Titanium steel added with Ni-Cu composite intermediate foil layer and processing method of titanium steel

By using Ni-Cu composite intermediate foil layer and high-efficiency ytterbium-doped fiber laser welding technology in titanium/steel differential metal welding, the formation of Ti-Fe binary brittle phase is hindered, significantly improving the mechanical properties of the joints, and solving the existing solutions The problem of Ti-Fe brittle phase in the technology has achieved good welding process performance and high tensile strength.

CN119057240AInactive Publication Date: 2024-12-03ANHUI POLYTECHNIC UNIV MECHANICAL & ELECTRICAL COLLEGE

Patent Information

Application Number
CN202411416369.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-11
Publication Date
2024-12-03
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The prior art is difficult to effectively suppress the formation of Ti-Fe binary brittle phase in titanium/steel different metal welding, resulting in less obvious improvement in the mechanical properties of the joints and the single intermediate layer material cannot completely hinder the diffusion of elements.

Method used

Using titanium steel with Ni-Cu composite intermediate foil layer, the welding parameters are adjusted through efficient ytterbium-doped fiber laser welding, so that the stainless steel-copper foil welds and copper-ni-foil welds are formed, hindering the diffusion of Fe and Ti elements and forming The nickel foil is not completely melted to inhibit the generation of the brittle phase.

Benefits of technology

It effectively hinders the diffusion of Fe and Ti elements, reduces the brittleness of the joint, improves the mechanical properties of the joint, reaches 448MPa, and has good welding process performance, avoiding defects such as cracks and pinholes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119057240A_ABST
    Figure CN119057240A_ABST
Patent Text Reader

Abstract

The invention discloses titanium steel added with a Ni-Cu composite middle foil layer and a processing method of the titanium steel. The titanium steel is characterized in that materials are sequentially overlapped according to the sequence of stainless steel, copper foil, nickel foil and titanium alloy from top to bottom, overlapping overlapping areas are welded, the materials are fused, and the Ni-Cu composite middle foil layer is obtained through welding. And a welding joint formed by welding seams formed by stainless steel-copper melting and welding seams formed by copper-nickel and nickel-titanium alloy under the heat conduction effect is formed. Nickel foil which is not completely molten exists in the joint, diffusion and combination of Fe and Ti elements are effectively hindered, generation of a Ti-Fe binary brittle phase is inhibited, the brittleness of the joint is reduced, and the mechanical property of the joint is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of (welding (connection) of dissimilar materials), and in particular relates to a titanium steel with a Ni-Cu composite intermediate foil layer added thereto and a processing method thereof, which is applied to the fields of new energy vehicles, aerospace, military manufacturing, etc. Background Art

[0002] Stainless steel has been widely used for many years due to its excellent mechanical properties and relatively low cost. However, with the development of industrial technology, its high quality and insufficient corrosion resistance have become increasingly prominent. Titanium alloy, as a metal material with high specific strength, stronger corrosion resistance and better comprehensive mechanical properties, can replace stainless steel to a certain extent, but its cost is relatively high. Therefore, in order to combine the excellent properties of stainless steel and titanium alloy while taking into account the production cost, stainless steel-titanium alloy composite structure has become an important research topic in many manufacturing industries.

[0003] At present, the preparation of titanium / steel dissimilar metal welding joints mainly adopts explosion welding, stir friction welding, electron beam welding, laser welding, etc., but except laser welding, other welding processes are mostly limited by the shape of welding materials, etc. In addition, due to the high energy density and concentrated heat input of laser welding, it has a certain inhibitory effect on the intermetallic compounds that are easy to produce during the welding of dissimilar materials. Therefore, laser welding process is the most widely used.

[0004] In the process of implementing the present invention, the inventors found that the prior art has at least the following problems:

[0005] In order to better suppress the formation of Ti-Fe binary brittle phase in the joint, the intermediate layer material is often added while using laser welding. However, when a single intermediate layer material, such as Cu, V, Ni, etc., is used to prepare titanium-steel dissimilar metal laser welding joints, although the diffusion of Ti and Fe elements in the parent material is hindered to a certain extent, a small amount of Ti-Fe brittle phase is still formed, so the improvement of the mechanical properties of the joint is not obvious.

