Aspects of the present invention are best understood from the following detailed description when read in conjunction with the accompanying drawings. It should be noted that, in accordance with standard practice in the industry, the various components are not drawn to scale. In fact, the dimensions of the various components may be arbitrarily increased or reduced for clarity of discussion.

[0017] Figure 1 It is a schematic diagram of the flow channel system used for preparing perovskite nanocrystals according to the present invention.

[0018] Figure 2 It is a flow chart of the method for preparing perovskite nanocrystals of the present invention.

[0019] Figure 3 (a) is an X-ray diffraction pattern of red perovskite nanocrystals in one embodiment of the present invention.

[0020] Figure 3 (b) is the X-ray diffraction pattern of existing CsPbBr3.

[0021] Figure 4 This is a TEM image of red perovskite nanocrystals in one embodiment of the present invention.

[0022] Figure 5 It is the absorption and emission spectra of perovskite nanocrystals in one embodiment of the present invention.

[0023] Implementation

[0024] The present invention may be more readily understood with reference to this detailed description and the examples included herein. A number of specific details are set forth in order to provide a thorough understanding of the examples described herein. However, it will be understood by those of ordinary skill in the art that the examples described herein may be practiced without these specific details. In addition, the description herein is not to be construed as limiting the scope of the present invention.

[0025] Unless otherwise specified in the text, in this specification (especially in the scope of the patent application), the terms "a", "an", "the", "said" and similar terms used should be understood to include both singular and plural forms. In addition, for the sake of clarity, the dimensions of various components and regions may be exaggerated in the drawings, and are not drawn according to the actual scale.

[0026] It should be understood that any numerical range cited in this specification is intended to include all sub-ranges included therein. For example, a range from "1 to 10" includes all sub-ranges between the stated minimum value 1 and the maximum value 10 (such as from 2 to 8, 3 to 6, or 4 to 9, etc.) and includes these two values, that is, a range including a minimum value equal to or greater than 1 and a maximum value equal to or less than 10. Because the disclosed numerical range is continuous, each value between the minimum and maximum values ​​is included. Unless otherwise specified, the various numerical ranges specified in this specification are approximate values.

[0027] Furthermore, in this document, the term "about" means an acceptable error for a particular value as determined by one of ordinary skill in the art, depending on how the value is measured or determined.

[0028] [Flow channel system for preparing perovskite nanocrystals]

[0029] The present invention prepares perovskite nanocrystals by using a flow channel system.

[0030] Please see Figure 1 The flow channel system of the present invention for preparing perovskite nanocrystals comprises:

[0031] A first flow channel P1 for conveying the cesium precursor solution 10, wherein the first flow channel P1 passes through a first heating zone 12 and is used for preheating the cesium precursor solution 10;

[0032] A second flow channel P2 for conveying the lead precursor solution 20, the second flow channel P2 passing through a second heating zone 22 for preheating the lead precursor solution 20;

[0033] A micro mixer 30 connecting the first flow channel P1 and the second flow channel P2;

[0034] The reactor 40 is connected to the micro mixer 30 .

[0035] The flow channel system is operated at a pressure of about 1 to about 12 bar.

[0036] According to some embodiments of the present invention, the inner diameters of the first flow channel P1 and the second flow channel P2 of the flow channel system of the present invention may be about 0.1 cm to about 5 cm, but not limited thereto.

[0037] According to some embodiments of the present invention, the first flow channel P1 and the second flow channel P2 of the flow channel system of the present invention can be independently Teflon tubes or metal tubes.

[0038] According to some embodiments of the present invention, the first flow channel P1 of the flow channel system of the present invention is a Teflon tube or a metal tube.

[0039] According to some embodiments of the present invention, the second flow channel P2 of the flow channel system of the present invention is a metal tube.

[0040] According to some embodiments of the present invention, the first heating zone 12 may be a water bath, an oil bath, an electric heating zone, an infrared heating zone, or other forms of heating zones. According to some embodiments of the present invention, the cesium precursor solution 10 may be preheated by passing the first flow channel P1 through the first heating zone 12, for example, the first flow channel P1 passing through the first heating zone 12 may be immersed in a water bath or an oil bath for heating; or the first flow channel P1 passing through the first heating zone 12 may be heated by a heater (e.g., an electric heater, an infrared heater, etc.) (but not limited thereto).

[0041] According to some embodiments of the present invention, the second heating zone 22 may be a water bath, an oil bath, an electric heating zone, an infrared heating zone, or other forms of heating zones. According to some embodiments of the present invention, the lead precursor solution 20 may be preheated by passing the second flow channel P2 through the second heating zone 22, for example, the second flow channel P2 passing through the second heating zone 22 may be immersed in a water bath or an oil bath for heating; or the second flow channel P2 passing through the second heating zone 22 may be heated by a heater (e.g., an electric heater, an infrared heater, etc.) (but not limited thereto).

[0042] According to some embodiments of the present invention, the aforementioned micro-mixer 30 is made of metal and is connected to the first flow channel P1 and the second flow channel P2, so that the cesium precursor solution 10 flows through the first flow channel P1 and is input into the micro-mixer 30 after being preheated, and the lead precursor solution 20 flows through the second flow channel P2 and is input into the micro-mixer 30 after being preheated. In some embodiments, the cesium precursor solution 10 and the lead precursor solution 20 are directly output to the subsequent reactor 40 only after converging in the micro-mixer 30, so the micro-mixer 30 does not need to be specially heated.

