Ultralow-gram-weight regenerated white-flour craft paper and preparation method thereof

By using 100% office composite waste paper and optimization process, recycled white-faced beef jam paper with low gram weight and strong performance was prepared, which solved the damage problem of existing white-faced beef jam paper in ceramic and tile packaging, and reduced production costs and Item damage rate improves product quality and customer satisfaction.

CN119041241APending Publication Date: 2024-11-29DONGGUAN NINE DRAGONS PAPER IND
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411285215.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-13
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The existing white-faced beef jam paper in ceramic and ceramic tile packaging is easy to slide and collide due to its high tightness, high smoothness and low friction, resulting in damage to the items. The raw materials and chemical auxiliary materials are consumed high during the pulping process, which is expensive.

Method used

Using 100% office composite waste paper as the surface slurry, combined with calcium carbonate and alkylkone dimers and other glue sizing agents, the pulping, flow and glue sizing process is optimized to prepare low-grain weight and high-quality Recycled white-faced beef jam paper.

Benefits of technology

It realizes recycled white-faced beef jam paper with low gram weight, strong performance and good moisture resistance, reduces production costs, meets the requirements of ceramic and ceramic tile packaging and interlayer bonding, reduces item damage, and improves customer satisfaction .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005042935730000211
    Figure BDA0005042935730000211
  • Figure BDA0005042935730000221
    Figure BDA0005042935730000221
Patent Text Reader

Abstract

The invention provides ultralow-gram-weight regenerated white craft paper and a preparation method thereof, the gram weight of the regenerated white craft paper is 100-120g / m < 2 >, and the regenerated white craft paper comprises a surface layer and a bottom layer. The preparation method comprises the following steps: carrying out deslagging treatment on surface layer regenerated pulp, and then mixing with calcium carbonate to obtain surface pulp; carrying out deslagging treatment on the bottom-layer regenerated pulp, and then mixing with a dry strength agent to obtain bottom pulp; mixing the surface pulp and the bottom pulp with a sizing agent, flowing to a pressurized screen, spraying to a net through a flowing pulp flowing box, dehydrating, carrying out vacuum suction compounding on a surface layer wet paper web and a bottom layer wet paper web, and sequentially carrying out mechanical dehydration, drying treatment, calendaring, rewinding and film coating, so as to obtain finished paper. According to the invention, 100% of office composite waste paper is used as surface layer pulp, 100% of national waste OCC is used as bottom layer pulp, and optimization of methods of paper pulp, drifting, sizing and the like is combined, so that the regenerated white-surface craft paper which is low in production energy consumption, low in gram weight, high in quality and strong in performance is obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of papermaking, and relates to a white-faced kraft paper, and in particular to an ultra-low gram-weight recycled white-faced kraft paper and a preparation method thereof. Background Art

[0002] Ordinary white-faced kraft paper has good printing performance and the unique high-strength performance of natural-color kraft paper. It is widely used in beverages, mineral water, and beer boxes. However, when used as packaging paper for ceramics and tiles, the disadvantages of ordinary white-faced kraft paper are exposed. Ordinary white-faced kraft paper has high density and high smoothness. During transportation and handling, it has low friction and is easy to slide and collide, causing damage to ceramics or tiles and affecting quality. In response to different market demands, it is of great significance to develop low-weight and high-bulk white-faced kraft paper. White-faced kraft paper with low gram weight and high bulk has a larger surface area at the same weight, can pack more items, and has high friction when items touch each other, and has a good buffering effect, which can keep the items intact to the maximum extent, reduce damage to items, reduce the claim rate, and improve customer satisfaction.

[0003] The common white-faced kraft paper currently available on the market is generally composed of three layers: the surface layer, the core layer and the bottom layer. The paper weight is generally controlled at 180g / m 2 The above mentioned materials consume a lot of materials. In addition, the manufacturing process of traditional white-faced kraft paper requires a high whiteness of the surface layer and the core layer pulp to meet the whiteness requirements of the finished paper. Generally, the surface layer is greater than 85 degrees. Therefore, under this whiteness requirement, the surface layer needs to be mixed with more than 50% bleached wood pulp to meet the whiteness and uniformity requirements of the finished paper. It is impossible to use 100% office composite waste paper as the surface layer pulp. The consumption of raw materials and chemical auxiliary materials in pulping production is high. In order to ensure the water-resistant effect of the finished paper, the traditional sizing process requires expensive surface sizing agents such as AKD, styrene acrylic acid (SAE), polyacrylamide (PAM), polyvinyl alcohol (PVA), etc., and a small amount of filler needs to be added to the surface layer, resulting in high sizing costs. However, the white-faced kraft paper used for packaging ceramics and tiles does not require a very high whiteness of the surface layer, and the water-resistant effect only needs to meet the requirement of 180S non-penetration, but it has higher requirements for tear resistance and interlayer bonding.

[0004] In order to improve the market competitiveness of the paper industry, continuously promote the high-end, intelligent and green development of the papermaking industry, deepen market development, achieve stable growth and improve efficiency in the industry, and promote the high-quality development of paper and paper products, it is imperative to develop paper that can meet market demand. Summary of the invention

[0005] The purpose of the present invention is to provide an ultra-low gram-weight recycled white-faced kraft paper and a preparation method thereof. The present invention uses 100% office composite waste paper as the surface layer pulp, and combines the optimization of pulping, flow conveying, sizing and other methods to obtain a recycled white-faced kraft paper with low production energy consumption, low gram-weight, high quality and strong performance.

[0006] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:

[0007] In a first aspect, the present invention provides an ultra-low grammage recycled white-faced kraft paper, wherein the recycled white-faced kraft paper comprises a surface layer and a bottom layer;

[0008] The gram weight of the recycled white kraft paper is 100-120 g / m 2 , for example, it can be 100g / m 2 , 104g / m 2 , 108g / m 2 , 112g / m 2 , 116g / m 2 or 120g / m 2 , but not limited to the listed values, other values ​​not listed within the numerical range are also applicable.

[0009] As a preferred technical solution of the present invention, the weight of the surface layer is 30 to 40 g / m 2 , for example, it can be 30g / m 2 , 32g / m 2 , 34g / m 2 , 36g / m 2 , 38g / m 2 or 40g / m 2 , but not limited to the listed values, other values ​​not listed within the numerical range are also applicable.

[0010] Preferably, the raw material for preparing the surface layer includes domestic composite office waste paper.

[0011] It is worth noting that the domestic composite office waste paper described in the present invention includes domestic large-flowered office waste paper and domestic small-flowered office waste paper in a mass ratio of 1:1.

[0012] Preferably, the weight of the bottom layer is 60 to 90 g / m 2 , for example, it can be 60g / m 2 , 63g / m 2 , 66g / m 2 , 69g / m 2 , 72g / m 2 , 75g / m 2 , 7g / m 2 , 81g / m 2 , 84g / m2 , 87g / m 2 or 90g / m 2 , but not limited to the listed values, other values ​​not listed within the numerical range are also applicable.