[0006] CN106695173A-A welding material for welding titanium-steel composite plate near titanium layer and its preparation method discloses a welding material for welding titanium-steel composite plate near titanium layer and its manufacturing method, the composition of the welding material is as follows by mass percentage: C≤0.02%, Si≤0.02%, Mn3.2-3.38%, P≤0.02%, S≤0.01%, Cr 13-15%, Cu0.012-0.014%, Fe≤0.7%, Ti 0.3-0.52, Co 0.032-0.038%, Nb+Ta 1.9-3%, and the balance is Ni. It also cannot solve the above technical problems. Summary of the invention

[0007] The technical problem to be solved by the present invention is to provide a titanium steel with a Ni-Cu composite intermediate foil layer and a processing method thereof.

[0008] In order to solve the above technical problems, the technical solution adopted by the present invention is: a titanium steel with a Ni-Cu composite intermediate foil layer added, the materials are overlapped and placed in the order of stainless steel, copper foil, nickel foil, and titanium alloy from top to bottom, and the overlapping areas are welded to fuse the materials.

[0009] After the materials are placed, use clamps to clamp them to maintain compression between the materials.

[0010] The fixture has a base plate, and the stainless steel, copper foil, nickel foil, and titanium alloy are placed on the base plate in sequence; clamping plates are provided on both sides of the base plate, and the clamping plates are connected to the base plate through fastening nuts, and the clamping plates can clamp the materials.

[0011] The copper foil is 0.05 mm thick, and the nickel foil is 0.3 mm thick.

[0012] The above-mentioned method for processing titanium steel with a Ni-Cu composite intermediate foil layer adopts a welding process, and the welding is performed using a high-efficiency ytterbium-doped fiber laser.

[0013] The materials are pretreated before welding. The stainless steel and titanium alloy base materials are polished with sandpaper to remove the oxide layer on the surface of the materials. Then, the stainless steel and titanium alloy base materials as well as the nickel and copper foils are cleaned with acetone to remove surface oil stains.

[0014] During welding, the laser emission angle is adjusted to weld the overlapping areas to obtain a stainless steel-copper foil weld. The copper foil middle layer continues to conduct heat downward to form a copper foil-nickel foil weld and a nickel foil-titanium alloy weld.

[0015] During welding, the welding speed and laser power are adjusted so that the middle layer of the vanadium foil is not completely melted. After welding, a joint consisting of a weld formed by the melting of stainless steel-copper, copper-vanadium, an incompletely melted nickel foil and a weld formed by heat conduction of nickel-titanium alloy is obtained, eliminating the brittleness of the joint.

[0016] The welding speed is 30mm / s, the laser power is 2900W-3100W, and the defocus is 0.

[0017] The laser emission angle is 9°-12° to the material surface

[0018] One of the above technical solutions has the following advantages or beneficial effects: by welding, a welded joint consisting of a weld formed by melting stainless steel-copper and a weld formed by heat conduction of copper-nickel and nickel-titanium alloy is formed. The presence of incompletely melted nickel foil in the joint effectively hinders the diffusion and combination of Fe and Ti elements, inhibits the generation of Ti-Fe binary brittle phase, reduces the brittleness of the joint, and improves the mechanical properties of the joint. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 A schematic diagram of the material placement sequence, welding structure and welding process provided in an embodiment of the present invention;

[0020] Figure 2 The microstructure morphology of the cross section of the titanium alloy-stainless steel weld of the present invention is as follows: (a) a low-magnification photograph of the cross section of a stainless steel-copper-nickel-titanium alloy weld, (b) a high-magnification photograph of the central area of ​​the cross section of a stainless steel-copper-nickel-titanium alloy weld near the stainless steel side, (c) a high-magnification photograph of the central area of ​​the cross section of a stainless steel-copper-nickel-titanium alloy weld near the titanium alloy side;

[0021] Figure 3 It is a schematic diagram of the preparation process of the titanium alloy-stainless steel welded joint of the present invention.