[0043] According to some embodiments of the present invention, the reactor 40 is connected to the micro-mixer 30 through a connecting pipe P3, and the connecting pipe P3 is a metal pipe. The cesium precursor solution 10 and the lead precursor solution 20 react in the reactor 40 to form perovskite nanocrystals. The volume in the reactor 40 can be about 1 mL to about 50 mL, and it can be heated by the third heating zone 42. The third heating zone 42 can be a water bath, an oil bath, an electric heating zone, an infrared heating zone, or other forms of heating zones. According to some embodiments of the present invention, the reactor 40 can be heated by immersing it in a water bath or an oil bath or by a heater (such as an electric heater, an infrared heater, etc.) to heat the reactor 40 (but not limited to this).

[0044] According to some embodiments of the present invention, the flow channel system for preparing perovskite nanocrystals of the present invention may further include:

[0045] a solvent storage tank 50 connected to the connecting pipe P3 at a connection point C through a delivery pipe P4 to provide a small amount of unheated solvent to the reactor 40, wherein the distance from the micro-mixer 30 to the connection point C is smaller than the distance from the connection point C to the reactor 40, and the ratio of the distance from the micro-mixer 30 to the connection point C to the distance from the connection point C to the reactor 40 is about 1:4 to 1:6; and

[0046] The collector 60 includes a pump and is connected to the reactor 40 through a delivery pipe P5 for collecting the perovskite nanocrystals obtained from the reactor 40 .

[0047] According to an embodiment of the present invention, the solvent storage tank 50 can provide a solvent to flush the reactor 40, thereby transporting the perovskite nanocrystal product remaining in the reactor 40 to the collector 60 (see Figure 2 Step S160). In addition, according to an embodiment of the present invention, after the cesium precursor solution 10 and the lead precursor solution 20 are merged in the micro mixer 30, the solvent storage tank 50 can provide additional solvent to the mixed solution after the merger as needed; especially when the added solvent is an unheated solvent, since the distance from the micro mixer 30 to the connecting point C is designed to be smaller than the distance from the connecting point C to the reactor 40, it is helpful to mix the solvent with the mixed solution in advance to obtain a good reaction effect.

[0048] In the present invention, the flow channel system used may be a micro-flow channel system.

[0049] [Method for preparing perovskite nanocrystals]

[0050] Please see Figure 2 As shown, the method of preparing perovskite nanocrystals using a flow channel system of the present invention comprises the following steps:

[0051] Step S110: Providing a cesium precursor solution 10

[0052] The present invention provides a cesium precursor solution in step S110. In some embodiments of the present invention, step S110 comprises mixing a cesium-containing compound with an organic ligand to prepare a cesium precursor solution. The molar concentration of cesium ions in the obtained cesium precursor solution is about 1 to about 40 mM, for example, about 1 mM, about 2 mM, about 3 mM, about 4 mM, about 5 mM, about 5.5 mM, about 6 mM, about 7 mM, about 8 mM, about 9 mM, about 10 mM, about 11 mM, about 12 mM, about 13 mM, about 14 mM, about 15 mM, about 16 mM, about 17 mM, about 18 mM, about 19 mM, about 20 mM, about 25 mM, about 30 mM, about 35 mM, or about 40 mM, preferably about 5 mM to about 35 mM.

[0053] The cesium-containing compound may be cesium oleate, cesium fluoride (CsF), cesium chloride (CsCl), cesium bromide (CsBr), cesium iodide (CsI), cesium carbonate (Cs2CO3) or a combination thereof. The organic ligand may be oleic acid, oleylamine or a combination thereof. According to some embodiments of the present invention, a suitable solvent may be added in the preparation step S110, such as 1-octadecene, oleic acid, oleylamine, trioctylphosphine (TOP), trioctylphosphine oxide (TOPO) or a combination thereof, but is not limited thereto.

[0054] According to some embodiments of the present invention, the cesium precursor solution 10 is preheated. According to some embodiments of the present invention, the preheating temperature of the cesium precursor solution 10 may be about 80° C. to about 150° C., for example, about 80° C., about 90° C., about 100° C., about 110° C., about 120° C., about 130° C., about 140° C., or about 150° C.

[0055] Step S120: Providing a lead precursor solution 20

[0056] In step S120 of the present invention, a lead precursor solution is provided. In some embodiments of the present invention, step S120 includes mixing the lead-containing compound with the organic ligand, and the volume molar concentration of lead ions in the obtained lead precursor solution is about 1 to about 40 mM, for example, about 1 mM, about 2 mM, about 3 mM, about 4 mM, about 5 mM, about 5.5 mM, about 6 mM, about 7 mM, about 8 mM, about 9 mM, about 10 mM, about 11 mM, about 12 mM, about 13 mM, about 14 mM, about 15 mM, about 16 mM, about 17 mM, about 18 mM, about 19 mM, about 20 mM, about 25 mM, about 30 mM, about 35 mM, or about 40 mM, preferably about 5 mM to about 35 mM.

