Method for preparing and analyzing lithofacies polished section of electric arc furnace slag
By optimizing the lithophase preparation process and polishing agent formula, the problems of low efficiency and poor sample quality in traditional methods are solved, and efficient and clear lithophase photosheet preparation is achieved to meet the analysis needs of arc furnace slag.
Patent Information
- Application Number
- CN202410997251.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-29
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Traditional lithophagometer preparation methods are inefficient, and cartilage and chromium oxide polishing agent are easily washed away by water, resulting in a long preparation time, and velvet polishing cloth is easily caused by new scratches, affecting the quality of the sample.
Using crushing, inlay, coarse grinding, medium grinding, fine grinding, rough polishing and fine polishing steps, use specific diamond grinding wheels and polishing agents, including running water lubrication and ultrasonic cleaning on the grinding and polishing machine, adjusting the polishing agent ratio and drip Add amounts to ensure the order and parameters of each step.
It significantly improves the sample preparation efficiency and reduces the adverse effects caused by personnel operation. The prepared lithophase optical sheet clearly displays the details of the phase under an optical microscope, meets the requirements of lithophase analysis, and has a higher quality than traditional methods.
Smart Images

Figure CN119043837A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of slag petrographic analysis, and in particular to a petrographic optical slice preparation and analysis method for electric arc furnace slag. Background Art
[0002] Petrographic analysis is a physical analysis method for process minerals. In the field of iron and steel metallurgy, it is mainly used for the phase analysis of various process minerals. After the petrographic samples are prepared, they are observed under an optical microscope to examine the type, quantity, size, shape, distribution state, etc. of the phases in the process minerals. The test results can guide the adjustment of metallurgical processes and can also be used for the comprehensive utilization of metallurgical by-products.
[0003] The number and output of green, environmentally friendly and energy-saving short-process steel mills are gradually increasing. As the core equipment of short-process steel mills, electric arc furnaces have completely different structures and processes from the converters used in long-process steel mills. This also determines that electric arc furnace steelmaking slag has unique physical and chemical properties, and the petrographic preparation of electric arc furnace slag also has different characteristics from the past.
[0004] The traditional petrographic preparation method is carried out in the following steps: (1) Sampling, cutting into small pieces of samples, and using the cut surface as the inspection surface; (2) Rough grinding: Add 120-150# corundum to the iron turntable, dissolve it in water and start the turntable, and grind the inspection surface roughly. During this period, it is necessary to continuously add water mixed with corundum to the turntable. After grinding until the scratch direction is consistent, clean the sample and the iron turntable (3) Intermediate grinding: Add 800-1000# corundum to the iron turntable, dissolve it in water and start the turntable, and grind the inspection surface intermediately. During this period, it is necessary to continuously add water mixed with corundum to the turntable. After grinding until the scratch direction is consistent, clean the sample. (4) Fine grinding: Use aluminum oxide slurry to finely grind the sample on a glass plate, remove all scratches and then clean it with water. (5) Polishing: Use velvet polishing cloth on the polishing machine, and use chromium oxide powder (which needs to be dissolved in water in advance) as the polishing agent. (6) After polishing, rinse with clean water and wipe dry with velvet or suede. Completed preparation. (Ren Yunfu. Lithofacies and Mineralogy of Iron and Steel Metallurgy [M]. Beijing, Metallurgical Industry Press. 1982, 41-42.)
[0005] The traditional preparation method currently has the following four shortcomings:
[0006] (1) After the diamond is dissolved in water, it is prepared on a turntable, which results in a very large loss. The diamond that has a grinding effect is easily washed away by water. The preparation efficiency is very low.
[0007] (2) During fine grinding, the time for fine grinding with alumina slurry on a glass plate is very long, generally not less than 40 minutes.
[0008] (3) During polishing, the chromium oxide dissolved in water can be easily washed away by water, and the polishing time is generally not less than 30 minutes.