[0013] Preferably, the raw materials for preparing the bottom layer include the following components in mass fractions: 10-30wt% of Class C domestic waste OCC and 70-90wt% of Class D domestic waste OCC.

[0014] Exemplarily, the content of the Class C domestic waste OCC is 10-30wt%, for example, it can be 10wt%, 14wt%, 18wt%, 22wt%, 26wt% or 30wt%, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0015] The content of the grade D domestic waste OCC is 70-90wt%, for example, it can be 70wt%, 74wt%, 78wt%, 82wt%, 86wt% or 90wt%, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0016] In the present invention, domestic office waste paper and corrugated box waste paper are used as raw materials to prepare ultra-low grammage recycled white kraft paper, which not only realizes the resource processing of waste paper, but also achieves stable growth and efficiency improvement of the papermaking industry, and promotes the high-quality development of paper and paper products.

[0017] In a second aspect, the present invention provides a method for preparing the ultra-low grammage recycled white kraft paper provided in the first aspect, the preparation method comprising the following steps:

[0018] (1) removing slag from the surface layer regenerated pulp and mixing it with calcium carbonate to obtain a dough;

[0019] (2) removing slag from the bottom recycled pulp and mixing with a dry strength agent to obtain a bottom pulp;

[0020] (3) After the surface stock and the bottom stock are mixed with sizing agents, they are respectively flowed to a pressure screen and then sprayed onto the screen through a flow headbox to obtain a surface wet paper web and a bottom wet paper web;

[0021] (4) dehydrating the surface wet paper web and the bottom wet paper web obtained in step (3) respectively, and then vacuum-suction-compounding the surface wet paper web and the bottom wet paper web to obtain an original paperboard;

[0022] (5) subjecting the raw paperboard obtained in step (4) to one shoe press, two shoe presses, three light presses, drying, calendering, rewinding and film coating in sequence to obtain finished paper;

[0023] There is no order distinction between steps (1) and (2).

[0024] In the present invention, by optimizing the pulping, flow conveying, sizing and other systems, the purpose of preparing the recycled white kraft paper with low gram weight, high quality and strong performance with lower energy consumption is achieved.

[0025] As a preferred technical solution of the present invention, the method for preparing the surface layer recycled pulp in step (1) comprises: transporting domestic composite office waste paper to a drum pulper through a chain conveyor to mix with sodium silicate and then subjecting it to pulping treatment, and then sequentially subjecting it to sand removal treatment, flotation deinking treatment, oxidative bleaching treatment and pulping to obtain the surface layer recycled pulp.

[0026] More specifically, the preparation method of the surface layer recycled pulp of the present invention comprises: transporting domestic composite office waste paper to a drum pulper through a chain conveyor to mix with sodium silicate and then subjecting the paper to pulping treatment, and then sequentially passing through a high-concentration desander, a coarse screen, a medium-concentration pre-fine screen, a primary flotation tank, a low-concentration positive desander, a low-concentration post-fine screen, a 1# thermal dispersion, a secondary flotation tank, concentration, a 2# thermal dispersion, a tertiary flotation tank, concentration, bleaching and a grinding disc pulping to achieve desanding treatment, flotation deinking treatment and oxidation bleaching treatment;

[0027] The present invention adopts high-concentration sand removal and low-concentration sand removal to remove heavy impurities; coarse screening, medium-concentration screening and low-concentration screening to remove large impurities; three-stage low-concentration flotation to remove ink and fine impurities in the slurry; combined with oxidation and reduction two-stage TCF bleaching to increase the whiteness of the slurry by 15-20ISO, the dust removal rate is more than 98%, and the ink removal rate is more than 90%.

[0028] As a preferred technical solution of the present invention, the pulping concentration of the pulping treatment is 15-22%, for example, it can be 15%, 16%, 17%, 18%, 19%, 20%, 21% or 22%, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0029] Preferably, the pulping treatment temperature is 50-60°C, for example, 50°C, 52°C, 54°C, 56°C, 58°C or 60°C, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0030] Preferably, the pH value of the pulping treatment is 7.0-8.0, for example, 7.0, 7.1, 7.2, 7.3, 7.4, 7.5, 7.6, 7.7, 7.8, 7.9 or 8.0, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0031] Preferably, the addition amount of sodium silicate is 3-6 kg / t slurry, for example, it can be 3 kg / t slurry, 3.3 kg / t slurry, 3.6 kg / t slurry, 3.9 kg / t slurry, 4.2 kg / t slurry, 4.5 kg / t slurry, 4.8 kg / t slurry, 5.1 kg / t slurry, 5.4 kg / t slurry, 5.7 kg / t slurry or 6 kg / t slurry, but is not limited to the listed values, and other values ​​not listed within the numerical range are equally applicable.

[0032] In the present invention, the sodium silicate is a permeable buffer and dispersant, which has a wetting and dispersing effect in the deinking of dough preparation, can saponify oil substances, disperse pigments, and protect the pulp from absorbing stains, and at the same time helps to stabilize hydrogen peroxide, so as to facilitate the performance of hydrogen peroxide.

[0033] In addition, the pulping process in the preparation process of the surface layer recycled pulp of the present invention is carried out in a drum pulper, which relies on the rotation of the drum to raise the height of the waste paper, and relies on the gravity of the waste paper itself to continuously perform periodic raising-falling beating to break the waste paper into pulp; the present invention reduces the cutting of fibers through gentle pulping, maintains the integrity of debris in the waste paper, can remove more impurities in the screening area of ​​the pulper, reduces the wear of subsequent equipment, and reduces the replacement cycle of equipment, thereby achieving the effect of energy saving and consumption reduction.

[0034] Preferably, the flotation deinking treatment includes primary flotation deinking, secondary flotation deinking and tertiary flotation deinking performed in sequence.

[0035] Preferably, the HLB value of the deinking agent used in the flotation deinking treatment is 11-12, for example, 11, 11.2, 11.4, 11.6, 11.8 or 12, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0036] Preferably, the usage amount of the deinking agent in the primary flotation deinking is 0.3-0.5 kg / t pulp, for example, it can be 0.3 kg / t pulp, 0.34 kg / t pulp, 0.38 kg / t pulp, 0.42 kg / t pulp, 0.46 kg / t pulp or 0.5 kg / t pulp, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0037] Preferably, the usage amount of the deinking agent in the secondary flotation deinking is 0.1-0.2 kg / t pulp, for example, 0.1 kg / t pulp, 0.12 kg / t pulp, 0.14 kg / t pulp, 0.16 kg / t pulp, 0.18 kg / t pulp or 0.2 kg / t pulp can be ignored, but it is not limited to the listed values, and other values ​​within the numerical range are not listed.

[0038] Preferably, the usage amount of the deinking agent in the tertiary flotation deinking is 0 kg / t pulp.