[0057] The lead-containing compound may be lead oleate, lead oleylamine, lead bromide (PbBr2), lead iodide (PbI2) or a combination thereof. The organic ligand may include oleic acid, oleylamine or a combination thereof. According to some embodiments of the present invention, a suitable solvent may be added in the preparation step S120, such as 1-octadecene, oleic acid, oleylamine, trioctylphosphine (TOP), trioctylphosphine oxide (TOPO) or a combination thereof, but the invention is not limited thereto.

[0058] According to some embodiments of the present invention, the preheating temperature of the lead precursor solution 20 is about 160° C. to about 220° C., for example, about 160° C., about 170° C., about 180° C., about 190° C., about 200° C., about 210° C. or about 220° C.; preferably, about 180° C. to about 200° C.

[0059] Step S130: Mix the cesium precursor solution 10 and the lead precursor solution 20

[0060] Step S130 of the present invention includes introducing the preheated cesium precursor solution 10 from the first flow channel P1 and the preheated lead precursor solution 20 from the second flow channel P2 into the micro mixer 30, so that they merge into the micro mixer 30 and then are transported to the reactor 40 of the next step. According to some embodiments of the present invention, the ratio of the flow rate of the cesium precursor solution 10 in the first flow channel P1 to the flow rate of the lead precursor solution 20 in the second flow channel P2 (Cs / Pb flow rate, in mol / s) is about 1 to about 0.2, for example, about 1, about 0.9, about 0.8, about 0.7, about 0.6, about 0.5, about 0.4, about 0.3, about 0.2.

[0061] Step S140: The cesium precursor solution 10 and the lead precursor solution 20 react

[0062] The step S140 of the present invention includes reacting the mixture of the cesium precursor solution 10 and the lead precursor solution 20 in a reactor 40 to obtain perovskite nanocrystals. According to some embodiments of the present invention, the reactor 40 can be immersed in a water bath or an oil bath in the third heating zone 42 for heating or heated by a heater (such as an electric heater, an infrared heater, etc.) (but not limited thereto), so that the reaction is carried out at a desired temperature. According to some embodiments of the present invention, the reaction temperature of step S140 is about 120°C to about 200°C, for example, about 120°C, about 130°C, about 140°C, about 150°C, about 160°C, 170°C, about 180°C or about 200°C; preferably about 150°C to about 180°C. The reactor 40 comprises a Teflon tube or a metal tube, preferably a metal tube.

[0063] Step S150: Collection and preservation of perovskite nanocrystals

[0064] The step S150 of the present invention includes collecting the perovskite nanocrystals obtained in step S140 with a collector 60, and performing steps such as centrifugation and purification on the perovskite nanocrystals. According to some embodiments of the present invention, step S150 further includes adding a solvent to preserve the perovskite nanocrystals, and the aforementioned solvents are, for example but not limited to, n-hexane, chloroform, toluene, and cyclohexane, which are commonly used solvents for preserving perovskite quantum dots.

[0065] The existing technology of synthesizing perovskite nanocrystals using a flow channel system mainly uses Teflon as the flow channel pipeline. Generally speaking, when trying to improve the quality of nanocrystal products, those with ordinary knowledge in the relevant technical field mainly start from adjusting the raw material composition, ratio or process parameters during the reaction (for example, reaction temperature, pressure, sequence of operation steps, etc.), but the inventors of this case unexpectedly found that by improving the pipeline material of the flow channel system (for example, reactor 40), the quantum efficiency of the obtained perovskite nanocrystal can be significantly improved to more than 80%, or even more than 90%. Without being bound by any particular theory, the inventors of this case believe that using metal pipes (such as stainless steel pipes) instead of Teflon pipes as pipelines of the flow channel system, especially reactor pipelines, helps to improve reaction efficiency and improve the quality of reaction products. This may be attributed to the fact that metals have higher thermal conductivity than Teflon, which helps to quickly transfer heat, more accurately control reaction temperature and promote mixing efficiency.

[0066] Generally speaking, operating at high temperature is conducive to promoting the formation of perovskite nanocrystals, and the flow channel system itself has a certain operating pressure to ensure that the reaction solution can flow stably. However, under high temperature and high pressure, the Teflon material may become soft and cause the flow channel system to be unusable, resulting in process interruption and the inability to stably mass-produce perovskite nanocrystals. In the present invention, the operating pressure of the flow channel system is generally controlled at about 1 to about 12 bar, the applicable temperature of the first heating zone 12 is about 80°C to about 150°C, and the material of the first flow channel P1 can be a Teflon tube or a metal tube. The inventor of the present case has found that it is particularly advantageous to use metal pipes in the flow channel system of the present invention (especially the related pipelines of the second heating zone 22 and the third heating zone 42 of step S120 and step S140). When the operating temperature exceeds 150°C and the operating pressure is 10 bar or higher, using metal pipes instead of Teflon pipes as the second flow channel P2 and the reactor 40 can not only promote the quantum efficiency of the obtained product to be increased to more than 80%, but also avoid the problem of Teflon material softening and causing process interruption when using high temperature and high pressure operating conditions. In addition, since the metal pipe has a higher thermal conductivity, it can achieve a good heat transfer effect, so that the solution in the metal pipe can maintain a good concentration uniformity and accurately control the reaction temperature, thereby further improving the process efficiency and product quality.