[0022] The marks in the above figures are: 1. stainless steel plate, 2. Cu, Ni foil composite intermediate layer, 3. titanium alloy plate, 4. clamping plate, 5. fastening nut, 6. bottom plate. DETAILED DESCRIPTION

[0023] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0024] Embodiment 1

[0025] See also Figures 1 to 3, a titanium steel with a Ni-Cu composite intermediate foil layer added, the materials are overlapped and placed in the order of stainless steel, copper foil, nickel foil, and titanium alloy from top to bottom, and the overlapping areas are welded to fuse the materials. After the materials are placed, they are clamped with a clamp to maintain a pressing force between the materials. The present invention addresses the problem of a large number of Ti-Fe binary brittle phases in titanium / steel dissimilar joints. A laser beam is used as a welding heat source, copper foil and nickel foil are superimposed as a composite intermediate layer material, and the welding structure is overlapped. By adjusting and optimizing the welding process parameters, a stainless steel-copper-nickel-titanium alloy welded joint is obtained. Since the melting point of metallic nickel is relatively high, and it will effectively hinder the diffusion of the parent material elements on both sides, the formation of Ti-Fe binary brittle phases in the joint is avoided, and at the same time, the Cu element is hindered from diffusing downward and combining with the Ti element to produce the Cu-Ti binary brittle phase, thereby greatly improving the mechanical properties of the joint.

[0026] The fixture has a bottom plate 6, on which stainless steel, copper foil, nickel foil and titanium alloy are placed in sequence; clamping plates 4 are provided on both sides of the bottom plate 6, which are connected to the bottom plate 6 by fastening nuts 5, and the clamping plates 4 can clamp the materials. The nuts are adjusted to maintain a certain clamping force between the contact surface of the welding base material and the intermediate layer material.

[0027] The copper foil is 0.05mm thick and the nickel foil is 0.3mm thick. When placing them, ensure that all materials are flat and there is no gap visible on the contact surface.

[0028] The above-mentioned titanium steel processing method with added Ni-Cu composite intermediate foil layer adopts a welding process, and the welding adopts a high-efficiency ytterbium-doped fiber laser for welding. The high-efficiency ytterbium-doped fiber laser is used for welding, and the process parameters are optimized to improve the joint performance, with the goal of obtaining the best weld morphology, avoiding defects such as cracks, pinholes, and droplet splashes.

[0029] Before welding, the materials are pretreated. Sandpaper is used to grind the stainless steel and titanium alloy base materials to remove the oxide layer on the surface of the materials. Then, acetone is used to clean the stainless steel and titanium alloy base materials as well as the nickel and copper foils to remove the surface oil stains. Sandpaper with a mesh size of about 3000 is used for grinding. It is not advisable to apply too much pressure during grinding to avoid damaging the thickness and flatness of the plate.

[0030] During welding, the laser emission angle is adjusted to weld the overlapping areas to obtain a stainless steel-copper foil weld. The copper foil middle layer continues to conduct heat downward to form a copper foil-nickel foil weld and a nickel foil-titanium alloy weld.

[0031] During welding, the welding speed and laser power are adjusted so that the middle layer of the vanadium foil is not completely melted. After welding, a joint consisting of a weld formed by the melting of stainless steel-copper, copper-vanadium, an incompletely melted nickel foil and a weld formed by heat conduction of nickel-titanium alloy is obtained, eliminating the brittleness of the joint.

[0032] Iron and copper metals can form a solid solution phase in the liquid phase, and nickel and copper metals can be infinitely soluble in each other. At the same time, since the welding temperature exceeds the solid solution temperature of nickel and titanium metals, and the heat input of the laser welding process is concentrated and the cooling speed is fast, a partial nickel-titanium austenite phase can be formed in the weld area. The possible solid solution treatment will eliminate the supersaturated solid solution and precipitation phase in nickel-titanium to a certain extent, eliminating the brittleness of the joint.

[0033] The welding speed is 30mm / s, the laser power is 2900W-3100W, and the defocus is 0. The laser emission angle is 9°-12° with the material surface. The welding speed and laser power are adjusted to make the vanadium foil intermediate layer incompletely melted, thereby controlling the Fe and Ti elements in the stainless steel and titanium alloy base materials from diffusing with each other. In the composite intermediate layer, the Cu foil thickness is 0.05mm, and the Ni foil thickness is 0.3mm. The parameters such as the spatial position and thickness of the intermediate layer, the welding speed of 35mm / s, and the defocus of 0 are kept unchanged. The laser power range is adjusted to 2900W-3300W, and welding is performed every time 100W is increased. When the power is 2900W and 3000W, due to the low laser power and insufficient heat input, the welded joint is not fully penetrated or has poor mechanical properties; when the laser power is 3200W and 3300W, When the laser power is too high, the stress of the joint is too large, and cracks of varying degrees appear after the joint is cooled, resulting in poor mechanical properties of the joint. When the laser power is 3100W, there is basically no Ti-Fe and Ti-Cu binary brittle phases in the weld area, and the main phases are (Fe, Ni), (Cu, Ni), and (β-Ti, Ni) solid solutions. The brittleness of the joint is reduced. At the same time, since the copper foil has very good ductility and plasticity, the stress of the joint is relieved during the welding and cooling process, thereby significantly improving the mechanical properties.

