High-flame-retardant environment-friendly cable
By using Zn-doped modified nanotitanium dioxide and calcium-aluminum composite fillers in cables, the problems of insufficient flame retardant performance and aging of traditional cables are solved, and efficient flame retardant effect and material stability are achieved, which significantly reduces fire hazards and the environment. pollute.
Patent Information
- Application Number
- CN202411364129.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-28
- Publication Date
- 2024-12-03
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Traditional cables produce toxic gases and smoke during combustion, which endanger human health and pollute the environment. Its flame retardant properties are limited, resulting in serious fire hazards, and the problems of material aging and cracking have not been effectively solved.
Zn-doped modified nanotitanium dioxide and calcium-aluminum composite filler is used to improve the flame retardant performance of the cable through compounding and catalytic action, and delay combustion through nano-effects and interface effects, while improving the ultraviolet protection ability of the material to prevent aging.
It significantly improves the flame retardant performance of the cable, delays combustion, reduces the release of toxic gases, enhances the overall strength and toughness of the material, reduces fire hazards, and delays the aging of the cable sheath.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of cables, and in particular to a highly flame-retardant and environmentally friendly cable and a preparation method thereof. Background Art
[0002] With the increasing global environmental awareness and the increasing safety requirements in the fields of construction, transportation, energy, etc., the environmental protection and flame retardancy of cable products have become the focus of the industry. Traditional cable materials often produce a large amount of toxic gases and smoke during the combustion process, which not only harms human health, but also causes serious pollution to the environment.
[0003] As an important carrier for power transmission and signal transmission, the performance of cables directly affects the safety and stability of the entire system. The flame retardant performance of traditional cables is limited. Once a fire occurs, the fire is likely to spread rapidly, increasing the degree of fire hazard. While considering the flame retardancy of cables, other properties of cable materials also need to be considered to expand their application level. Based on this, the present invention proposes a highly flame retardant and environmentally friendly cable and a preparation method thereof. Summary of the invention
[0004] The present invention provides a highly flame-retardant and environmentally friendly cable and a preparation method thereof, the purpose of which is to improve the flame-retardant properties of the cable material while effectively preventing the aging and cracking of the cable material.
[0005] The technical solution of the present invention is as follows: The invention provides a highly flame-retardant and environmentally friendly cable. The cable sheath is composed of the following raw materials in parts by weight: 45-55 parts of polyvinyl chloride, 15-20 parts of ethylene-vinyl acetate copolymer, 4-6 parts of Zn-doped modified nano titanium dioxide, 8-10 parts of calcium-aluminum composite filler, 4-6 parts of maleic anhydride grafted polyethylene, 0.4-0.6 parts of lubricant, and 0.5-1 parts of antioxidant.
[0006] As a further technical solution, the preparation method of the calcium-aluminum composite filler includes: ultrasonically dispersing nano-calcium carbonate in ethanol, adding an aluminate coupling agent when the temperature is controlled to 60-70°C, stirring for 20-30 minutes, adding aluminum hydroxide when heated to 75-85°C, continuing to stir for 60-80 minutes, and continuing to stir for 20-30 minutes after cooling to room temperature.
[0007] As a further technical solution, the weight ratio of the nano-calcium carbonate, ethanol, aluminate coupling agent and aluminum hydroxide is (30-40): (45-55): (0.15-0.2): (20-30).
[0008] As a further technical solution, the aluminate coupling agent is aluminate coupling agent DL2411.
[0009] Among them, the addition of aluminate coupling agent DL2411 can improve the dispersibility and compatibility of nano calcium carbonate and aluminum hydroxide in cable materials. This allows them to be more evenly distributed in the material, forming a more effective flame retardant network. In addition, the coupling agent may also enhance the interfacial bonding between the filler and the cable material matrix, improving the overall strength and toughness of the material.