[0067] Therefore, according to some embodiments of the present invention, the pipeline of the reactor 40 is a metal pipe.

[0068] According to some embodiments of the present invention, the pipeline of the reactor 40 and the pipeline of step S120 (the second flow channel P2) are metal pipes.

[0069] According to some embodiments of the present invention, the pipeline of the reactor 40, the pipeline of step S120 (the second flow channel P2), the pipeline between the micro mixer 30 and the reactor 40 (i.e., the connecting pipe P3; see Figure 1 ) is a metal tube.

[0070] According to some embodiments of the present invention, the pipeline of the reactor 40, the pipeline of step S110 (first flow channel P1), the pipeline of step S120 (second flow channel P2), the pipeline between the micro mixer 30 and the reactor 40 (i.e., the connecting pipe P3; see Figure 1 ) is a metal tube.

[0071] According to some embodiments of the present invention, the pipeline of the reactor 40, the pipeline of step S120 (the second flow channel P2), the pipeline between the micro mixer 30 and the reactor 40 (i.e., the connecting pipe P3; see Figure 1 ) is a metal tube, and the pipeline (first flow channel P1) of step S110 is a Teflon tube.

[0072] According to some embodiments of the present invention, all pipelines in the flow channel system used in the present invention are metal pipes.

[0073] According to some embodiments of the present invention, except for the pipeline (first flow channel P1) in step S110, all pipelines in the flow channel system used in the present invention are metal pipes.

[0074] According to some embodiments of the present invention, the metal tubes in the flow channel system of the present invention may be the same or different, and the thermal conductivity of the metal is about 10W / m K or more, such as but not limited to: stainless steel, copper, aluminum or other metals or alloys. According to a preferred embodiment of the present invention, the metal tube is a stainless steel tube.

[0075] The Teflon tube in the flow channel system of the present invention can be a Teflon tube known to those skilled in the art. According to some embodiments of the present invention, the Teflon tube in the flow channel system of the present invention can be made of polytetrafluoroethylene (PTFE), fluorinated ethylene propylene copolymer (FEP), tetrafluoroethylene-perfluoroalkoxy vinyl ether copolymer (PFA) or the like.

[0076] According to some embodiments of the present invention, the portion of the first flow channel P1 passing through the first heating zone 12 may be a single annular pipeline or a pipeline consisting of multiple continuous annular pipelines (eg, Figure 1 In other embodiments of the present invention, the portion of the first flow channel P1 passing through the first heating zone 12 may be a single U-shaped pipeline or a pipeline consisting of a plurality of continuous U-shaped pipelines (such as a serpentine pipeline), but the shape of the portion of the first flow channel P1 passing through the first heating zone 12 is not limited to the above description.

[0077] According to some embodiments of the present invention, the portion of the second flow channel P2 passing through the second heating zone 22 may be a single annular pipeline or a pipeline consisting of multiple continuous annular pipelines (eg, Figure 1 In other embodiments of the present invention, the portion of the second flow channel P2 passing through the second heating zone 22 may be a single U-shaped pipeline or a pipeline consisting of a plurality of continuous U-shaped pipelines (such as a serpentine pipeline), but the shape of the portion of the second flow channel P2 passing through the second heating zone 22 is not limited to the above description.

[0078] According to some embodiments of the present invention, the portion of the reactor 40 passing through the third heating zone 42 may be a single annular pipeline or a pipeline consisting of multiple continuous annular pipelines (e.g., Figure 1 In other embodiments of the present invention, the portion of the reactor 40 passing through the third heating zone 42 may be a single U-shaped pipeline or a pipeline consisting of a plurality of continuous U-shaped pipelines (such as a serpentine pipeline), but the shape of the portion of the reactor 40 passing through the third heating zone 42 is not limited to the above description.

[0079] According to some embodiments of the present invention, the flow channel system of the present invention can be operated at an operating pressure of about 1 bar or above. According to a preferred embodiment of the present invention, the flow channel system of the present invention is driven by a motor, and there is a certain operating pressure to ensure that the solution in the pipeline can flow stably, and the pressure can be further increased to improve the smoothness of the pipeline. In the present invention, the operating pressure is between about 1.1 and about 12 bar, for example, a pressure of about 2 bar, about 3 bar, about 4 bar, about 5 bar, about 6 bar, about 7 bar, about 8 bar, about 9 bar, about 10 bar, about 11 bar or about 12 bar. Preferably, it is about 2 to about 10 bar (for example, a pressure of about 2 bar, about 4 bar, about 6 bar, about 8 bar or about 10 bar), preferably about 2 to about 6 bar.

[0080] The inventors of this case further discovered that although some Teflon tubes can withstand a heat temperature of up to about 200°C after being improved, when the Teflon tube is subjected to a reaction at a high temperature (e.g., over 150°C) and a high pressure (e.g., 2 bar or higher), the Teflon tube will become soft and cannot be used. Therefore, in the present invention, especially when operating at high temperature and high pressure, the use of metal tubes has process advantages compared to Teflon tubes. In addition, if the preheating temperature in step S110 is higher than 150°C, the cesium precursor may be decomposed prematurely, so step S110 is preferably performed at a temperature below 150°C, and a Teflon tube can be used in the first flow channel P1 of step S110 as needed. Compared to metal tubes, Teflon tubes are relatively cheap and have economic advantages. The inventors experimentally discovered that the use of Teflon tubes in this step has no adverse effect on the quantum efficiency of the product.