[0034] Through welding, a welded joint consisting of a stainless steel-copper weld formed by melting, and a copper-nickel and nickel-titanium alloy weld formed by heat conduction is formed. The presence of incompletely melted nickel foil in the joint effectively hinders the diffusion and combination of Fe and Ti elements, inhibits the generation of Ti-Fe binary brittle phase, reduces the brittleness of the joint, and improves the mechanical properties of the joint.

[0035] The present invention significantly improves the mechanical properties of the titanium / steel dissimilar metal overlap laser welding joint by innovatively adding a copper-nickel composite intermediate layer and coordinating the titanium / steel dissimilar metal laser thermal welding with an overlap structure. Through the titanium / steel dissimilar metal laser thermal welding process with an overlap structure adding a copper-nickel composite intermediate layer, more solid solutions are formed in the joint during the welding process, and less intermetallic compounds are produced, thereby optimizing the structure in the titanium / steel dissimilar metal weld joint and improving the mechanical properties of the joint. This titanium / steel dissimilar metal laser thermal welding process with an overlap structure adding a copper-nickel composite intermediate layer is original in the field of dissimilar material welding (connection).

[0036] Beneficial effects:

[0037] (1) The stainless steel-titanium alloy laser lap welded joint prepared by the method of the present invention has good surface morphology, uniform weld, no defects such as cracks, pinholes, droplet splashing, and incomplete penetration, and has good welding process performance;

[0038] (2) Stainless steel-copper-nickel-titanium alloy is overlapped from top to bottom, and the stainless steel surface is irradiated with laser. Only one welding is required to obtain a welded joint under the action of heat conduction;

[0039] (3) Control the thickness of the composite intermediate layer respectively, hinder the mutual diffusion of Ti and Fe elements in the parent material, inhibit the generation of Ti-Fe binary brittle phase, reduce the brittleness of the joint, and improve the mechanical properties of the joint;

[0040] (4) During the welding process, most materials form solid solutions, and few intermetallic compounds are produced. The addition of copper foil makes the joint have better plasticity and ductility, reduces the brittleness of the joint, and improves the mechanical properties of the joint;

[0041] (5) The tensile strength of the composite welded joints consisting of welds formed by melting stainless steel and copper, and welds formed by heat conduction of copper-nickel and nickel-titanium alloys reaches 448 MPa.

[0042] Embodiment 2

[0043] See also Figures 1 to 3 The titanium / steel dissimilar metal laser lap welding process method with the addition of a Cu-Ni foil composite intermediate layer of the present invention is to solve the problem of a large amount of Ti-Fe binary brittle phase in the titanium / steel dissimilar joint. The laser beam is used as the welding heat source, and the Cu-Ni foil is superimposed as the composite intermediate layer material. Since the titanium alloy has a high reflectivity to laser, the stainless steel is placed on the top layer when designing the welding structure. At the same time, the Cu foil is placed on the Ni foil, thereby further avoiding the generation of the Cu-Ti binary brittle phase and further improving the mechanical properties. The specific steps are as follows:

[0044] (1) Pre-welding treatment: Before welding, use sandpaper to lightly grind the stainless steel and titanium alloy base materials to remove the surface oxide layer of the material, and then use acetone to clean the stainless steel and titanium alloy base materials as well as nickel and copper foil to remove surface oil stains;

[0045] (2) Welding structure: The welding base material and the intermediate layer material are overlapped and placed in the order of stainless steel, copper foil, nickel foil, and titanium alloy from top to bottom, and a special clamp is used to fix the placed materials, and the nut is adjusted to maintain a certain compression force between the contact surface of the welding base material and the intermediate layer material;

[0046] (3) Welding process: Use high-efficiency ytterbium-doped fiber laser for welding. The fiber laser emission angle is 9-12°, the laser power is 2900W-3300W, the welding speed is 35mm / s, and the defocus is 0. The joint performance is improved to obtain the optimal weld morphology and avoid defects such as cracks, pinholes, and droplet splashes.

