Stress relieving method and manufacturing method of pole piece and manufacturing method of battery roll core

By using a DC device to output current in the electrode welding area of ​​the lithium battery electrode sheet to generate thermal effect to eliminate stress, and welding under the thermal extension state, the problem of insufficient stress release in the prior art is solved, and the battery length is improved Cycling performance and stability.

CN119050260AActive Publication Date: 2024-11-29DONGGUAN CHAM BATTERY TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411257579.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-09
Publication Date
2024-11-29
Estimated Expiration
2044-09-09

AI Technical Summary

Technical Problem

In the manufacturing of lithium batteries, drying treatment cannot effectively release stress in the electrode sheet, especially in the electrode welding area and the negative electrode sheet finish overhang, resulting in the battery being easily broken during long cycles, affecting battery performance and safety. sex.

Method used

By connecting the electrode welding area with the DC device, the thermal effect of the current is used to achieve and maintain a temperature of 50°C to 60°C to eliminate the stress of the electrode sheet and performing the electrode welding while maintaining the thermal extension characteristics to avoid Anti-destruction of the surface oxide layer.

Benefits of technology

Effectively eliminate stress on the electrode plate, improve the long cycle performance of the battery, prevent fractures at the electrode welding position and the negative electrode plate closing overhang, and improve the stability and safety of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119050260A_ABST
    Figure CN119050260A_ABST
Patent Text Reader

Abstract

The invention discloses a stress relieving method and a manufacturing method of a pole piece and a manufacturing method of a battery roll core, and the stress relieving method of the pole piece comprises the following steps: providing a pretreated pole piece which comprises a tab welding area; and connecting the tab welding area with a direct current device, outputting current through the tab welding area by utilizing the direct current device, and enabling the tab welding area to reach and keep the temperature required for eliminating the stress so as to eliminate the stress of the tab welding area. According to the application, the stress of the pole piece can be fully eliminated, so that the welding position of the tab or the overhang area of the negative pole piece cannot be easily broken due to the stress in the long-cycle process of the battery after the subsequent pole piece is manufactured into the battery roll core, and the long-cycle performance of the battery is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of secondary batteries, and in particular to a stress elimination method and a manufacturing method of a pole piece and a manufacturing method of a battery core. Background Art

[0002] In the field of battery manufacturing technology, especially in the lithium battery manufacturing process, drying is a very critical link. This is because the moisture in the lithium battery will have a serious impact on the performance of the battery, such as reducing the battery capacity and affecting the safety of the battery. Therefore, after coating, it is generally necessary to vacuum bake the entire set of pole pieces or the bare battery cells after winding to eliminate the moisture in the pole pieces. In addition, this treatment method can also release the stress in the pole pieces and improve the performance of the battery.

[0003] However, this method has limited effect on stress relief of the current collector, especially in stress concentration areas (e.g., the lug welding area, the overhang area at the end of the negative pole piece, etc.). In some manufacturing processes, the stress of the current collector is eliminated by heat transfer during the lug welding process by heating the welding seat and welding head. This method is not only inefficient, but also easily damages the anti-oxidation layer on the surface of the current collector. In addition, during the long cycle of the battery, the lug welding position or the overhang area at the end of the negative pole piece is prone to fracture due to high stress, thereby increasing the resistance of the internal and external current loops, and even causing diving (capacity decay) to cause battery failure. Summary of the invention

[0004] The purpose of this application is to provide a stress elimination method and a manufacturing method of a pole piece and a manufacturing method of a battery core, which can fully eliminate the stress of the pole piece, prevent the pole piece from cracking due to stress problems, and improve the long cycle performance of the battery.

[0005] In order to achieve the above-mentioned purpose, the present application provides a method for eliminating stress of a pole piece, comprising:

[0006] Providing a pre-processed pole piece, wherein the pre-processed pole piece includes a pole lug welding area;

[0007] The tab welding area is connected to a direct current device, and the direct current device is used to output current through the tab welding area to make the tab welding area reach and maintain a temperature required for stress elimination so as to eliminate stress in the tab welding area.