[0081] According to some embodiments of the present invention, in step S110, the cesium precursor solution 10 may be preheated in the first flow channel P1 to about 80° C. to about 150° C. at an operating pressure of about 1 bar or more, and the operating pressure is preferably about 2 to about 10 bar, and more preferably about 2 to about 6 bar.

[0082] According to some embodiments of the present invention, in step S120, the lead precursor solution 20 may be preheated to a temperature exceeding about 150° C. in the second flow channel P2 at an operating pressure of about 1 bar or more, the operating pressure is preferably about 2 to 10 bar, more preferably about 2 to about 6 bar, and the preheating temperature is preferably about 160° C. or more to about 220° C., more preferably about 180° C. to about 200° C. When the heating temperature of the lead precursor is less than 160° C., perovskite nanocrystals with a quantum efficiency of less than 80% will be obtained.

[0083] According to some embodiments of the present invention, in step S140, the mixture of the cesium precursor solution 10 and the lead precursor solution 20 is reacted in the reactor 40 at an operating pressure of about 1 to 12 bar, and the reaction temperature is about 120° C. to about 200° C.; the operating pressure is preferably about 2 to 10 bar, and the reaction temperature is preferably about 150° C. to about 180° C. The reaction synthesis residence time of the cesium precursor and the lead precursor in the reactor 40 is about 0.2 minutes to about 1 minute, but is not limited thereto.

[0084] The method for preparing perovskite nanocrystals of the present invention further comprises the step of performing solvent washing S160, which comprises inputting a solvent from a solvent storage tank 50 into a connecting pipe P3 connecting the micro mixer 30 and the reactor 40, allowing the solvent to flow into the reactor 40 to wash the reactor 40, so as to transport the perovskite nanocrystal product remaining in the reactor 40 to the collector 60 to improve the yield, wherein the solvent can be a solvent that does not react with the perovskite nanocrystals, such as but not limited to octadecene.

[0085] [Perovskite Nanocrystals]

[0086] According to some embodiments of the present invention, the molecular formula of the obtained perovskite nanocrystal is CsPb(Br x I 1–x )3, wherein 0≤x≤1. The perovskite nanocrystal size (particle diameter) of the present invention is between about 10 and about 300 nm, preferably between about 15 and about 200 nm, more preferably between about 20 and about 100 nm, about 20 and about 60 nm, or about 20 and about 40 nm.

[0087] According to some embodiments of the present invention, the perovskite nanocrystals of the present invention are red perovskite nanocrystals.

[0088] According to some embodiments of the present invention, the perovskite nanocrystals of the present invention have a light emission wavelength of about 630 to about 670 nm and a half-width of about 20 to about 40 nm under the excitation of a light source with a wavelength of about 200 to about 500 nm.

[0089] In the field of display applications, blue LED (wavelength of 450 to 495nm) or ultraviolet LED (wavelength of 200 to 400nm) is usually used as the excitation light source. In addition, according to the color gamut standard Rec.2020 (or BT.2020), the center of the blue light wavelength is 467nm; the center of the green light wavelength is 532nm; and the center of the red light wavelength is 630nm. Therefore, the perovskite nanocrystal of the present invention is suitable as the red light emitting material of the display; and the half-height width of the perovskite nanocrystal is narrower than that of the phosphor, which means that the color purity of the perovskite nanocrystal is higher, which can improve the color gamut width of the display.

[0090] According to some embodiments of the present invention, the perovskite nanocrystals of the present invention have a quantum efficiency of more than 80%, and more preferably have a quantum efficiency of more than 90%.

[0091] According to some embodiments of the present invention, the perovskite nanocrystals of the present invention have the following Figure 3 (a) shows an X-ray diffraction (XRD) pattern, which comprises characteristic peaks at the following 2θ reflection angles: 14.6°±0.3°, 20.8°±0.3°, 29.5°±0.3°, 36.2°±0.3° and 42.1°±0.3°.

[0092] The perovskite nanocrystals of the present invention have high quantum efficiency and can be applied to various technical fields, such as color conversion display technology, energy materials, intelligent sensing, biomedical imaging, etc. Taking color conversion display technology as an example, high quantum efficiency perovskite nanocrystals can improve various optical properties, such as color purity, brightness, etc., and thus can advantageously improve the performance and quality of products.

[0093] Examples

[0094] Test items and instruments

[0095] The structure of perovskite crystals: X-ray diffraction spectroscopy (XRD) was used, the model of which was D2 Phaser Diffractometer from Bruker.

[0096] The morphology of perovskite crystals was studied using a transmission electron microscope (TEM), model JEM-2100F from JEOL.

[0097] The spectral wavelength and optical rotation properties of perovskite crystals were measured using a photoluminescence spectroscopy (PL) instrument, model FLS1000 from Edinburgh.

[0098] Quantum efficiency: An absolute PL quantum yield spectrometer (model C11347 from Hamamatsu Photonics) was used.