[0009] (4) The velvet polishing cloth used for process mineral preparation is relatively thin, and it is easy for new scratches to be generated due to the residual particles or particles falling from the sample due to the unclean cleaning of the iron plate. Summary of the invention
[0010] The object of the present invention is to provide a petrographic optical section preparation and analysis method of electric arc furnace slag, which is mainly used to realize the petrographic optical section preparation of electric arc furnace slag and can effectively improve the preparation efficiency and effect of the sample.
[0011] In order to solve the above technical problems, the technical solution adopted by the present invention is:
[0012] A method for preparing and analyzing petrographic optical films of electric arc furnace slag comprises the following steps:
[0013] Step 1, breaking;
[0014] Step 2, inlay: take 5-20g of crushed slag particles and put them into an inlay mold;
[0015] Step 3, rough grinding: take the solidified sample out of the mold and perform rough grinding with a No. 20-40 diamond grinding wheel. The grinding machine speed is ≤60rad / min. The slag cross-sectional area exposed by rough grinding accounts for 50%-80% of the entire inspection surface.
[0016] Step 4, intermediate grinding: Use a diamond grinding wheel of No. 80-120 for intermediate grinding, the grinding machine speed is ≤100rad / min, during intermediate grinding, the sample is changed 90° direction, and the sample is ground until no trace of rough grinding can be seen by the naked eye;
[0017] Step 5, fine grinding, is carried out on a speed-adjustable metallographic sample pre-grinding machine or a grinding and polishing machine, and the fine grinding process needs to be lubricated with running water;
[0018] Step 6, rough polishing: rough polishing is performed on a metallographic sample grinder and polisher with adjustable speed, 1-3 ml of rough polishing agent is evenly sprayed on the polishing fabric, the speed of the grinder and polisher is 800-1200 rad / min, water is used for lubrication during the polishing process, water is dripped from the middle of the polishing disc, the dripping amount is 25-80 drops / min, and the inspection surface of the slag part is polished until there is no grinding mark;
[0019] Step 7, fine polishing: carried out on a metallographic sample grinding and polishing machine with adjustable speed, the polishing fabric is woolen cloth, the polishing agent jet grinding and polishing machine speed is 800-1200rad / min, the polishing process is lubricated with water, water is dripped from the middle of the polishing disc, the dripping amount is 15-60 drops / min, and the inspection surface of the slag part is polished to have no grinding marks;
[0020] Step 8: Perform petrographic analysis and measurement under an optical microscope.
[0021] Wherein, step 5 specifically includes the following steps:
[0022] Fine grinding 1: Use 120# metallographic sandpaper for fine grinding 1 on a pre-grinding machine or a grinding and polishing machine, with a speed range of 100-200rad / min. Before starting, the sample needs to be changed 90° in direction and ground until no trace of intermediate grinding can be seen by the naked eye. Then the sample needs to be changed 90° in direction again and ground until no trace of the previous grinding can be seen by the naked eye.
[0023] Fine grinding 2: Use 240# metallographic sandpaper for fine grinding 2 on a pre-grinding machine or a grinding and polishing machine, with a speed range of 200-400rad / min. Before starting, the sample needs to be changed 90° in direction and ground until the marks of the previous grinding can be seen with the naked eye;
[0024] Fine grinding 3: Use 400# metallographic sandpaper for fine grinding 3 on a pre-grinding machine or a grinding and polishing machine, with a speed range of 200-400rad / min. Before starting, the sample needs to be changed 90° in direction and ground until the previous grinding marks are invisible to the naked eye. Then the sample needs to be changed 90° in direction and ground again until the previous grinding marks are invisible to the naked eye.
[0025] Fine grinding 4: Use 600# metallographic sandpaper for fine grinding 4 on a pre-grinder or grinder-polisher, with a speed range of 400-600rad / min. Before starting, the sample needs to be changed 90° in direction and ground until no traces of the previous grinding can be seen by the naked eye.
[0026] Furthermore, in step 6, the polishing fabric is canvas or woolen cloth.
[0027] Among them, the rough polishing polishing agent configuration method is as follows:
[0028] 15g-45g 2.5μm diamond polishing paste;
[0029] Add to 100-150ml deionized water;
[0030] Then add 100-150ml of anhydrous ethanol;
[0031] 5-15ml dishwashing liquid and 7-9g sodium dodecylbenzene sulfonate, use an ultrasonic cleaner to shake until there is no agglomerated polishing paste in the solution.