[0008] Optionally, the pretreated electrode sheet is a positive electrode sheet and / or a negative electrode sheet.

[0009] Optionally, the maximum output current of the DC device is 100A.

[0010] Optionally, the voltage adjustment range of the DC device is 0-30V.

[0011] Optionally, the temperature required for stress elimination is in the range of 50°C to 60°C.

[0012] Optionally, the DC device is used to output current so that the tab welding area maintains the temperature required for stress elimination for a first period of time.

[0013] In order to achieve the above-mentioned object, the present application also provides a method for manufacturing a pole piece, including the pole piece stress elimination method as described above;

[0014] The pole piece manufacturing method also includes:

[0015] The electrode tab is welded to the pre-treated electrode sheet in a state where the pre-treated electrode sheet still maintains thermal ductility after the stress is eliminated.

[0016] Optionally, after the pre-treated electrode sheet is stress-free, the electrode tab is welded to the pre-treated electrode sheet within a second time period, and the second time period is 1 to 3 seconds.

[0017] In order to achieve the above-mentioned object, the present application also provides a method for manufacturing a battery roll core for a secondary battery, comprising:

[0018] Providing a pre-processed pole piece, wherein the pre-processed pole piece includes a pole lug welding area;

[0019] Connecting the tab welding area to a direct current device, using the direct current device to output current through the tab welding area and causing the tab welding area to reach and maintain a temperature required for stress elimination to eliminate stress in the tab welding area;

[0020] Welding the tab to the tab welding area;

[0021] The material to be wound is wound into a bare winding core, wherein the material to be wound includes the pre-treated pole piece after the pole ear is welded.

[0022] Optionally, the core material to be wound includes a positive electrode sheet, a negative electrode sheet and a separator, the pre-treated electrode sheet after welding the electrode tabs is the positive electrode sheet and / or the negative electrode sheet, and the separator is used to separate the positive electrode sheet and the negative electrode sheet.

[0023] In an embodiment of the present application, the pole piece stress elimination method is to eliminate the stress in the pole piece welding area by connecting the pole piece lug welding area of ​​the pre-treated pole piece to a direct current device, and using the direct current device to output current through the pole piece lug welding area and make the pole piece welding area reach and maintain the temperature required for stress elimination. The embodiment of the present application utilizes the thermal effect of the current to generate heat inside the substrate of the pre-treated pole piece, thereby achieving effective stress elimination. In addition, the conductivity of the substrate of the pre-treated pole piece is higher than the conductivity of the surface anti-oxidation layer of the pre-treated pole piece, so the thermal effect of the current will be concentrated on the substrate, which can avoid external heat transfer from damaging the surface anti-oxidation layer of the pre-treated pole piece. This method can fully eliminate the stress of the pole piece, so that after the subsequent pole piece is made into a battery roll core, the welding position of the pole piece or the area at the end overhang of the negative pole piece will not be easily broken due to stress during the long cycle of the battery, thereby improving the long cycle performance of the battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 This is a flow chart of a method for eliminating stress of a pole piece according to an embodiment of the present application.

[0025] Figure 2 Schematic diagram of the connection between the tab welding area and the DC device in the embodiment of the present application.

[0026] Figure 3 It is a schematic diagram of the DC device outputting current to the pole piece in the embodiment of the present application.

[0027] Figure 4 This is a flow chart of a method for manufacturing a pole piece according to an embodiment of the present application.

[0028] Figure 5 This is a schematic diagram of the electrode tab being welded to the electrode piece according to an embodiment of the present application.

[0029] Figure 6 Flow chart of a method for manufacturing a battery roll core according to an embodiment of the present application.

[0030] Figure 7 This is a schematic diagram of a bare core obtained after winding according to an embodiment of the present application. DETAILED DESCRIPTION

[0031] In order to explain the technical content, structural features and achieved effects of the present application in detail, the following is a detailed description in combination with the implementation methods and the accompanying drawings.