[0039] In the present invention, the first-stage flotation deinking adopts Mac-cell vertical flotation cell, which has high operation stability, simple control parameters, large demand for flotation foam, and low sensitivity to the amount and concentration of incoming slurry foam; the second-stage flotation deinking and the third-stage flotation deinking adopt Eco-cell flotation cell, which has high flotation efficiency, moderate yield, and more interlocking control parameters; a Venturi foam generator is used, which is highly sensitive to the amount and concentration of incoming slurry foam;

[0040] In addition, the deinking agent used in the flotation deinking treatment of the present invention is a surface active deinking agent with rich foaming capacity and good ink removal effect; the deinking agent has rich foaming capacity and the ink removal rate of three-stage flotation can reach more than 80%.

[0041] Preferably, the oxidative bleaching treatment comprises an oxidative bleaching stage and a reductive bleaching stage performed sequentially.

[0042] Preferably, the oxidizing agent used in the oxidative bleaching stage comprises hydrogen peroxide.

[0043] Preferably, the reducing agent used in the reduction bleaching stage comprises sodium borohydride and sodium bisulfite.

[0044] In the oxidation bleaching treatment of the present invention, hydrogen peroxide is mainly used as an oxidation bleaching agent in the oxidation bleaching stage. The HO 2- It reacts with the double bonds in the pigment to achieve the effect of decolorization. In the reduction bleaching section, sodium borohydride and sodium bisulfite are used to generate sodium dithionite with high reducing properties online, thereby destroying the carbonyl groups in the pigment molecules to achieve the bleaching effect. Through redox bleaching, the whiteness of the pulp can be increased by more than 15ISO.

[0045] As a preferred technical solution of the present invention, the whiteness of the surface layer recycled pulp in step (1) is 80 to 85 degrees, for example, it can be 80 degrees, 81 degrees, 82 degrees, 83 degrees, 84 degrees or 85 degrees, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0046] Preferably, the A of the surface layer regenerated pulp in step (1) is -1 to 1, for example, it can be -1, -0.6, -0.3, 0, 0.4, 0.7 or 1, but not limited to the listed values, and other values ​​within the numerical range not listed; B is -2 to 6, for example, it can be -2, -1, 0, 1, 2, 3, 4, 5 or 6, but not limited to the listed values, and other values ​​within the numerical range not listed.

[0047] In the present invention, A represents red and green, and B represents yellow and blue.

[0048] Preferably, the dust content in the surface regenerated slurry in step (1) is less than 60 mg / cm 3 , for example, it can be 58 mg / cm 3 、56mg / cm 3 、54mg / cm 3 , 52mg / cm 3 、50mg / cm 3 or 45 mg / cm 3 The above values ​​are not limited to the above listed values, and other values ​​not listed in the above listed values ​​are also applicable.

[0049] Preferably, the residual ink content (ERIC) in the surface layer regenerated pulp in step (1) is less than 30, for example, it can be 28, 26, 24, 22, 20 or 15, but is not limited to the listed values, and other values ​​within the numerical range not listed.

[0050] As a preferred technical solution of the present invention, the method for preparing the bottom layer regenerated pulp in step (2) includes: transporting Class C domestic waste OCC and Class D domestic waste OCC to a hydraulic pulper through a chain conveyor for pulping treatment, and then sequentially performing slag removal treatment, coarse screening treatment, fine screening treatment, concentration treatment and thermal dispersion treatment to obtain the bottom layer regenerated pulp.

[0051] In the present invention, the slag removal treatment in the preparation method of the bottom recycled pulp adopts a high-concentration slag remover. The present invention optimizes the low-concentration slag removal process, increases the ash content of the base paper, and saves energy consumption. In addition, the present invention uses a combination of Class C domestic waste OCC and Class D domestic waste OCC as raw materials. The fiber length in the waste paper is relatively short, and the bottom recycled pulp can be obtained without using disc grinding and pulping.

[0052] As a preferred technical solution of the present invention, the concentration of calcium carbonate in step (1) is 10-12wt%, for example, it can be 10wt%, 10.4wt%, 10.8wt%, 11.2wt%, 11.6wt% or 12wt%, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0053] Preferably, the amount of calcium carbonate added in step (1) is 35-50 kg / t paper, for example, 35 kg / t paper, 38 kg / t paper, 41 kg / t paper, 44 kg / t paper, 47 kg / t paper or 50 kg / t paper, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0054] In the present invention, by mixing calcium carbonate with a particle size of 63 to 68 into the surface layer recycled pulp, the surface uniformity and whiteness of the surface layer can be improved, and the paper smoothness can reach more than 10S.

[0055] Preferably, the solid content of the dry strength agent in step (2) is 15-25wt%, for example, 15wt%, 17wt%, 19wt%, 21wt%, 23wt% or 25wt%, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0056] Preferably, the amount of the dry strength agent added in step (2) is 5 to 15 kg / t of paper, for example, 5 kg / t of paper, 7 kg / t of paper, 9 kg / t of paper, 11 kg / t of paper, 13 kg / t of paper or 15 kg / t of paper, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0057] Preferably, the dry strength agent in step (2) includes polyacrylamide or modified starch.

[0058] In the present invention, by mixing the dry strength agent into the bottom recycled pulp, the hydroxyl groups in the dry strength agent molecules form hydrogen bonds with the hydroxyl groups on the surface of cellulose, thereby increasing the binding force between fibers and giving the paper better physical properties.

[0059] As a preferred technical solution of the present invention, the sizing agent in step (3) comprises an alkyl ketene dimer.

[0060] Preferably, the concentration of the alkyl ketene dimer is 12 to 15 wt%, for example, it can be 12 wt%, 12.3 wt%, 12.6 wt%, 12.9 wt%, 13.2 wt%, 13.5 wt%, 13.8 wt%, 14.1 wt%, 14.4 wt%, 14.7 wt% or 15 wt%, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0061] Preferably, the addition amount of the alkyl ketene dimer is 15-25 kg / t paper, for example, 15 kg / t paper, 17 kg / t paper, 19 kg / t paper, 21 kg / t paper, 23 kg / t paper or 25 kg / t paper, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0062] The present invention adopts the method of in-slurry sizing, and mixes the sizing agent before the surface slurry and the bottom slurry are sent to the pressure screen, so that the water absorption value of the front side (surface layer) of the finished paper is less than 40, and the water absorption value of the back side (bottom layer) is less than 50. The paper sheet has both good moisture resistance and good bulk and bending properties.

[0063] As a preferred technical solution of the present invention, the dryness of the base paperboard in step (4) is 18-22%, for example, 18%, 19%, 20%, 21% or 22%, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0064] Preferably, the pressure of the shoe press in step (5) is 700-800 KN, for example, it can be 700 KN, 720 KN, 740 KN, 760 KN, 780 KN or 800 KN, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0065] Preferably, the pressure of the second shoe press in step (5) is 1000-1100 KN, for example, it can be 1000 KN, 1020 KN, 1040 KN, 1060 KN, 1080 KN or 1100 KN, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0066] Preferably, the pressure of the three light presses in step (5) is 40-50 KN, for example, 40 KN, 42 KN, 44 KN, 46 KN, 48 KN or 50 KN, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0067] Preferably, the device used for the drying process in step (5) comprises a drying cylinder drying device.