[0099] Example 1

[0100] 1. Microfluidic system

[0101] The microfluidic system used in Example 1 of the present invention is as follows Figure 1 As shown, the prepared cesium precursor solution 10 enters the polytetrafluoroethylene tube P1 for preheating. The length of the polytetrafluoroethylene tube P1 is about 64 cm, the inner diameter of the tube is about 0.5 cm, and the inner diameter of the portion passing through the first heating zone 12 (which is a pipe that is locked in the polytetrafluoroethylene tube P1 body) is about 0.2 cm, and its volume is about 10 mL, wherein the first heating zone 12 is heated by a closed electric heating tube. The prepared lead precursor solution 20 enters the stainless steel tube P2 for preheating. The length of the stainless steel tube P2 is about 64 cm, the inner diameter of the tube is about 0.5 cm, and the inner diameter of the portion passing through the second heating zone 22 (which is a pipe that is locked in the stainless steel tube P2 body) is about 0.2 cm, and its volume is about 10 mL, wherein the second heating zone 22 is heated by a closed electric heating tube. The polytetrafluoroethylene tube P1 and the stainless steel tube P2 are respectively connected to the stainless steel micro mixer 30, and the micro mixer 30 is connected to the stainless steel reactor 40 through a connecting tube P3 with a total length of about 38 cm. The delivery tube P4 of the solvent storage tank 50 is connected to the connecting tube P3 at a connecting point C, wherein the length from the micro mixer 30 to the connecting point C is about 6 cm, and the length from the connecting point C to the reactor is about 32 cm. The inner diameters of the connecting tube P3 and the delivery tube P4 are both about 0.2 cm. The reactor 40 is a continuous annular pipeline with an inner diameter of about 0.2 cm and a volume of about 2 mL, wherein the third heating zone 42 is heated by a closed electric heating tube, and the reactor 40 has a delivery tube P5 (which is locked to the reactor 40 by sleeve connection) connected to a collector 60 for collecting perovskite nanocrystal samples, which is about 50 cm long and has an inner diameter of about 0.5 cm.

[0102] 2. Preparation method

[0103] The flow channel system is used to synthesize perovskite nanocrystals with high quantum efficiency. The detailed synthesis steps are as follows:

[0104] A. Preparation of cesium precursor solution: Weigh 110 mg of cesium carbonate (Cs2CO3), 3.8 mL of oleic acid and 25 mL of 1-octadecene into a three-necked flask and place a stirring magnet in it, then seal it with a serum stopper. Set the magnet stirring speed to 300 rpm for stirring, heat the mixed solution to 120°C and remove the water in the solution with a vacuum system for 1 hour. When cesium carbonate is completely dissolved in oleic acid and 1-octadecene and becomes a clear and transparent solution, the cesium precursor solution is obtained.

[0105] B. Preparation of lead precursor solution: Weigh 111 mg of lead bromide (PbBr2), 209.2 mg of lead iodide (PbI2), 20 mL of oleic acid, 40 mL of oleylamine and 35 mL of octadecene into a three-necked flask and put in a stirring magnet, and then seal it with a serum stopper. Set the magnet stirring speed to 300 rpm for stirring, heat the mixed solution to 120°C and remove the water in the solution with a vacuum system for 1 hour. When the lead bromide and lead iodide are completely dissolved in oleic acid, oleylamine and octadecene and a clear yellow solution is obtained, the lead precursor solution is obtained.

[0106] C.CsPb(Br 0.4 I 0.6 )3 Synthesis of red perovskite nanocrystals: The flow instrument is driven by a pressure of 2 to 6 bar (the operating pressure value may not be fixed to a specific value, but may be changed or adjusted according to the fluidity in the pipeline), and the cesium precursor solution obtained above is flowed through a polytetrafluoroethylene tube to be preheated to 150°C, and the lead precursor solution obtained above is flowed through a stainless steel tube to be preheated to 180°C. The preheated cesium precursor solution and the lead precursor solution are collected in a micro mixer, mixed, and fed into a reactor at a temperature of 180°C. After reacting for 50 minutes, CsPb(Br) is obtained. 0.4 I 0.6 )3 Red perovskite nanocrystals. After the crude product is collected, it is purified by centrifugation and dispersed in n-hexane solvent for storage.

[0107] 3. Test results

[0108] like Figure 3 As shown, the XRD standard spectrum of CsPbBr3 ( Figure 3 (b)) compared with the CsPb(Br 0.4 I 0.6 )3 Peak of red perovskite nanocrystals ( Figure 3 (a)) shifts to the left because the addition of iodine ions causes the characteristic peak to shift.

[0109] The obtained CsPb(Br 0.4 I 0.6 )3Perovskite nanocrystals were analyzed by transmission electron microscopy and their morphology was observed to be square (such as Figure 4 ), and the particle size is between about 20 and about 40 nm.