[0032] In order to make the above-mentioned purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are described in detail below in conjunction with the accompanying drawings. In the following description, many specific details are set forth to facilitate a full understanding of the present application. However, the present application can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present application, so the present application is not limited by the specific embodiments disclosed below.

[0033] Embodiment 1

[0034] See also Figures 1 to 3 This embodiment discloses a method for eliminating stress of a pole piece, comprising:

[0035] S11 , providing a pre-processed pole piece 1 , wherein the pre-processed pole piece 1 includes a pole lug welding area 11 .

[0036] Specifically, the pre-treated electrode sheet 1 is a positive electrode sheet and / or a negative electrode sheet.

[0037] Furthermore, the pre-treated pole piece 1 is made of a current collector through a pole piece manufacturing process, and the pole piece manufacturing process includes:

[0038] (1) Slurry preparation: The positive / negative electrode active material, conductive agent, binder and an appropriate amount of solvent are mixed evenly to form positive / negative electrode slurry.

[0039] Specifically, common positive electrode active materials include lithium cobalt oxide, lithium manganese oxide, lithium iron phosphate and ternary materials (such as nickel cobalt lithium manganese oxide), etc. Common negative electrode active materials include graphite, silicon-based materials, lithium titanate, etc. Conductive agents such as carbon black and graphene are used to improve the conductivity of the electrode, while binders such as polyvinylidene fluoride (PVDF) are used to bond the active material to the current collector.

[0040] (2) Coating: The positive / negative electrode slurry is evenly coated on the surface of the current collector.

[0041] The prepared positive / negative slurry is evenly coated on the current collector. The coating process needs to control the thickness and uniformity of the slurry to ensure the quality of the positive / negative electrode sheets.

[0042] Generally speaking, the base material of the current collector used in the positive electrode sheet is aluminum foil, while the base material of the current collector used in the negative electrode sheet is copper foil.

[0043] (3) Rolling: The coated current collector is subjected to a rolling process.

[0044] Rolling can enhance the bonding strength between the active material and the foil to prevent the active material from peeling off during the electrolyte immersion and battery use. In addition, ensuring that the surface of the pole piece is smooth and flat, preventing the burrs on the coating surface from piercing the diaphragm and causing a short circuit, and compacting the pole piece coating material can reduce the volume of the pole piece to increase the energy density of the battery.

[0045] The pole piece rolling is divided into two methods: cold rolling and hot rolling. In terms of rolling procedures, it can be divided into single rolling and multiple rolling. The multiple rolling process is relatively complicated, but it can reduce the rebound of the pole piece, and the pole piece has good gloss and high thickness consistency.

[0046] (4) Cutting: Cut the rolled current collector into required sizes to obtain pole pieces.

[0047] (5) Baking: Baking the electrode.

[0048] The main purpose of baking the electrode is to remove moisture and organic solvents in the electrode and improve the stability and electrochemical performance of the electrode. By baking, the active substances in the electrode can be fully dried to avoid performance degradation or safety problems caused by residual moisture in the subsequent production and use.

[0049] Generally speaking, the baking temperature of the positive electrode is slightly higher than that of the negative electrode. Depending on the material and process requirements, the baking temperature is usually between 100-130°C. For example, studies have shown that the positive electrode is best baked at 110-130°C for 12 hours, while the negative electrode is preferably baked at 100-120°C for 12 hours. However, the specific baking temperature needs to be adjusted according to the design and production process of the battery.

[0050] Usually, the baking process needs to be carried out in a vacuum environment or under the protection of an inert gas. The surface of the electrode to be baked needs to be clean and free of impurities, and after baking it needs to be cooled to room temperature before being taken out.

[0051] S12, connecting the tab welding area 11 to the DC device 2, using the DC device 2 to output current through the tab welding area 11 and making the tab welding area 11 reach and maintain the temperature required for eliminating stress so as to eliminate stress in the tab welding area 11.

[0052] The tab welding area 11 is connected to the DC device 2 as shown in FIG. Figure 2 and Figure 3 As shown, Figure 3 The direction of the arrow is the direction of the current.

[0053] Specifically, an anti-oxidation layer is formed on the surface of the pre-treated electrode piece 1 .