[0068] Preferably, the outlet temperature of the drying cylinder is ≥100°C, for example, it can be 100°C, 102°C, 104°C, 106°C, 108°C or 110°C, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0069] In the present invention, the number of drying cylinders in the drying cylinder drying device is 6 groups, and the outlet temperature of the drying cylinders is ≥100°C, so that the paper web temperature reaches above 90°C to ensure the ripening effect of alkyl ketene dimer (AKD).

[0070] As a preferred technical solution of the present invention, the second aspect of the present invention provides a method for preparing the ultra-low grammage recycled white kraft paper as described in the first aspect, comprising the following steps:

[0071] (1) removing slag from the surface layer regenerated pulp and mixing it with calcium carbonate to obtain a dough;

[0072] The preparation method of the surface layer recycled pulp comprises: transporting domestic composite office waste paper to a drum pulper through a chain conveyor and mixing with sodium silicate for pulping treatment, and then sequentially performing sand removal treatment, flotation deinking treatment, oxidation bleaching treatment and beating to obtain the surface layer recycled pulp; the pulping concentration of the pulping treatment is 15-22%, the temperature is 50-60°C, and the pH value is 7.0-8.0; the amount of sodium silicate added is 3-6kg / t pulp; the flotation deinking treatment comprises primary flotation deinking, secondary flotation deinking and tertiary flotation deinking performed sequentially; the HLB value of the deinking agent used in the flotation deinking treatment is 11-12; the amount of the deinking agent used in the primary flotation deinking is 0.3-0.5kg / t pulp, and the amount of the deinking agent used in the secondary flotation deinking is 0.1-0.2kg / t pulp;

[0073] The whiteness of the surface layer recycled pulp is 80-85 degrees, A=-1-1, B=-2-6, and the dust content is less than 60 mg / cm 3 , ink residue is less than 30mg / cm 3 ;

[0074] The concentration of calcium carbonate is 10-12 wt %, and the amount of calcium carbonate added is 35-50 kg / t paper;

[0075] (2) removing slag from the bottom recycled pulp and mixing with a dry strength agent to obtain a bottom pulp;

[0076] The preparation method of the bottom recycled pulp comprises: transporting the Class C domestic waste OCC and the Class D domestic waste OCC to a hydraulic pulper through a chain conveyor for pulping, and then sequentially performing a slag removal treatment, a coarse screening treatment, a fine screening treatment, a concentration treatment and a thermal dispersion treatment to obtain the bottom recycled pulp;

[0077] The solid content of the dry strength agent is 15-25wt%, and the addition amount of the dry strength agent is 5-15kg / t paper;

[0078] (3) After the alkyl ketene dimer is mixed with the top stock and the bottom stock, the top stock and the bottom stock are respectively flowed to a pressure screen and then sprayed onto the screen through a flow headbox to obtain a top layer wet paper web and a bottom layer wet paper web;

[0079] Wherein, the concentration of the alkyl ketene dimer is 12-15 wt %, and the addition amount of the alkyl ketene dimer is 15-25 kg / t paper;

[0080] (4) dehydrating the surface wet paper web and the bottom wet paper web obtained in step (3) respectively, and then vacuum-suction-compounding the surface wet paper web and the bottom wet paper web to obtain an original paperboard;

[0081] (5) subjecting the raw paperboard obtained in step (4) to one shoe press, two shoe presses, three light presses, drying, calendering, rewinding and film coating in sequence to obtain finished paper;

[0082] The pressure of the first shoe press is 700-800KN, the pressure of the second shoe press is 1000-1100KN, and the pressure of the third light press is 40-50KN; the drying device includes a drying cylinder drying device; the outlet temperature of the drying cylinder drying device is ≥100℃;

[0083] There is no order distinction between steps (1) and (2).

[0084] Compared with the prior art, the present invention has the following beneficial effects:

[0085] (1) The present invention innovates the papermaking process, so that the surface layer recycled pulp uses 100% office composite waste paper, and the bottom layer recycled pulp uses 100% OCC domestic waste paper, which can still meet the requirements of white-faced kraft paper for packaging ceramics and tiles for tear resistance, folding resistance and interlayer bonding strength, greatly reducing the production cost of a ton of paper;

[0086] (2) The recycled white-faced kraft paper obtained by the preparation method provided by the present invention has an ultra-low grammage; the in-slurry sizing method is adopted, so that the recycled white-faced kraft paper has good moisture resistance, good bulk and bending properties. DETAILED DESCRIPTION

[0087] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0088] Example 1

[0089] This embodiment provides an ultra-low gram-weight recycled white-faced kraft paper, wherein the recycled white-faced kraft paper comprises a surface layer and a bottom layer; the gram-weight of the recycled white-faced kraft paper is 100 g / m 2 .

[0090] The surface layer has a grammage of 35 g / m 2 ; The raw materials for preparing the surface layer include domestic composite office waste paper;

[0091] The base layer has a grammage of 65 g / m 2 The raw materials for preparing the bottom layer include the following components in mass fraction: 20wt% of Class C domestic waste OCC and 80wt% of Class D domestic waste OCC.

[0092] The preparation method of the ultra-low gram-weight recycled white kraft paper comprises the following steps:

[0093] (1) removing slag from the surface layer regenerated pulp and mixing it with calcium carbonate to obtain a dough;

[0094] The preparation method of the surface layer recycled pulp comprises: transporting domestic composite office waste paper to a drum pulper through a chain conveyor and mixing with sodium silicate, then performing pulping treatment, and then sequentially performing sand removal treatment, flotation deinking treatment, oxidation bleaching treatment and beating to obtain the surface layer recycled pulp; the pulping concentration of the pulping treatment is 18%, the temperature is 55°C, and the pH value is 7.5; the amount of sodium silicate added is 4.5kg / t pulp; the flotation deinking treatment includes primary flotation deinking, secondary flotation deinking and tertiary flotation deinking performed sequentially; the HLB value of the deinking agent used in the flotation deinking treatment is 11.5; the amount of the deinking agent used in the primary flotation deinking is 0.4kg / t pulp, and the amount of the deinking agent used in the secondary flotation deinking is 0.15kg / t pulp;

[0095] The whiteness of the surface layer recycled pulp is 82 degrees, A=0, B=1, and the dust content is less than 60 mg / cm 3 , ink residue <30;

[0096] The concentration of calcium carbonate is 11wt%, and the amount of calcium carbonate added is 42kg / t paper;

[0097] (2) removing slag from the bottom recycled pulp and mixing with a dry strength agent to obtain a bottom pulp;

[0098] The preparation method of the bottom recycled pulp comprises: transporting the Class C domestic waste OCC and the Class D domestic waste OCC to a hydraulic pulper through a chain conveyor for pulping, and then sequentially performing a slag removal treatment, a coarse screening treatment, a fine screening treatment, a concentration treatment and a thermal dispersion treatment to obtain the bottom recycled pulp;