[0032] 6. The method for preparing and analyzing the petrographic optical film of electric arc furnace slag according to claim 4, characterized in that the method for preparing the fine polishing agent is as follows:
[0033] 10-20g 0.5μm diamond polishing paste;
[0034] Add to 50-100 ml of deionized water;
[0035] Add 150-250ml of anhydrous ethanol;
[0036] 10-40ml dishwashing liquid and 3-5g sodium dodecylbenzene sulfonate. Use an ultrasonic cleaner to shake until there is no agglomerated polishing paste in the solution.
[0037] Preferably, in step 1, a crusher is used to crush the slag into particles of 1-5 mm.
[0038] Furthermore, in step 2, the amount of slag loaded is 1 / 3 of the height of the mold.
[0039] Compared with the prior art, the present invention has the following beneficial effects:
[0040] The present invention is mainly used to realize the preparation and analysis of petrographic optical films of electric arc furnace slag. In this application, the use of certain process parameters in the process steps can greatly reduce the adverse effects caused by human operation; more importantly, the present invention determines the order and parameters of each step from grinding to polishing according to the characteristics of electric arc furnace slag, and invents two polishing agents for use in combination. The prepared petrographic optical film can clearly show the quantity, size, morphology and distribution of various phases in the electric arc furnace slag under an optical microscope, which fully meets the requirements of petrographic analysis. The entire sample preparation process takes about 30 minutes, which is much more efficient than the traditional method and has high quality of prepared samples. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.
[0042] Figure 1 This is one of the typical optical microscopic morphology images of the electric arc furnace slag petrographic morphology of the present invention.
[0043] Figure 2 This is the second typical optical microscopic morphology of the electric arc furnace slag petrographic morphology of the present invention.
[0044] Figure 3 This is the third typical optical microscopic morphology of the electric arc furnace slag petrographic morphology of the present invention. DETAILED DESCRIPTION
[0045] Embodiment 1
[0046] This embodiment discloses a method for preparing and analyzing petrographic optical films of electric arc furnace slag, which specifically includes the following steps:
[0047] Step 1, crushing: Use a crusher to crush the slag into particles of 1-5mm; in actual use, if the particles are large, the position of the particles in the mold is difficult to control, the observation surface is insufficient, and a single particle is likely to cause the sample to be unrepresentative; if the particles are too small, some special structures of the physical phase will be destroyed, and the actual physical phase size, distribution form, etc. cannot be tested during analysis;
[0048] Step 2, inlay: Take 5-20g of crushed slag particles and put them into the inlay mold. The amount of slag loaded generally accounts for 1 / 3 of the height of the mold; so as to ensure that the amount of slag and the amount of resin have a specific ratio to avoid the situation of secondary breakage due to insufficient strength after inlay;
[0049] Mold size: diameter 15-30mm or rectangular: length × width × height (15-30mm) × (15-20mm) × (15-25mm), use commercial high-hardness cold mounting resin and curing agent for mounting, the hardness after solidification is 60-70HRC, mix the resin and curing agent in proportion, pour into the mold filled with an appropriate amount of slag, stir the resin with a small stick to make it fully mixed with the slag particles, and at the end of the stirring, use a small stick to press the slag particles to the bottom of the mold (test surface) as much as possible;
[0050] In actual use, vibration sedimentation method can also be used to achieve rapid sinking of slag particles.
[0051] (3) Rough grinding: After solidification, take the sample out of the mold and use a No. 20-40 diamond grinding wheel with a grinding machine speed not exceeding 60 rad / min for rough grinding. The slag cross-sectional area exposed during rough grinding should account for 50%-80% of the entire inspection surface.
[0052] (4) Intermediate grinding: Use a diamond grinding wheel No. 80-120 (grinding machine speed does not exceed 100 rad / min) for intermediate grinding. Intermediate grinding requires the sample to be changed 90° and ground until no traces of rough grinding can be seen by the naked eye.