[0054] More specifically, the anti-oxidation layer is a chromium passivation layer or an aluminum passivation layer.

[0055] In the process of outputting current, the thermal effect of the current is used to generate heat inside the pre-processed electrode 1, thereby achieving effective stress elimination. At this time, the conductivity of the substrate of the pre-processed electrode 1 is higher than the anti-oxidation layer on the surface, so the thermal effect of the current will be concentrated on the substrate of the pre-processed electrode 1, thereby avoiding the damage of the anti-oxidation layer on the surface of the pre-processed electrode 1 by external heat transfer.

[0056] Specifically, the maximum output current of the DC device 2 is 100 A. Of course, the present application does not impose any limitation on the maximum output current of the DC device 2 .

[0057] Specifically, the voltage adjustment range of the DC device 2 is 0-30 V. Of course, the present application does not limit the voltage adjustment range of the DC device 2.

[0058] Specifically, the temperature required for stress relief is in the range of 50°C to 60°C.

[0059] It is understood that the temperature required to relieve stress is a range and is not limited to a specific value.

[0060] Specifically, the DC device 2 outputs current to keep the electrode tab welding area 11 at the temperature required for stress elimination for a first time period, and the first time period needs to be set in combination with actual conditions. In addition, it is also possible to determine whether stress elimination is completed by observing or measuring the parameters of the electrode piece, and the power-on time period does not need to be set to a certain time period.

[0061] Specifically, the DC device 2 includes a DC voltage-stabilized power supply, a DC constant current source and a high-power DC power supply, which can be selected according to needs.

[0062] In the embodiment of the present application, the pole piece stress elimination method is to connect the pole lug welding area 11 of the pre-treated pole piece 1 with the direct current device 2, and use the direct current device 2 to output current through the pole lug welding area 11 so that the pole lug welding area 11 reaches and maintains the temperature required for stress elimination to eliminate the stress of the pole lug welding area 11. The embodiment of the present application utilizes the thermal effect of the current to generate heat inside the substrate of the pre-treated pole piece 1, thereby achieving effective stress elimination. In addition, the conductivity of the substrate of the pre-treated pole piece 1 is higher than the conductivity of the surface anti-oxidation layer of the pre-treated pole piece 1, so the thermal effect of the current will be concentrated on the substrate, which can avoid external heat transfer from damaging the surface anti-oxidation layer of the pre-treated pole piece 1. This method can fully eliminate the stress of the pole piece, so that after the subsequent pole piece is made into a battery roll core, the welding position of the pole lug 3 or the area at the end overhang of the negative pole piece will not be easily broken due to stress during the long cycle of the battery, thereby improving the long cycle performance of the battery.

[0063] Embodiment 2

[0064] See also Figure 4 and Figure 5 This embodiment discloses a method for manufacturing a pole piece, comprising:

[0065] S21 , providing a pre-processed pole piece 1 , wherein the pre-processed pole piece 1 includes a pole lug welding area 11 .

[0066] S22 , connecting the tab welding area 11 to the DC device 2 , using the DC device 2 to output current through the tab welding area 11 and allowing the tab welding area 11 to reach and maintain a temperature required for eliminating stress, so as to eliminate stress in the tab welding area 11 .

[0067] It should be understood that the specific implementation details of step S21 and step S22 are the same as step S11 and step S12 of embodiment 1, and are not described in detail here.

[0068] S23, welding the electrode tab 3 to the pre-treated electrode sheet 1 while the pre-treated electrode sheet 1 still maintains the thermal ductility property after the stress is eliminated.

[0069] Specifically, after the pre-processed electrode sheet 1 eliminates stress, the electrode tab 3 is welded to the pre-processed electrode sheet 1 within the second time period, and the second time period is 1 to 3 seconds. Of course, the second time period is not limited to this.

[0070] See also Figure 5 It should be understood that after the stress of the pole ear welding area 11 is eliminated, the welding of the pole ear 3 should be completed as quickly as possible to ensure that the pole piece maintains better thermal ductility during the welding process. In addition, the positive pole ear is welded to the positive pole sheet, and the negative pole ear is welded to the negative pole sheet. The number of pole ears 3 can be single or multiple.