[0010] As a further technical solution, the preparation method of the Zn-doped modified nano-titanium dioxide includes: after fully mixing tetrabutyl titanate and anhydrous ethanol, adding 0.5 mol / L nitric acid to adjust the pH to 2-3 to obtain a mixed solution A, slowly adding Zn (NO3) 3 solution to the mixed solution A at a rate of 2 seconds / drop, stirring for 80-100 minutes to obtain a transparent colloid, aging for 20-24 hours, and drying at a temperature of 70-80°C to obtain a solid, grinding, and then placing it in a muffle furnace at a temperature of 300-340°C for calcination for 3-4 hours.
[0011] As a further technical solution, the volume ratio of tetrabutyl titanate and anhydrous ethanol is 1:(2-3).
[0012] As a further technical solution, the concentration of the Zn(NO3)3 solution is 0.08-0.1 mol / L.
[0013] As a further technical solution, the antioxidant includes antioxidant 168 or antioxidant 2246.
[0014] As a further technical solution, the lubricant is polyethylene wax.
[0015] As a further technical solution, the preparation steps of the cable sheath include: weighing raw materials in proportion and mixing them, and sending the mixture into a twin-screw extruder for melt extrusion and granulation, wherein the screw speed is 500-520r / min, the temperature of the first zone of the extruder is 110-120°C, the temperature of the second zone is 125-135°C, and the head discharge temperature is 140-150°C.
[0016] The working principle and beneficial effects of the present invention are: 1. The present invention is compounded by Zn-doped modified nano titanium dioxide and calcium-aluminum composite filler, wherein nano calcium carbonate and aluminum hydroxide in the calcium-aluminum composite filler are both effective flame retardants; nano calcium carbonate will decompose at high temperature to produce flame retardant gases such as carbon dioxide and water vapor, which can dilute the combustible gas and reduce the temperature of the combustion area, and aluminum hydroxide will also decompose to produce water vapor and aluminum oxide, and aluminum oxide can form a dense carbon layer covering the surface of the cable material, isolating oxygen and heat, and further preventing combustion; and the catalytic effect of Zn-doped modified nano titanium dioxide can promote the decomposition of the flame retardant in the calcium-aluminum composite filler and the formation of the carbon layer. At the same time, the nano effect of nano titanium dioxide and the synergistic flame retardant effect of the calcium-aluminum composite filler are superimposed on each other, so that the flame retardant performance of the cable material is significantly improved.
[0017] 2. The present invention utilizes the addition of Zn-doped modified nano titanium dioxide to enhance the flame retardant effect, wherein nano titanium dioxide has a large specific surface area and a high surface energy due to its extremely small particle size; this makes it easier to interact with other components in the cable material to form a tighter bond; at the same time, the dispersion of nanoparticles in the material can form more interfaces, which can more effectively absorb and disperse energy when exposed to heat or fire, thereby delaying the combustion of the material.
[0018] 3. The present invention can change the crystal structure and electronic properties of nano-titanium dioxide by doping it with Zn. The introduction of Zn may form new energy levels or defects, and these changes help to improve the catalytic activity and stability of nano-titanium dioxide; in the flame retardant process, the modified nano-titanium dioxide may more effectively catalyze the decomposition of the flame retardant, produce more flame retardant gas or form a denser carbon layer, thereby improving the flame retardant properties of the cable material.