[0053] (5) Fine grinding needs to be divided into 4 steps and carried out on a metallographic sample pre-grinding machine or grinding and polishing machine with adjustable speed. The fine grinding process requires running water lubrication.
[0054] Fine grinding 1: Use 120# metallographic sandpaper for fine grinding 1 on a pre-grinder or grinder-polisher, with a speed range of 100-200rad / min. Before starting, the sample needs to be changed 90° in direction and ground until the marks of intermediate grinding are invisible to the naked eye. Then the sample needs to be changed 90° in direction again and ground until the marks of the previous grinding are invisible to the naked eye.
[0055] Fine grinding 2: Use 240# metallographic sandpaper for fine grinding 2 on a pre-grinder or grinder-polisher, with a speed range of 200-400rad / min. Before starting, the sample needs to be changed 90° in direction and ground until the marks of the previous grinding can be seen with the naked eye.
[0056] Fine grinding 3: Use 400# metallographic sandpaper for fine grinding 3 on a pre-grinder or grinder-polisher, with a speed range of 200-400rad / min. Before starting, the sample needs to be changed 90° in direction and ground until the previous grinding marks are no longer visible to the naked eye. Then the sample needs to be changed 90° in direction and ground again until the previous grinding marks are no longer visible to the naked eye.
[0057] Fine grinding 4: Use 600# metallographic sandpaper for fine grinding 4 on a pre-grinder or grinder-polisher, with a speed range of 400-600rad / min. Before starting, the sample needs to be changed 90° in direction and ground until no traces of the previous grinding can be seen by the naked eye.
[0058] In the present invention, fine grinding is divided into four steps, and metallographic sandpapers with different mesh sizes are used to perform fine grinding from different angles, which can improve the quality of fine grinding and improve the final sample grinding effect.
[0059] (5) Rough polishing: Rough polishing is performed on a metallographic specimen grinding and polishing machine with adjustable speed. The polishing fabric is canvas or woolen cloth. The rough polishing agent needs to be prepared separately. Spray 1-3 ml of the rough polishing agent evenly on the polishing fabric. The speed of the grinding and polishing machine is 800-1200 rad / min. The polishing process is lubricated with water. Water is dripped from the middle of the polishing disc at a dripping rate of 25-80 drops / min. The inspection surface of the slag part is polished until there is no grinding mark.
[0060] Preparation method of rough polishing polishing agent: add 15g-45g 2.5μm diamond polishing paste into 100-150ml deionized water, then add 100-150ml anhydrous ethanol, 5-15ml detergent and 7-9g sodium dodecylbenzene sulfonate, and vibrate with an ultrasonic cleaner until there is no agglomerated polishing paste in the solution.
[0061] In the prior art, the commonly used polishing agent for petrography is chromium trioxide mixed with water, and diamond polishing agent is also used. However, due to the long preparation time of petrographic samples, the advantage of the rough polishing agent in the present invention is that it ensures that at the beginning of polishing, anhydrous ethanol has a certain wettability and can quickly play a lubricating role. After the anhydrous ethanol evaporates, the combination of water, detergent and sodium dodecylbenzene sulfonate has a certain moisturizing property, and the later polishing also has a certain lubricity. Compared with the lubricant in the prior art that only lubricates, the rough polishing agent is more suitable for the preparation of petrographic optical films of electric arc furnace slag.
[0062] At the same time, chromium trioxide is used to mix with water. Since the chromium trioxide polishing powder is packed in bags and has a size of 2.5μm, there is a large difference, which leads to poor effect of the configured polishing agent.
[0063] (6) Fine polishing: It is carried out on a metallographic specimen grinding and polishing machine with adjustable speed. The polishing fabric is woolen cloth. The fine polishing agent is prepared separately. The speed of the polishing agent jet grinding and polishing machine is 800-1200rad / min. The polishing process is lubricated with water. Water is dripped from the middle of the polishing disc at a dripping rate of 15-60 drops / min. The inspection surface of the slag part is polished until there is no grinding mark.
[0064] Preparation method of fine polishing polishing agent: add 10-20g 0.5μm diamond polishing paste to 50-100ml deionized water, then add 150-250ml anhydrous ethanol, 10-40ml detergent and 3-5g sodium dodecylbenzene sulfonate. Use ultrasonic cleaning machine to shake until there is no agglomerated polishing paste in the solution.