[0071] Specifically, the tab welding area 11 is usually located at a specific position of the pole piece, and the selection of this position depends on the design of the battery, the layout of the tab 3 and the requirements of the welding process. Generally speaking, the welding area needs to meet the following conditions:

[0072] (1) Easy to operate: The welding area should be convenient for the operation of the welding equipment to ensure that the welding head can be accurately aligned and pressure can be applied during the welding process.

[0073] (2) Welding quality: The welding area should be able to produce good welding results, that is, the welding point should be firm and free of defects such as cracks and cold welds.

[0074] (3) Structural stability: The electrode tab 3 and the electrode piece after welding should have good structural stability and be able to withstand various forces and stresses generated during the use of the battery.

[0075] Specifically, the welding methods that can be selected are mainly ultrasonic welding and laser welding.

[0076] Embodiment 3

[0077] See also Figure 6 and Figure 7 This embodiment discloses a method for manufacturing a battery roll core for a secondary battery, comprising:

[0078] S31 , providing a pre-processed pole piece 1 , wherein the pre-processed pole piece 1 includes a pole lug welding area 11 .

[0079] S32 , connecting the tab welding area 11 to the DC device 2 , using the DC device 2 to output current through the tab welding area 11 and allowing the tab welding area 11 to reach and maintain a temperature required for eliminating stress, so as to eliminate stress in the tab welding area 11 .

[0080] It should be understood that the specific implementation details of step S31 and step S32 are the same as step S21 and step S22 of embodiment 2 and step S11 and step S12 of embodiment 1, and are not described in detail here.

[0081] S33 , welding the tab 3 to the tab welding area 11 .

[0082] It should be understood that the specific implementation details of step S33 are the same as those of step S23 in embodiment 2, and are not described in detail here.

[0083] S34, winding the material to be wound into a bare winding core 4 (such as Figure 7 As shown), the material to be wound includes the pre-treated pole piece 1 after welding the pole ear 3.

[0084] Specifically, the winding core material includes a positive electrode sheet, a negative electrode sheet and a separator. The pre-treated electrode sheet 1 after welding the electrode tab 3 is a positive electrode sheet and / or a negative electrode sheet. The separator is used to separate the positive electrode sheet and the negative electrode sheet.

[0085] In the above-mentioned battery core manufacturing process, the pre-treated electrode sheet 1 can be a positive electrode sheet or a negative electrode sheet. Before winding into a core, the positive electrode sheet, the diaphragm and the negative electrode sheet are placed in a certain order, such as the order of diaphragm-positive electrode-diaphragm-negative electrode, and then wound by a winder. During the winding process of the winder, it is necessary to ensure the alignment and fit between the positive electrode sheet, the negative electrode sheet and the diaphragm (especially the end 5 of the diaphragm) to avoid problems such as misalignment or wrinkles and uneven thickness at the end 5 of the diaphragm. In addition, after the winding is completed, the bare core 4 is fixed with a termination tape 6 to ensure the integrity and stability of the battery structure, while providing reliable insulation protection to prevent internal short circuits in the battery.

[0086] After winding is completed, it can also be processed through the following processes:

[0087] (1) Filling electrolyte: The electrolyte is filled into the bare core 4 by impregnation or coating to achieve ion transfer between the positive and negative electrodes.

[0088] (2) Sealing and packaging: The core is sealed and a sealant is added to the seal to ensure that the electrolyte does not leak. The core is then placed in an aluminum-plastic composite film bag and heat-sealed.

[0089] (3) Forming test: Perform appearance inspection, electrical performance test and safety performance test on the finished core to ensure that the core meets the design requirements and quality standards.

[0090] Specifically, the above method is suitable for making the core of secondary batteries such as cylindrical batteries and soft pack batteries.