[0099] The solid content of the dry strength agent is 20wt%, and the addition amount of the dry strength agent is 10kg / t paper;

[0100] (3) After the alkyl ketene dimer is mixed with the top stock and the bottom stock, the top stock and the bottom stock are respectively flowed to a pressure screen and then sprayed onto the screen through a flow headbox to obtain a top layer wet paper web and a bottom layer wet paper web;

[0101] Wherein, the concentration of the alkyl ketene dimer is 13.5wt%, and the addition amount of the alkyl ketene dimer is 20kg / t paper;

[0102] (4) dehydrating the surface wet paper web and the bottom wet paper web obtained in step (3) respectively, and then vacuum-suction-compounding the surface wet paper web and the bottom wet paper web to obtain an original paperboard;

[0103] (5) subjecting the raw paperboard obtained in step (4) to one shoe press, two shoe presses, three light presses, drying, calendering, rewinding and film coating in sequence to obtain finished paper;

[0104] The pressure of the first shoe press is 750KN, the pressure of the second shoe press is 1050KN, and the pressure of the third light press is 45KN; the drying device includes a drying cylinder drying device; the outlet temperature of the drying cylinder drying device is ≥100℃;

[0105] There is no order distinction between steps (1) and (2).

[0106] Example 2

[0107] This embodiment provides an ultra-low gram-weight recycled white-faced kraft paper, wherein the recycled white-faced kraft paper comprises a surface layer and a bottom layer; the gram-weight of the recycled white-faced kraft paper is 110 g / m 2 .

[0108] The surface layer has a grammage of 36 g / m 2 ; The raw materials for preparing the surface layer include domestic composite office waste paper;

[0109] The base layer has a grammage of 74 g / m 2 The raw materials for preparing the bottom layer include the following components in mass fraction: 10wt% of Class C domestic waste OCC and 90wt% of Class D domestic waste OCC.

[0110] The preparation method of the ultra-low gram-weight recycled white kraft paper comprises the following steps:

[0111] (1) removing slag from the surface layer regenerated pulp and mixing it with calcium carbonate to obtain a dough;

[0112] The preparation method of the surface layer recycled pulp comprises: transporting domestic composite office waste paper to a drum pulper through a chain conveyor and mixing with sodium silicate, then performing pulping treatment, and then sequentially performing sand removal treatment, flotation deinking treatment, oxidation bleaching treatment and beating to obtain the surface layer recycled pulp; the pulping concentration of the pulping treatment is 15%, the temperature is 50°C, and the pH value is 7.0; the amount of sodium silicate added is 3kg / t pulp; the flotation deinking treatment includes sequentially performing primary flotation deinking, secondary flotation deinking and tertiary flotation deinking; the HLB value of the deinking agent used in the flotation deinking treatment is 11; the amount of the deinking agent used in the primary flotation deinking is 0.3kg / t pulp, and the amount of the deinking agent used in the secondary flotation deinking is 0.2kg / t pulp;

[0113] The whiteness of the surface layer recycled pulp is 80 degrees, A=-1, B=-2, and the dust content is less than 60 mg / cm 3 , the ink residue is less than 30;

[0114] The concentration of calcium carbonate is 10wt%, and the amount of calcium carbonate added is 50kg / t paper;

[0115] (2) removing slag from the bottom recycled pulp and mixing with a dry strength agent to obtain a bottom pulp;

[0116] The preparation method of the bottom recycled pulp comprises: transporting the Class C domestic waste OCC and the Class D domestic waste OCC to a hydraulic pulper through a chain conveyor for pulping, and then sequentially performing a slag removal treatment, a coarse screening treatment, a fine screening treatment, a concentration treatment and a thermal dispersion treatment to obtain the bottom recycled pulp;

[0117] The solid content of the dry strength agent is 15wt%, and the addition amount of the dry strength agent is 15kg / t paper;

[0118] (3) After the alkyl ketene dimer is mixed with the top stock and the bottom stock, the top stock and the bottom stock are respectively flowed to a pressure screen and then sprayed onto the screen through a flow headbox to obtain a top layer wet paper web and a bottom layer wet paper web;

[0119] Wherein, the concentration of the alkyl ketene dimer is 12wt%, and the addition amount of the alkyl ketene dimer is 25kg / t paper;

[0120] (4) dehydrating the surface wet paper web and the bottom wet paper web obtained in step (3) respectively, and then vacuum-suction-compounding the surface wet paper web and the bottom wet paper web to obtain an original paperboard;

[0121] (5) subjecting the raw paperboard obtained in step (4) to one shoe press, two shoe presses, three light presses, drying, calendering, rewinding and film coating in sequence to obtain finished paper;

[0122] The pressure of the first shoe press is 700KN, the pressure of the second shoe press is 1100KN, and the pressure of the third light press is 40KN; the drying device includes a drying cylinder drying device; the outlet temperature of the drying cylinder drying device is ≥100℃;

[0123] There is no order distinction between steps (1) and (2).

[0124] Example 3

[0125] This embodiment provides an ultra-low gram-weight recycled white-faced kraft paper, wherein the recycled white-faced kraft paper comprises a top layer and a bottom layer; the gram-weight of the recycled white-faced kraft paper is 118 g / m 2 .

[0126] The surface layer has a grammage of 38 g / m 2 ; The raw materials for preparing the surface layer include domestic composite office waste paper;

[0127] The base layer has a grammage of 80 g / m 2The raw materials for preparing the bottom layer include the following components in mass fraction: 30wt% of Class C domestic waste OCC and 70wt% of Class D domestic waste OCC.

[0128] The preparation method of the ultra-low gram-weight recycled white kraft paper comprises the following steps:

[0129] (1) removing slag from the surface layer regenerated pulp and mixing it with calcium carbonate to obtain a dough;

[0130] The preparation method of the surface layer recycled pulp comprises: transporting domestic composite office waste paper to a drum pulper through a chain conveyor and mixing with sodium silicate for pulping, and then sequentially performing sand removal, flotation deinking, oxidation bleaching and beating to obtain the surface layer recycled pulp; the pulping concentration of the pulping treatment is 22%, the temperature is 60°C, and the pH value is 8.0; the amount of sodium silicate added is 6kg / t pulp; the flotation deinking treatment comprises sequentially primary flotation deinking, secondary flotation deinking and tertiary flotation deinking; the HLB value of the deinking agent used in the flotation deinking treatment is 12; the amount of the deinking agent used in the primary flotation deinking is 0.5kg / t pulp, and the amount of the deinking agent used in the secondary flotation deinking is 0.1kg / t pulp;

[0131] The whiteness of the surface layer recycled pulp is 85 degrees, A=1, B=6, and the dust content is less than 60 mg / cm 3 , the ink residue is less than 30;

[0132] The concentration of calcium carbonate is 12wt%, and the amount of calcium carbonate added is 35kg / t paper;

[0133] (2) removing slag from the bottom recycled pulp and mixing with a dry strength agent to obtain a bottom pulp;