[0047] Adjust the welding speed and laser power to prevent the vanadium foil middle layer from completely melting, thereby preventing the Fe and Ti elements in the stainless steel and titanium alloy base materials from diffusing with each other. In the composite middle layer, the thickness of the Cu foil is 0.05mm, and the thickness of the Ni foil is 0.3mm. Keep the spatial position and thickness of the middle layer, the welding speed of 35mm / s, and the defocus amount of 0 unchanged. Adjust the laser power range to 2900W-3300W, and weld once every 100W increase. When the power is 2900W and 3000W, the laser power is too low and the heat input is insufficient, so the welded joint is not fully penetrated or has poor mechanical properties; when the laser power is 3200W and 3300W, When the laser power is too high, the stress of the joint is too large, and cracks of varying degrees appear after the joint is cooled, resulting in poor mechanical properties of the joint. When the laser power is 3100W, there is basically no Ti-Fe and Ti-Cu binary brittle phases in the weld area, and the main phases are (Fe, Ni), (Cu, Ni), and (β-Ti, Ni) solid solutions. The brittleness of the joint is reduced. At the same time, since the copper foil has very good ductility and plasticity, the stress of the joint is relieved during the welding and cooling process, thereby significantly improving the mechanical properties.

[0048] The innovative use of adding a copper-nickel composite intermediate layer and cooperating with the titanium / steel dissimilar metal laser thermal welding of the overlap structure has greatly improved the mechanical properties of the titanium / steel dissimilar metal overlap laser welding joint. Through the titanium / steel dissimilar metal laser thermal welding process with an overlap structure adding a copper-nickel composite intermediate layer, more solid solutions are formed in the joint during the welding process, and less intermetallic compounds are produced, which optimizes the organization in the titanium / steel dissimilar metal welded joint and improves the mechanical properties of the joint. This titanium / steel dissimilar metal laser thermal welding process with an overlap structure adding a copper-nickel composite intermediate layer is original in the field of dissimilar material welding (connection).

[0049] The structure adopts the form of upper and lower overlap. The laser process uses laser thermal conduction welding. The process parameters are set, and the laser is controlled to directly irradiate the stainless steel surface. The weld formed by melting stainless steel-copper and the weld formed by heat conduction of copper-nickel and nickel-titanium alloy are prepared by heat conduction. The composite welding joints are composed of welds formed by heat conduction of stainless steel-copper. Since the nickel foil is thicker and there is a certain unmelted layer, and the copper foil is placed on the nickel foil when placing the middle layer, it has a good barrier effect on the mutual diffusion of Ti, Fe, Ti, and Cu elements in the joint, and largely avoids the formation of Ti-Fe and Ti-Cu binary brittle phases. In addition, the addition of copper foil can give full play to its advantages of good plasticity and ductility in the joint, so that the stress of the joint can be relieved during the cooling process, further improving the mechanical properties of the joint.

[0050] Beneficial effects:

[0051] Uniform, without defects such as cracks, pinholes, droplet splashing, incomplete penetration, etc., and good welding process performance;

[0052] (2) Stainless steel-copper-nickel-titanium alloy is overlapped from top to bottom, and the stainless steel surface is irradiated with laser. Only one welding is required to obtain a welded joint under the action of heat conduction;

[0053] (3) Control the thickness of the composite intermediate layer respectively, hinder the mutual diffusion of Ti and Fe elements in the parent material, inhibit the generation of Ti-Fe binary brittle phase, reduce the brittleness of the joint, and improve the mechanical properties of the joint;

[0054] (4) During the welding process, most materials form solid solutions, and few intermetallic compounds are produced. The addition of copper foil makes the joint have better plasticity and ductility, reduces the brittleness of the joint, and improves the mechanical properties of the joint;

[0055] (5) The tensile strength of the composite welded joints consisting of welds formed by melting stainless steel and copper, and welds formed by heat conduction of copper-nickel and nickel-titanium alloys reaches 448 MPa.

[0056] After adopting the above scheme, welding is performed to form a welded joint consisting of a weld formed by melting stainless steel and copper, and a weld formed by heat conduction of copper-nickel and nickel-titanium alloys. The presence of incompletely melted nickel foil in the joint effectively hinders the diffusion and combination of Fe and Ti elements, inhibits the generation of Ti-Fe binary brittle phase, reduces the brittleness of the joint, and improves the mechanical properties of the joint. A titanium steel with a Ni-Cu composite intermediate foil layer added, the materials are overlapped and placed in the order of stainless steel, copper foil, nickel foil, and titanium alloy from top to bottom, and the overlapping overlap area is welded to fuse the materials.