[0065] In the present application, the polishing agent used in the rough polishing step has the same composition as that used in the fine polishing step, but the ratio of the two is different; rough polishing requires a large amount of diamond particles to participate in grinding, while fine polishing does not require so many diamonds. At the same time, increasing the amount of anhydrous ethanol during fine polishing can effectively prevent dirt from adhering to the surface of the inspection surface; at the same time, the viscosity of the fine polishing agent is ensured in the fine polishing step, so that the fine polishing agent is more uniform as a whole, so as to improve the effect of fine polishing, and the amount of detergent used in the fine polishing agent is greater than the amount of detergent used in the rough polishing agent.
[0066] (7) Petrographic analysis and measurement under an optical microscope.
[0067] In order to facilitate those skilled in the art to further understand the present invention, the present invention is further described below in conjunction with specific implementation cases.
[0068] Case 1
[0069] 1. Sample:
[0070] The electric arc furnace slag with a crushed particle size of about 3mm is used, with a composition of 17.38% TFe, 15.19% FeO, 17.39% SiO2, CaO31.31%, MgO4.17%, a basicity of 2.04, and a hardness of 65HRC.
[0071] 2. Mounting: Take 7.2 g of crushed slag particles, put them into a silicone mounting mold with a diameter of 25 mm, and use FEMA brand metallographic cold mounting material (FXB model) to mount them. Mix the resin and curing agent in a 2:1 ratio, pour it into the mold filled with an appropriate amount of slag, and stir the resin with a small stick to fully mix it with the slag particles. When the stirring is finished, use a small stick to press the slag particles to the bottom of the mold as much as possible.
[0072] 3. Rough grinding: Take the solidified sample out of the mold and use a No. 20 diamond grinding wheel at a grinding machine speed of 50 rad / min for rough grinding. The slag cross-sectional area exposed by rough grinding should account for about 70% of the entire inspection surface.
[0073] 4. Intermediate grinding: Use a No. 80 diamond grinding wheel and a grinding machine speed of 80 rad / min for intermediate grinding. Change the direction of the sample by 90° and grind until no traces of rough grinding can be seen by the naked eye.
[0074] 5. Fine grinding is carried out on a metallographic sample pre-grinding machine with adjustable speed, and the fine grinding process is lubricated with running water.
[0075] The steps of fine grinding are as follows:
[0076] Fine grinding 1: On the pre-grinding machine, use 120# metallographic sandpaper for fine grinding 1, with a speed range of 100rad / min. Before starting, the sample is changed 90° in direction and ground until the marks of intermediate grinding are invisible to the naked eye. Then the sample is changed 90° in direction again and ground until the marks of the previous grinding are invisible to the naked eye.
[0077] Fine grinding 2: Use 240# metallographic sandpaper for fine grinding 2 on the pre-grinding machine, with a speed range of 200rad / min, and change the direction of the sample by 90° until the previous grinding marks are no longer visible to the naked eye.
[0078] Fine grinding 3: Use 400# metallographic sandpaper for fine grinding 3 on the pre-grinding machine, with a speed range of 300rad / min. The sample is changed 90° in direction and ground until the previous grinding marks are no longer visible to the naked eye. Then the sample is changed 90° in direction and ground again until the previous grinding marks are no longer visible to the naked eye.
[0079] Fine grinding 4: Use 600# metallographic sandpaper to perform fine grinding 4 on the pre-grinding machine, with a speed range of 600rad / min. Change the direction of the sample by 90° and grind until no traces of the previous grinding can be seen by the naked eye.
[0080] 6. Rough polishing: Rough polishing is performed on a speed-adjustable metallographic specimen grinding and polishing machine. The polishing fabric is woolen cloth. About 3 ml of rough polishing agent is evenly sprayed on the polishing fabric. The speed of the grinding and polishing machine is 1200 rad / min. Water is used for lubrication during the polishing process. Water is dripped from the middle of the polishing disc at a rate of 60 drops / min. The inspection surface of the slag part is polished until there is no grinding mark.