[0134] The preparation method of the bottom recycled pulp comprises: transporting the Class C domestic waste OCC and the Class D domestic waste OCC to a hydraulic pulper through a chain conveyor for pulping, and then sequentially performing a slag removal treatment, a coarse screening treatment, a fine screening treatment, a concentration treatment and a thermal dispersion treatment to obtain the bottom recycled pulp;

[0135] The solid content of the dry strength agent is 25wt%, and the addition amount of the dry strength agent is 5kg / t paper;

[0136] (3) After the alkyl ketene dimer is mixed with the top stock and the bottom stock, the top stock and the bottom stock are respectively flowed to a pressure screen and then sprayed onto the screen through a flow headbox to obtain a top layer wet paper web and a bottom layer wet paper web;

[0137] Wherein, the concentration of the alkyl ketene dimer is 15wt%, and the addition amount of the alkyl ketene dimer is 15kg / t paper;

[0138] (4) dehydrating the surface wet paper web and the bottom wet paper web obtained in step (3) respectively, and then vacuum-suction-compounding the surface wet paper web and the bottom wet paper web to obtain an original paperboard;

[0139] (5) subjecting the raw paperboard obtained in step (4) to one shoe press, two shoe presses, three light presses, drying, calendering, rewinding and film coating in sequence to obtain finished paper;

[0140] The pressure of the first shoe press is 800KN, the pressure of the second shoe press is 1000KN, and the pressure of the third light press is 50KN; the drying device includes a drying cylinder drying device; the outlet temperature of the drying cylinder drying device is ≥100℃;

[0141] There is no order distinction between steps (1) and (2).

[0142] Example 4

[0143] This embodiment provides an ultra-low gram-weight recycled white-faced kraft paper, wherein the recycled white-faced kraft paper comprises a surface layer and a bottom layer; the gram-weight of the recycled white-faced kraft paper is 105 g / m 2 .

[0144] The surface layer has a grammage of 32 g / m 2 ; The raw materials for preparing the surface layer include domestic composite office waste paper;

[0145] The base layer has a grammage of 73 g / m 2 The raw materials for preparing the bottom layer are adjusted to include the following components by mass fraction: 50wt% of Class C domestic waste OCC and 50wt% of Class D domestic waste OCC.

[0146] The preparation method of the ultra-low grammage recycled white kraft paper is the same as that in Example 1.

[0147] Example 5

[0148] This embodiment provides an ultra-low gram-weight recycled white-faced kraft paper, wherein the recycled white-faced kraft paper comprises a top layer and a bottom layer; the gram-weight of the recycled white-faced kraft paper is 115 g / m 2 .

[0149] The surface layer has a grammage of 30 g / m 2 ; The raw materials for preparing the surface layer include domestic composite office waste paper;

[0150] The base layer has a grammage of 85 g / m 2 ; The raw material for preparing the bottom layer is adjusted to 100wt% of Class C domestic waste OCC.

[0151] The preparation method of the ultra-low grammage recycled white kraft paper is the same as that in Example 1.

[0152] Example 6

[0153] This embodiment provides an ultra-low gram-weight recycled white-faced kraft paper, wherein the recycled white-faced kraft paper comprises a top layer and a bottom layer; the gram-weight of the recycled white-faced kraft paper is 120 g / m 2 .

[0154] The surface layer has a grammage of 40 g / m 2 ; The raw materials for preparing the surface layer include domestic composite office waste paper;

[0155] The base layer has a grammage of 80 g / m 2 The raw materials for preparing the bottom layer include the following components in mass fraction: 20wt% of Class C domestic waste OCC and 80wt% of Class D domestic waste OCC.

[0156] The preparation method of the ultra-low gram-weight recycled white kraft paper differs from that of Example 1 only in that:

[0157] In this embodiment, in the method for preparing the surface layer regenerated pulp in step (1), the amount of the deinking agent used in the primary flotation deinking is adjusted to 0.2 kg / t pulp, and the amount of the deinking agent used in the secondary flotation deinking is adjusted to 0.5 kg / t pulp.

[0158] Example 7

[0159] This embodiment provides an ultra-low gram-weight recycled white-faced kraft paper, wherein the recycled white-faced kraft paper comprises a surface layer and a bottom layer; the gram-weight of the recycled white-faced kraft paper is 103 g / m 2 .

[0160] The surface layer has a grammage of 36 g / m 2 ; The raw materials for preparing the surface layer include domestic composite office waste paper;

[0161] The base layer has a grammage of 67 g / m 2 The raw materials for preparing the bottom layer include the following components in mass fraction: 20wt% of Class C domestic waste OCC and 80wt% of Class D domestic waste OCC.

[0162] The preparation method of the ultra-low gram-weight recycled white kraft paper differs from that of Example 1 only in that:

[0163] In this embodiment, in the method for preparing the surface layer regenerated pulp in step (1), the amount of the deinking agent used in the primary flotation deinking is adjusted to 0.7 kg / t pulp, and the amount of the deinking agent used in the secondary flotation deinking is adjusted to 0 kg / t pulp.

[0164] Example 8

[0165] This embodiment provides an ultra-low gram-weight recycled white-faced kraft paper, wherein the recycled white-faced kraft paper comprises a top layer and a bottom layer; the gram-weight of the recycled white-faced kraft paper is 102 g / m 2 .

[0166] The surface layer has a grammage of 36 g / m 2 ; The raw materials for preparing the surface layer include domestic composite office waste paper;

[0167] The weight of the bottom layer is 66 g / m 2 The raw materials for preparing the bottom layer include the following components in mass fraction: 20wt% of Class C domestic waste OCC and 80wt% of Class D domestic waste OCC.

[0168] The preparation method of the ultra-low gram-weight recycled white kraft paper differs from that of Example 1 only in that:

[0169] In this embodiment, the whiteness of the surface layer recycled pulp is adjusted to 70 degrees, A=2, B=3, and the dust content is 90 mg / cm 3 , ink residue is 50mg / cm 3 .

[0170] Example 9

[0171] This embodiment provides an ultra-low gram-weight recycled white-faced kraft paper, wherein the recycled white-faced kraft paper comprises a surface layer and a bottom layer; the gram-weight of the recycled white-faced kraft paper is 101 g / m 2 .

[0172] The surface layer has a grammage of 34 g / m 2 ; The raw materials for preparing the surface layer include domestic composite office waste paper;

[0173] The weight of the bottom layer is 66 g / m 2 The raw materials for preparing the bottom layer include the following components in mass fraction: 20wt% of Class C domestic waste OCC and 80wt% of Class D domestic waste OCC.

[0174] The preparation method of the ultra-low gram-weight recycled white kraft paper differs from that of Example 1 only in that:

[0175] In this embodiment, the amount of calcium carbonate added in step (1) is adjusted to 25 kg / t paper.

[0176] Example 10

[0177] This embodiment provides an ultra-low gram-weight recycled white-faced kraft paper, wherein the recycled white-faced kraft paper comprises a surface layer and a bottom layer; the gram-weight of the recycled white-faced kraft paper is 105 g / m 2 .