[0110] CsPb(Br 0.4 I 0.6 )3 Red perovskite nanocrystals were measured by photoluminescence spectrometer and absolute quantum efficiency meter. The results are as follows Figure 5 As shown. CsPb(Br 0.4 I 0.6 )3 The emission center of the perovskite nanocrystal is about 650nm, the half-width is about 30nm, the quantum efficiency is 91.5%, and the absorption spectrum can be observed in CsPbX3 PbX4 2- In detail, the absorption peak of the CsPbX3 structure generally has a higher absorption intensity as the wavelength becomes shorter. Figure 5 As shown, the absorption intensity increases from long wavelength to short wavelength, and the absorption intensity of CsPbX3 is PbX4 2- The absorption peak position moves depending on the halogen used. When X is I, PbI4 2- The corresponding absorption is about 430nm [6] With the doping of Br, the absorption peak will blue shift, and from the CsPb (Br 0.4 I 0.6 )3, the original upward trend is CsPb(Br 0.4 I 0.6 )3 inherent absorption, and a small flat area at about 410nm (such as Figure 5 The dotted circle area is Pb(Br,I)4 2- absorption signal.

[0111] Comparative Example 1

[0112] Comparative Example 1 uses the same flow channel system and synthesis steps as Example 1, except that all stainless steel tubes are replaced with polytetrafluoroethylene tubes. Although polytetrafluoroethylene that can withstand high temperatures above 200°C is used, due to the pressure of 2 to 6 bar in the pipeline, the polytetrafluoroethylene tube preheated in the heating zone softens, and thus the perovskite nanocrystals of the present invention cannot be successfully synthesized. If the pressure is reduced to avoid softening of the pipeline, the reaction solution flows too slowly in the pipeline, and the perovskite nanocrystals of the present invention cannot be successfully synthesized.

[0113] Comparative Example 2

[0114] Comparative Example 2 uses the same flow channel system and synthesis steps as Example 1, except that the preheating temperature of the lead precursor solution is set to 150° C., ie, less than 160° C., and the quantum efficiency of the obtained perovskite nanocrystals approaches 0%.

[0115] Comparative Example 3

[0116] Comparative Example 3 uses the same flow channel system and synthesis steps as Example 1, except that the stainless steel material of the reactor is replaced with polytetrafluoroethylene. However, due to the pressure of 2 to 6 bar in the pipeline, the polytetrafluoroethylene tube heated in the heating zone softens, and the perovskite nanocrystals of the present invention cannot be successfully synthesized. If the pressure is reduced to avoid softening of the pipeline, the reaction solution flows too slowly in the pipeline, and the perovskite nanocrystals of the present invention cannot be successfully synthesized.

[0117] Comparative Example 4

[0118] Comparative Example 4 uses the same flow channel system and synthesis steps as Example 1, except that the stainless steel tube used to transport the lead precursor solution is replaced with a polytetrafluoroethylene tube. However, due to the pressure of 2 to 6 bar in the pipeline, the polytetrafluoroethylene tube preheated in the heating zone softens, and the perovskite nanocrystals of the present invention cannot be successfully synthesized. If the pressure is reduced to avoid softening of the pipeline, the reaction solution flows too slowly in the pipeline, and the perovskite nanocrystals of the present invention cannot be successfully synthesized.

[0119] The materials and heating temperatures of each pipeline in the above-mentioned Example 1 and Comparative Examples 1 to 4 and the quantum efficiency of the obtained perovskite nanocrystals (if any) are shown in Table 1. From the results obtained in the examples of the present invention and the comparative examples, it can be understood that the present invention can obtain perovskite nanocrystals with a quantum efficiency greater than 90% by using a metal tube as a reactor for reacting a cesium precursor with a lead precursor and adjusting the preheating temperature of the lead precursor to be higher than the preheating temperature of the cesium precursor.

[0120] [Table 1]

[0121] Example 1 Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Cs precursor pipeline PTFE PTFE PTFE PTFE PTFE Pb precursor pipeline Stainless steel PTFE Stainless steel Stainless steel PTFE Reactor pipeline Stainless steel PTFE Stainless steel PTFE Stainless steel Cs precursor heating temperature 150℃ 150℃ 150℃ 150℃ 150℃ Pb precursor heating temperature 180℃ 180℃ 150℃ 180℃ 180℃ Reactor temperature 180℃ 180℃ 180℃ 180℃ 180℃ Quantum efficiency 91.5% N / A ≒0 N / A N / A

[0122] The above has been a fairly broad overview of the technical features and advantages of the present invention so that the present invention can be fully understood. Those skilled in the art will appreciate that various modifications and variations may be made to the present invention without departing from the scope or spirit of the present invention. In view of the foregoing, the present invention is intended to cover modifications and variations of the present invention, provided that they fall within the scope of the claims and their equivalents.

[0123] [References]

[0124] 1.Zhang,Y.;Saidaminov,M.I.;Dursun,I.;Yang,H.;Murali,B.;Alarousu,E.;Yengel,E.;Alshankiti,B.A.;Bakr,O.M.;Mohammed,O.F.,Zero-DimensionalCs4PbBr6Perovskite Nanocrystals.J.Phys.Chem.Lett.2017,8,961–965.

[0125] 2.Zhang,H.;Liao,Q.;Wu,Y.;Chen,J.;Gao,Q.;Fu,H.,Pure Zero-DimensionalCs4PbBr6 Single Crystal Rhombohedral Microdisks with High Luminescence and Stability.Phys.Chem.Chem.Phys.2017,19,29092–29098.