[0091] In summary, in the embodiment of the present application, by connecting the pole ear welding area 11 of the pre-treated pole piece 1 to the DC device 2, the pole ear welding area 11 reaches and maintains the temperature required for stress elimination by outputting current, and the thermal effect of the current is used to generate heat inside the substrate of the pre-treated pole piece 1, thereby effectively eliminating stress. In addition, the conductivity of the substrate of the pre-treated pole piece 1 is higher than the conductivity of the surface anti-oxidation layer of the pre-treated pole piece 1, so the thermal effect of the current will be concentrated on the substrate, which can avoid the damage of the surface anti-oxidation layer of the pre-treated pole piece 1 by external heat transfer. And after power is turned on, the pole ear 3 is welded to the pole ear welding area 11 within the second time length to ensure that the pre-treated pole piece 1 maintains better thermal ductility during the welding process. Finally, the pre-treated pole piece 1 is made into a bare winding core 4 through a winding process. The present application can fully eliminate the stress of the winding core, so that the welding position of the pole ear 3 or the area at the end overhang of the negative pole piece will not be easily broken due to stress during the long cycle of the battery, thereby improving the long cycle performance of the battery.

[0092] The above disclosure is only a preferred example of the present application, and its role is to facilitate the technical personnel in this field to understand and implement it. Of course, it cannot be used to limit the scope of rights of the present application. Therefore, equivalent changes made according to the scope of the patent application of the present application still fall within the scope covered by the present application.

Claims

1. A method for eliminating stress of a pole piece, characterized in that: include: Providing a pre-processed pole piece, wherein the pre-processed pole piece includes a pole lug welding area; The tab welding area is connected to a direct current device, and the direct current device is used to output current through the tab welding area to make the tab welding area reach and maintain a temperature required for stress elimination so as to eliminate stress in the tab welding area.

2. The pole piece stress relief method according to claim 1, characterized in that: The pre-treated electrode sheet is a positive electrode sheet and / or a negative electrode sheet.

3. The pole piece stress relief method according to claim 1, characterized in that: The maximum output current of the DC device is 100A.

4. The pole piece stress relief method according to claim 1, characterized in that: The voltage adjustment range of the DC device is 0-30V.

5. The pole piece stress relief method according to claim 1, characterized in that: The temperature required for stress relief is in the range of 50°C to 60°C.

6. The pole piece stress relief method according to claim 1, characterized in that: The DC device is used to output current so that the tab welding area maintains the temperature required for stress elimination for a first time period.

7. A method for manufacturing a pole piece, characterized in that: A method for eliminating stress of a pole piece according to any one of claims 1 to 6; The pole piece manufacturing method also includes: The electrode tab is welded to the pre-treated electrode sheet in a state where the pre-treated electrode sheet still maintains thermal ductility after the stress is eliminated.

8. The method for manufacturing a pole piece according to claim 7, characterized in that: After the pre-processed electrode sheet is stress-free, the electrode tab is welded to the pre-processed electrode sheet within a second time period, and the second time period is 1 to 3 seconds.

9. A method for manufacturing a battery core for a secondary battery, characterized in that: include: Providing a pre-processed pole piece, wherein the pre-processed pole piece includes a pole lug welding area; Connecting the tab welding area to a direct current device, using the direct current device to output current through the tab welding area and causing the tab welding area to reach and maintain a temperature required for stress elimination to eliminate stress in the tab welding area; Welding the tab to the tab welding area; The material to be wound is wound into a bare winding core, wherein the material to be wound includes the pre-treated pole piece after the pole ear is welded.

10. The method for manufacturing a battery roll core according to claim 9, characterized in that: The core material to be wound includes a positive electrode sheet, a negative electrode sheet and a separator. The pre-treated electrode sheet after welding the electrode tabs is the positive electrode sheet and / or the negative electrode sheet. The separator is used to separate the positive electrode sheet and the negative electrode sheet.

Citation Information

Patent Citations

  • Method for joining electrically conductive parts

    DE19735219A1

  • Method for manufacturing of nonaqueous electrolyte secondary battery electrode, and manufacturing method of nonaqueous electrolyte secondary battery electrode group