[0178] The surface layer has a grammage of 40 g / m2 ; The raw materials for preparing the surface layer include domestic composite office waste paper;

[0179] The base layer has a grammage of 65 g / m 2 The raw materials for preparing the bottom layer include the following components in mass fraction: 20wt% of Class C domestic waste OCC and 80wt% of Class D domestic waste OCC.

[0180] The preparation method of the ultra-low gram-weight recycled white kraft paper differs from that of Example 1 only in that:

[0181] In this embodiment, the amount of calcium carbonate added in step (1) is adjusted to 60 kg / t paper.

[0182] Embodiment 11

[0183] This embodiment provides an ultra-low gram-weight recycled white-faced kraft paper, wherein the recycled white-faced kraft paper comprises a top layer and a bottom layer; the gram-weight of the recycled white-faced kraft paper is 104 g / m 2 .

[0184] The surface layer has a grammage of 36 g / m 2 ; The raw materials for preparing the surface layer include domestic composite office waste paper;

[0185] The base layer has a grammage of 68 g / m 2 The raw materials for preparing the bottom layer include the following components in mass fraction: 20wt% of Class C domestic waste OCC and 80wt% of Class D domestic waste OCC.

[0186] The preparation method of the ultra-low gram-weight recycled white kraft paper differs from that of Example 1 only in that:

[0187] In this embodiment, the amount of the dry strength agent added in step (2) is adjusted to 2 kg / t paper.

[0188] Example 12

[0189] This embodiment provides an ultra-low gram-weight recycled white-faced kraft paper, wherein the recycled white-faced kraft paper comprises a surface layer and a bottom layer; the gram-weight of the recycled white-faced kraft paper is 101 g / m 2 .

[0190] The surface layer has a grammage of 38 g / m 2 ; The raw materials for preparing the surface layer include domestic composite office waste paper;

[0191] The base layer has a grammage of 63 g / m 2 The raw materials for preparing the bottom layer include the following components in mass fraction: 20wt% of Class C domestic waste OCC and 80wt% of Class D domestic waste OCC.

[0192] The preparation method of the ultra-low gram-weight recycled white kraft paper differs from that of Example 1 only in that:

[0193] In this embodiment, the amount of the dry strength agent added in step (2) is adjusted to 20 kg / t paper.

[0194] Embodiment 13

[0195] This embodiment provides an ultra-low gram-weight recycled white-faced kraft paper, wherein the recycled white-faced kraft paper comprises a surface layer and a bottom layer; the gram-weight of the recycled white-faced kraft paper is 103 g / m 2 .

[0196] The surface layer has a grammage of 34 g / m 2 ; The raw materials for preparing the surface layer include domestic composite office waste paper;

[0197] The base layer has a grammage of 69 g / m 2 The raw materials for preparing the bottom layer include the following components in mass fraction: 20wt% of Class C domestic waste OCC and 80wt% of Class D domestic waste OCC.

[0198] The preparation method of the ultra-low gram-weight recycled white kraft paper differs from that of Example 1 only in that:

[0199] In this example, the amount of alkyl ketene dimer added in step (3) is adjusted to 10 kg / t paper.

[0200] Embodiment 14

[0201] This embodiment provides an ultra-low gram-weight recycled white-faced kraft paper, wherein the recycled white-faced kraft paper comprises a top layer and a bottom layer; the gram-weight of the recycled white-faced kraft paper is 104 g / m 2 .

[0202] The surface layer has a grammage of 40 g / m 2 ; The raw materials for preparing the surface layer include domestic composite office waste paper;

[0203] The base layer has a grammage of 64 g / m 2 The raw materials for preparing the bottom layer include the following components in mass fraction: 20wt% of Class C domestic waste OCC and 80wt% of Class D domestic waste OCC.

[0204] The preparation method of the ultra-low gram-weight recycled white kraft paper differs from that of Example 1 only in that:

[0205] In this example, the amount of alkyl ketene dimer added in step (3) is adjusted to 30 kg / t paper.

[0206] Comparative Example 1

[0207] This comparative example provides an ultra-low gram-weight recycled white-faced kraft paper, wherein the recycled white-faced kraft paper comprises a top layer and a bottom layer; the gram-weight of the recycled white-faced kraft paper is 125 g / m 2 .

[0208] The surface layer has a grammage of 45 g / m 2 ; The raw materials for preparing the surface layer include domestic composite office waste paper;

[0209] The base layer has a grammage of 80 g / m 2 The raw materials for preparing the bottom layer include the following components in mass fraction: 20wt% of Class C domestic waste OCC and 80wt% of Class D domestic waste OCC.

[0210] The preparation method of the ultra-low gram-weight recycled white kraft paper differs from that of Example 1 only in that:

[0211] In this comparative example, the sizing in the pulp described in step (3) is adjusted as follows: after the drying treatment described in step (4), the sample paper is put into the surface sizing machine for front and back mode sizing. The solid content of the sizing material for the front side is 6.5%, the viscosity of the sizing material is 20 mPa·s, and the amount of glue applied is 1.5 g / m 2 The solid content of the back sizing material is 10%, the viscosity of the material is 50mPa·s, and the amount of glue applied is 2g / m 2 .

[0212] Performance testing:

[0213] The ultra-low grammage recycled white kraft paper provided in the above examples and comparative examples was tested for bursting resistance, folding endurance, smoothness and water absorption, and the results are shown in Table 1;

[0214] The bursting resistance is determined according to GB / T 1539-2007 "Determination of bursting resistance of paperboard", the folding resistance is determined according to GB / T 457-2008 "Determination of folding resistance of paper and paperboard", the water absorption is determined according to GB / T 461.3-2005 "Determination of water absorption of paper and paperboard (immersion method)"; and the smoothness is determined according to GB456 "Determination of smoothness of paper and paperboard (Buick method)".

[0215] Table 1

[0216]

[0217]

[0218] According to Table 1, we can know the following points:

[0219] (1) Comprehensive analysis of Examples 1-3 shows that the recycled white-faced kraft paper provided by the present invention has excellent physical properties on the basis of having ultra-low grammage, and can meet the needs of consumers for white-faced kraft paper;

[0220] (2) Comprehensive analysis of Example 1 and Examples 4-5 shows that the adjustment of the raw materials for preparing the bottom layer will affect the tear resistance and folding resistance of the finished paper;

[0221] When the usage ratio of Class C domestic waste OCC and Class D domestic waste OCC is 1:1, compared with Example 1, the tear resistance and folding resistance indexes are improved; when Class C domestic waste OCC is omitted, the tear resistance and folding resistance indexes are reduced;

[0222] (3) Comprehensive analysis of Example 1 and Examples 6-8 shows that the adjustment of the surface layer recycled pulp parameters will affect the smoothness of the obtained ultra-low grammage recycled white kraft paper;