[0081] The method of preparing the rough polishing agent is as follows:
[0082] 30g of 2.5μm diamond polishing paste is added to 150ml of deionized water, followed by 150ml of anhydrous ethanol, 5ml of detergent and 7g of sodium dodecylbenzene sulfonate. The solution is shaken with an ultrasonic cleaner until there is no agglomerated polishing paste in the solution.
[0083] 7. Fine polishing: It is carried out on an adjustable speed metallographic specimen grinder and polisher. The polishing fabric is woolen cloth. About 1.5 ml of fine polishing agent is evenly sprayed on the polishing fabric. The speed of the grinder and polisher is 1200 rad / min. Water is dripped from the middle of the polishing disc at a rate of 40 drops / min. Polish until there are no signs of grinding on the inspection surface of the slag part.
[0084] The method of preparing the fine polishing agent is as follows:
[0085] 15g of 0.5μm diamond polishing paste is added to 50ml of deionized water, followed by 250ml of anhydrous ethanol, 30ml of detergent and 5g of sodium dodecylbenzene sulfonate. Use an ultrasonic cleaner to vibrate until there is no agglomerated polishing paste in the solution.
[0086] 8. Perform petrographic analysis and measurement under an optical microscope.
[0087] The morphology of the prepared samples under optical microscope is shown in Figure 1-3 , the details of each phase can be clearly displayed; Figure 1-Figure 3 In the process, the morphology of the electric furnace slag under the optical microscope can be clearly displayed, and the subtle organizational structure and the color contrast of the phase can be clearly displayed. This shows that the preparation effect is equivalent to that of the traditional method, but the influence of human factors is reduced and the efficiency is greatly improved.
[0088] The present invention realizes the preparation of petrographic films of electric arc furnace slag by coordinating the rotation speed values of pre-grinders and grinder-polishers, the grades and usage order of sandpapers in each process from rough grinding to fine grinding, the type selection of polishing fabrics in the polishing process, the spraying amount of polishing agent, the rotation speed value of the grinder-polishers, and the rough polishing polishing agent and the fine polishing polishing agent.
[0089] The present invention has developed a new method for preparing petrographic films of electric arc furnace slag according to the characteristics of electric arc furnace slag, determined the order and parameters of each step from grinding to polishing, and invented two polishing agents for use in combination. The prepared petrographic films can clearly show the quantity, size, morphology and distribution of various phases in the electric arc furnace slag under an optical microscope, fully meeting the requirements of petrographic analysis. The present invention replaces the technology in the preparation of petrographic films, and has improved efficiency and effect in actual use.
[0090] Although the preferred embodiments of the present invention have been described, those skilled in the art may make other changes and modifications to these embodiments once they have learned the basic creative concept. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the present invention.
[0091] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. It should be pointed out that any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing and analyzing petrographic optical films of electric arc furnace slag, It is characterized in that The specific steps include: Step 1, breaking; Step 2, inlay: take 5-20g of crushed slag particles and put them into the inlay mold; Step 3, rough grinding: take the solidified sample out of the mold and perform rough grinding with a No. 20-40 diamond grinding wheel. The grinding machine speed is ≤60rad / min. The slag cross-sectional area exposed by rough grinding accounts for 50%-80% of the entire inspection surface. Step 4, intermediate grinding: Use a diamond grinding wheel of No. 80-120 for intermediate grinding, the grinding machine speed is ≤100rad / min, during intermediate grinding, the sample is changed 90° direction, and the sample is ground until no trace of rough grinding can be seen by the naked eye; Step 5, fine grinding, is carried out on a speed-adjustable metallographic sample pre-grinding machine or a grinding and polishing machine, and the fine grinding process needs to be lubricated with running water; Step 6, rough polishing: rough polishing is performed on a metallographic sample grinder and polisher with adjustable speed, 1-3 ml of rough polishing agent is evenly sprayed on the polishing fabric, the speed of the grinder and polisher is 800-1200 rad / min, water is used for lubrication during the polishing process, water is dripped from the middle of the polishing disc, the dripping amount is 25-80 drops / min, and the inspection surface of the slag part is polished until there is no grinding mark; Step 7, fine polishing: carried out on a metallographic sample grinding and polishing machine with adjustable speed, the polishing fabric is woolen cloth, the polishing agent jet grinding and polishing machine speed is 800-1200rad / min, the polishing process is lubricated with water, water is dripped from the middle of the polishing disc, the dripping amount is 15-60 drops / min, and the inspection surface of the slag part is polished to have no grinding marks; Step 8: Perform petrographic analysis and measurement under an optical microscope.