[0126] 3.Chen,Y.M.;Zhou,Y.;Zhao,Q.;Zhang,J.Y.;Ma,J.P.;Xuan,T.T.;Guo,S.Q.;Yong,Z.J.;Wang,J.;Kuroiwa,Y.;Moriyoshi,C.;Sun,H.T.,Cs4PbBr6 / CsPbBr3PerovskiteComposites with Near-Unity Luminescence Quantum Yield:Large-Scale Synthesis,Luminescence and Formation Mechanism,and White Light-Emitting DiodeApplication.ACS Appl.Mater.Interfaces 2018,10,15905–15912.

[0127] 4.Phillips,T.W.;Lignos,I.G.;Maceiczyk,R.M.;deMello,A.J.;deMello,J.C.,Nanocrystal synthesis in microfluidic reactors:where next?Lab Chip 2014,14,3172–3180.

[0128] 5. Lignos, I.; Stavrakis, S.; Nedelcu, G.; Protesescu, L.; deMello, AJ; Kovalenko, MVSynthesis of Cesium Lead Halide Perovskite Nanocrystals in a Droplet-Based Microfluidic Platform: Fast Parametric Space Mapping. NanoLett. 2016, 16, 1869–1877.

[0129] 6.Manser, JS; Saidaminov, MI; Christians, JA; Bakr, OM; Kamat, PVMaking and Breaking of Lead Halide Perovskites. Acc.Chem.Res.2016,49,330–338.

[0130] Explanation of symbols

[0131] 10: Cesium precursor solution

[0132] 12: First heating zone

[0133] 20: Lead precursor solution

[0134] 22: Second heating zone

[0135] 30: Micro mixer

[0136] 40: Reactor

[0137] 42: The third heating zone

[0138] 50:Solvent storage tank

[0139] 60: Collector

[0140] C: Connecting point

[0141] P1: First runner

[0142] P2: Second flow channel

[0143] P3: Connecting pipe

[0144] P4: Transport pipe

[0145] P5: Delivery pipe

[0146] S110: Providing cesium precursor solution

[0147] S120: Provide lead precursor solution

[0148] S130: Mixing cesium precursor solution and lead precursor solution

[0149] S140: Cesium precursor solution and lead precursor solution react

[0150] S150: Collection and preservation of perovskite nanocrystals

[0151] S160: Perform solvent flushing.

Claims

1. A method for preparing perovskite nanocrystals using a flow channel system, wherein include: Providing cesium precursor solution and lead precursor solution; Preheating the cesium precursor solution and the lead precursor solution respectively; and The preheated cesium precursor and the preheated lead precursor are then combined and transported to a reactor for reaction to obtain perovskite nanocrystals. wherein the reactor comprises a metal tube.

2. The method according to claim 1, wherein the preheating temperature of the cesium precursor is about 80°C to about 150°C, and the preheating temperature of the lead precursor is above 160°C to about 220°C. The method according to claim 1 , wherein the metal tube is made of stainless steel.

4. The method of claim 1, wherein the flow channel system is operated at a pressure of about 1 to about 12 bar.

5. The method according to claim 1, wherein the flow channel system include: A first flow channel for conveying the cesium precursor solution, wherein the first flow channel passes through a first heating zone and is used for preheating the cesium precursor solution; A second flow channel for conveying the lead precursor solution, the second flow channel passing through a second heating zone for preheating the lead precursor solution; a micro mixer connected to the first flow channel and the second flow channel; and The reactor is connected to the micromixer. 6 . The method according to claim 5 , wherein the first flow channel and the second flow channel are each independently a Teflon tube or a metal tube. 7 . The method according to claim 6 , wherein the first flow channel is a Teflon tube, and the second flow channel is a stainless steel tube.

8. The method according to claim 1, wherein the cesium precursor solution comprises a cesium-containing compound, and the cesium ion volume molar concentration thereof is about 1 mM to about 40 mM, and the lead precursor solution comprises a lead-containing compound, and the lead ion volume molar concentration thereof is about 1 mM to about 40 mM, wherein the cesium-containing compound comprises cesium oleate, cesium fluoride (CsF), cesium chloride (CsCl), cesium bromide (CsBr), cesium iodide (CsI), cesium carbonate (Cs 2 CO 3 ) or a combination thereof, wherein the lead-containing compound comprises lead oleate, lead oleylamine, lead bromide (PbBr 2 ), lead iodide (PbI 2 ) or a combination thereof.

9. The method of claim 1, wherein the cesium precursor solution or the lead precursor solution further comprises an organic ligand, and the organic ligand comprises oleic acid, oleylamine, or a combination thereof.

10. The method of claim 1, wherein a ratio of flow rates of the cesium precursor solution and the lead precursor solution (Cs / Pb flow rate) is about 1 to about 0.

2.

11. A perovskite nanocrystal prepared by the method of any one of claims 1 to 10, and having a quantum efficiency of at least about 80%.

12. The perovskite nanocrystal of claim 11, wherein the perovskite nanocrystal has one or more of the following properties: (1) a crystal size of about 10 to about 300 nm, (2) It has an emission wavelength of about 630 to about 670 nm and a half-width of about 20 to about 40 nm when excited by a light source with a wavelength of about 200 to about 500 nm.