[0057] In the description of the present invention, it is necessary to understand that the terms "coaxial", "bottom", "one end", "top", "middle", "the other end", "upper", "one side", "top", "inside", "front", "center", "both ends" and the like indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present invention.

[0058] In the present invention, unless otherwise clearly stipulated and limited, the terms such as "installation", "setting", "connection", "fixation" and "screw-on" should be understood in a broad sense. For example, it can be a fixed connection, a detachable connection, or an integral one; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium; it can be the internal connection of two elements or the interaction relationship between two elements. Unless otherwise clearly defined, ordinary technicians in this field can understand the specific meanings of the above terms in the present invention according to the specific circumstances.

[0059] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A titanium steel with a Ni-Cu composite intermediate foil layer added, characterized in that: The materials are overlapped and placed in the order of stainless steel, copper foil, nickel foil and titanium alloy from top to bottom, and the overlapping areas are welded to fuse the materials.

2. The titanium steel with added Ni-Cu composite intermediate foil layer as claimed in claim 1, characterized in that: After the materials are placed, use clamps to clamp them to maintain compression between the materials.

3. The titanium steel with added Ni-Cu composite intermediate foil layer as claimed in claim 2, characterized in that: The fixture has a base plate, and the stainless steel, copper foil, nickel foil, and titanium alloy are placed on the base plate in sequence; clamping plates are provided on both sides of the base plate, and the clamping plates are connected to the base plate through fastening nuts, and the clamping plates can clamp the materials.

4. The titanium steel with added Ni-Cu composite intermediate foil layer as claimed in claim 3, characterized in that: The copper foil is 0.05 mm thick, and the nickel foil is 0.3 mm thick.

5. The method for processing titanium steel with a Ni-Cu composite intermediate foil layer added as claimed in any one of claims 1 to 3, characterized in that: The processing method adopts welding technology, and the welding adopts high-efficiency ytterbium-doped fiber laser for welding.

6. The titanium steel with added Ni-Cu composite intermediate foil layer as claimed in claim 5, characterized in that: The materials are pretreated before welding. The stainless steel and titanium alloy base materials are polished with sandpaper to remove the oxide layer on the surface of the materials. Then, the stainless steel and titanium alloy base materials as well as the nickel and copper foils are cleaned with acetone to remove surface oil stains.

7. The titanium steel with added Ni-Cu composite intermediate foil layer as claimed in claim 6, characterized in that: During welding, the laser emission angle is adjusted to weld the overlapping areas to obtain a stainless steel-copper foil weld. The copper foil middle layer continues to conduct heat downward to form a copper foil-nickel foil weld and a nickel foil-titanium alloy weld.

8. The titanium steel with added Ni-Cu composite intermediate foil layer as claimed in claim 7, characterized in that: During welding, the welding speed and laser power are adjusted so that the middle layer of the vanadium foil is not completely melted. After welding, a joint consisting of a weld formed by the melting of stainless steel-copper, copper-vanadium, an incompletely melted nickel foil and a weld formed by heat conduction of nickel-titanium alloy is obtained, eliminating the brittleness of the joint.

9. The titanium steel with added Ni-Cu composite intermediate foil layer as claimed in claim 8, characterized in that: The welding speed is 30mm / s, the laser power is 2900W-3100W, and the defocus is 0.

10. The titanium steel with added Ni-Cu composite intermediate foil layer as claimed in claim 9, characterized in that: The laser emission angle is 9°-12° to the material surface.

Citation Information

Patent Citations

  • Welding material for welding near-titanium layer of titanium-steel composite plate, and preparation method thereof

    CN106695173A

  • Stainless steel-tita nium alloy different metal laser welding method

    CN105855705A

  • Diffusion welding method of titanium alloy and dissimilar metal of stainless steel

    CN107030367A

  • Method for manufacturing metal-based composite material containing graphene interlayer

    CN108188668A

  • Preparation method of titanium-steel composite board

    CN108326516A

Cited By

  • Dissimilar metal sheet welding method for preparing middle layer based on laser cladding

    CN120587669A

  • A method for welding dissimilar metal thin plates based on laser cladding for preparing an intermediate layer

    CN120587669B

  • Method for joining two sheet steel parts and corresponding connection

    DE102025101411A1