2. The method for preparing and analyzing petrographic optical films of electric arc furnace slag according to claim 1, It is characterized in that Step 5 specifically includes the following steps: Fine grinding 1: Use 120# metallographic sandpaper for fine grinding 1 on a pre-grinding machine or a grinding and polishing machine, with a speed range of 100-200rad / min. Before starting, the sample needs to be changed 90° in direction and ground until no trace of intermediate grinding can be seen by the naked eye. Then the sample needs to be changed 90° in direction again and ground until no trace of the previous grinding can be seen by the naked eye. Fine grinding 2: Use 240# metallographic sandpaper for fine grinding 2 on a pre-grinding machine or a grinding and polishing machine, with a speed range of 200-400rad / min. Before starting, the sample needs to be changed 90° in direction and ground until the marks of the previous grinding can be seen with the naked eye; Fine grinding 3: Use 400# metallographic sandpaper for fine grinding 3 on a pre-grinding machine or a grinding and polishing machine, with a speed range of 200-400rad / min. Before starting, the sample needs to be changed 90° in direction and ground until the previous grinding marks are invisible to the naked eye. Then the sample needs to be changed 90° in direction and ground again until the previous grinding marks are invisible to the naked eye. Fine grinding 4: Use 600# metallographic sandpaper for fine grinding 4 on a pre-grinder or grinder-polisher, with a speed range of 400-600rad / min. Before starting, the sample needs to be changed 90° in direction and ground until no traces of the previous grinding can be seen by the naked eye.
3. The method for preparing and analyzing petrographic optical films of electric arc furnace slag according to claim 1, Features: In step 6, the polishing fabric is canvas or woolen cloth.
4. The method for preparing and analyzing petrographic optical films of electric arc furnace slag according to claim 1, It is characterized in that The method of preparing the rough polishing agent is as follows: 15g-45g 2.5μm diamond polishing paste; Add to 100-150ml deionized water; Then add 100-150ml of anhydrous ethanol; 5-15ml dishwashing liquid and 7-9g sodium dodecylbenzene sulfonate, use an ultrasonic cleaner to shake until there is no agglomerated polishing paste in the solution.
5. The method for preparing and analyzing petrographic optical films of electric arc furnace slag according to claim 3, It is characterized in that The method of preparing the fine polishing agent is as follows: 10-20g 0.5μm diamond polishing paste; Add to 50-100 ml of deionized water; Add 150-250ml of anhydrous ethanol; 10-40ml dishwashing liquid and 3-5g sodium dodecylbenzene sulfonate; use an ultrasonic cleaner to shake until there is no agglomerated polishing paste in the solution.
6. The method for preparing and analyzing petrographic optical films of electric arc furnace slag according to claim 1, Features: In step 1, a crusher is used to crush the slag into particles of 1-5 mm.
7. A method for preparing and analyzing petrographic optical films of electric arc furnace slag according to any one of claims 1 to 6, Features: In step 2, the amount of slag loaded should be 1 / 3 of the mold height.
Citation Information
Patent Citations
On-site metallographic examination polishing method applicable to tower material
CN103433813A
Metallographic sample preparation method for brittle and hard oxide layer on inner wall of heating surface tube
CN103759999A
Metallographic sample polishing agent
CN108085686A
Metallography test method for fastener silver coating thickness
CN108645678A
Method for accurately detecting components of composite inclusions in steel
CN116818756A
Cited By
Sintered ore sample preparation method, device, equipment, medium and program product
CN119860963A
Fixture for preparing artificial fracture of small-specification wire bar and artificial fracture preparation method