[0223] (4) Comprehensive analysis of Example 1 and Examples 9-10 shows that the amount of calcium carbonate added to the dough will affect the uniformity and whiteness of the straight surface; when the amount of calcium carbonate added is too high, the whiteness and smoothness of the ultra-low grammage recycled white-faced kraft paper obtained will be too high, resulting in color difference in batches of paper, which will have an adverse effect on the product, or cause the uniformity of the paper to deteriorate, the physical indicators to deteriorate, the retention of the slurry to deteriorate, and will also affect the sizing effect of AKD to a certain extent; when the amount of calcium carbonate added is too low, the whiteness and smoothness of the ultra-low grammage recycled white-faced kraft paper obtained will be too low, resulting in color difference in batches of paper, which will have an adverse effect on the product;

[0224] (5) Comprehensive analysis of Example 1 and Examples 11-12 shows that the amount of dry strength agent added to the base slurry affects the physical properties of the paper; when the amount of dry strength agent added is too high, the physical properties of the finished paper cannot be further improved, resulting in a waste of raw materials and an increase in the preparation cost; when the amount of dry strength agent added is too low, the tear and fold resistance indexes are too low;

[0225] (6) Comprehensive analysis of Example 1 and Examples 13-14 shows that the amount of sizing agent added affects the water absorption and physical properties of the finished paper; when the amount of sizing agent added is too high (such as Example 14), the physical properties of the finished paper cannot be further improved, resulting in a waste of raw materials and an increase in the preparation cost; it may even lead to poor bonding or printing of the paperboard; when the amount of sizing agent added is too low (such as Example 13), it will lead to low water absorption;

[0226] (7) Comprehensive analysis of Example 1 and Comparative Example 1 shows that the sizing method affects the water absorption of the resulting paper, and the grammage of the resulting paper is relatively high.

[0227] In summary, the present invention uses 100% office composite waste paper as the surface layer pulp and 100% domestic waste OCC as the bottom layer pulp, and combines the optimization of pulping, flow conveying, sizing and other methods to obtain a recycled white-faced kraft paper with low production energy consumption, low grammage, high quality and strong performance.

[0228] The applicant declares that the specific embodiments described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. An ultra-low weight recycled white kraft paper, characterized in that: The recycled white kraft paper comprises a surface layer and a bottom layer; The gram weight of the recycled white kraft paper is 100-120 g / m 2 .

2. The ultra-low weight recycled white kraft paperboard according to claim 1, characterized in that: The surface layer has a grammage of 30 to 40 g / m 2 ; Preferably, the raw material for preparing the surface layer includes domestic composite office waste paper; Preferably, the weight of the bottom layer is 60 to 90 g / m 2 ; Preferably, the raw materials for preparing the bottom layer include the following components in mass fractions: 10-30wt% of Class C domestic waste OCC and 70-90wt% of Class D domestic waste OCC.

3. A method for preparing the ultra-low grammage recycled white kraft paper as claimed in claim 1 or 2, characterized in that: The preparation method comprises the following steps: (1) removing slag from the surface layer regenerated pulp and mixing it with calcium carbonate to obtain a dough; (2) removing slag from the bottom recycled pulp and mixing with a dry strength agent to obtain a bottom pulp; (3) After the surface stock and the bottom stock are mixed with sizing agents, they are respectively flowed to a pressure screen and then sprayed onto the screen through a flow headbox to obtain a surface wet paper web and a bottom wet paper web; (4) dehydrating the surface wet paper web and the bottom wet paper web obtained in step (3) respectively, and then vacuum-suction-compounding the surface wet paper web and the bottom wet paper web to obtain an original paperboard; (5) subjecting the raw paperboard obtained in step (4) to one shoe press, two shoe presses, three light presses, drying, calendering, rewinding and film coating in sequence to obtain finished paper; There is no order distinction between steps (1) and (2).

4. The preparation method according to claim 3, characterized in that: The preparation method of the surface layer recycled pulp in step (1) comprises: conveying domestic composite office waste paper to a drum pulper through a chain conveyor, mixing with sodium silicate, and then performing pulping treatment, and then performing sand removal treatment, flotation deinking treatment, oxidation bleaching treatment and pulping in sequence to obtain the surface layer recycled pulp.

5. The preparation method according to claim 4, characterized in that: The pulping concentration of the pulping treatment is 15-22%; Preferably, the temperature of the pulping treatment is 50-60°C; Preferably, the pH value of the pulping treatment is 7.0 to 8.0; Preferably, the addition amount of the sodium silicate is 3-6 kg / t slurry; Preferably, the flotation deinking treatment includes primary flotation deinking, secondary flotation deinking and tertiary flotation deinking performed in sequence; Preferably, the HLB value of the deinking agent used in the flotation deinking treatment is 11 to 12; Preferably, the amount of deinking agent used in the primary flotation deinking is 0.3-0.5 kg / t pulp; Preferably, the usage amount of the deinking agent in the secondary flotation deinking is 0.1-0.2 kg / t pulp.

6. The preparation method according to any one of claims 3 to 5, characterized in that: The whiteness of the surface layer regenerated pulp in step (1) is 80 to 85 degrees; Preferably, in step (1), the surface layer regenerated pulp has A=-1 to 1, B=-2 to 6; Preferably, the dust content in the surface regenerated slurry in step (1) is less than 60 mg / cm 3 ; Preferably, the residual ink (ERIC) in the surface layer regenerated pulp in step (1) is less than 30.

7. The preparation method according to claim 3, characterized in that: The preparation method of the bottom layer regenerated pulp in step (2) comprises: conveying Class C domestic waste OCC and Class D domestic waste OCC to a hydraulic pulper for pulping through a chain conveyor, and then sequentially performing deslagging treatment, coarse screening treatment, fine screening treatment, concentration treatment and thermal dispersion treatment to obtain the bottom layer regenerated pulp.

8. The preparation method according to claim 3, characterized in that: The concentration of calcium carbonate in step (1) is 10-12 wt %; Preferably, the amount of calcium carbonate added in step (1) is 35-50 kg / t paper; Preferably, the solid content of the dry strength agent in step (2) is 15 to 25 wt %; Preferably, the amount of the dry strength agent added in step (2) is 5 to 15 kg / t paper.

9. The preparation method according to any one of claims 3 to 8, characterized in that: The sizing agent in step (3) comprises an alkyl ketene dimer; Preferably, the concentration of the alkyl ketene dimer is 12 to 15 wt %; Preferably, the addition amount of the alkyl ketene dimer is 15-25 kg / t paper.

10. The preparation method according to any one of claims 3 to 9, characterized in that: The dryness of the raw paperboard in step (4) is 18-22%; Preferably, the pressure of the shoe press in step (5) is 700-800 KN; Preferably, the pressure of the second shoe press in step (5) is 1000-1100 KN; Preferably, the pressure of the three light pressures in step (5) is 40-50 KN; Preferably, the device used for the drying process in step (5) comprises a drying cylinder drying device; Preferably, the outlet temperature of the drying cylinder is ≥100°C.

Citation Information

Patent Citations

  • White craft paper and production method thereof

    CN103437242A

  • Waste paper regenerated color card paper and production process thereof