[0019] 4. The Zn-doped modified nano-titanium dioxide in the present invention has strong absorption and scattering effects on ultraviolet rays, which can effectively reduce the radiation damage of ultraviolet rays to cable materials. Zn doping may further enhance the ultraviolet protection ability, thereby delaying the aging of cable sheath materials. DETAILED DESCRIPTION
[0020] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0021] Example 1 In this embodiment, a highly flame-retardant and environmentally friendly cable is provided, wherein the cable sheath is composed of the following raw materials in parts by weight: 50 parts of polyvinyl chloride, 17 parts of ethylene-vinyl acetate copolymer, 5 parts of Zn-doped modified nano-titanium dioxide, 9 parts of calcium-aluminum composite filler, 5 parts of maleic anhydride grafted polyethylene, 0.5 parts of lubricant polyethylene wax, and 0.7 parts of antioxidant 168; Among them, the preparation method of Zn-doped modified nano titanium dioxide includes: fully mixing tetrabutyl titanate and anhydrous ethanol in a volume ratio of 1:2.5, adding 0.5 mol / L nitric acid to adjust the pH to 2.5 to obtain a mixed solution A, slowly adding a Zn(NO3)3 solution with a concentration of 0.09 mol / L to the mixed solution A at a rate of 2 seconds / drop, stirring for 90 minutes to obtain a transparent colloid, aging for 22 hours, and drying at a temperature of 75°C to obtain a solid, grinding, and then placing it in a muffle furnace at a temperature of 320°C for calcination for 3.5 hours.
[0022] The preparation method of the calcium-aluminum composite filler comprises: ultrasonically dispersing nano calcium carbonate in ethanol, adding aluminate coupling agent DL2411 when the temperature is controlled to be 65°C, stirring for 25 minutes, adding aluminum hydroxide when heated to 80°C, continuing to stir for 70 minutes, and continuing to stir for 25 minutes after cooling to room temperature; the weight ratio of nano calcium carbonate, ethanol, aluminate coupling agent and aluminum hydroxide is 35:50:0.17:25; The preparation steps of the cable sheath include: weighing raw materials in proportion and mixing them, and sending the mixture into a twin-screw extruder for melt extrusion and granulation, wherein the screw speed is 510r / min, the temperature of the first zone of the extruder is 115°C, the temperature of the second zone is 130°C, and the head discharge temperature is 145°C.
[0023] Example 2 The present embodiment provides a highly flame-retardant and environmentally friendly cable, wherein the cable sheath is composed of the following raw materials in parts by weight: 45 parts of polyvinyl chloride, 15 parts of ethylene-vinyl acetate copolymer, 4 parts of Zn-doped modified nano-titanium dioxide, 8 parts of calcium-aluminum composite filler, 4 parts of maleic anhydride grafted polyethylene, 0.4 parts of lubricant polyethylene wax, and 0.5 parts of antioxidant 2246; Among them, the preparation method of Zn-doped modified nano titanium dioxide includes: fully mixing tetrabutyl titanate and anhydrous ethanol in a volume ratio of 1:2, adding 0.5 mol / L nitric acid to adjust the pH to 2 to obtain a mixed solution A, slowly adding a Zn(NO3)3 solution with a concentration of 0.08 mol / L to the mixed solution A at a rate of 2 seconds / drop, stirring for 80 minutes to obtain a transparent colloid, aging for 20 hours, drying at a temperature of 70°C to obtain a solid, grinding, and then placing it in a muffle furnace at a temperature of 300°C for calcination for 3 hours.
[0024] The preparation method of the calcium-aluminum composite filler comprises: ultrasonically dispersing nano calcium carbonate in ethanol, adding aluminate coupling agent DL2411 when the temperature is controlled to be 60°C, stirring for 20 minutes, adding aluminum hydroxide when heated to 75°C, continuing to stir for 60 minutes, and continuing to stir for 20 minutes after cooling to room temperature; the weight ratio of nano calcium carbonate, ethanol, aluminate coupling agent and aluminum hydroxide is 30:45:0.15:20; The preparation steps of the cable sheath include: weighing raw materials in proportion and mixing them, and sending the mixture into a twin-screw extruder for melt extrusion and granulation, wherein the screw speed is 500r / min, the temperature of the first zone of the extruder is 110°C, the temperature of the second zone is 125°C, and the head discharge temperature is 140°C.
[0025] Example 3 The present embodiment provides a highly flame-retardant and environmentally friendly cable, wherein the cable sheath is composed of the following raw materials in parts by weight: 55 parts of polyvinyl chloride, 20 parts of ethylene-vinyl acetate copolymer, 6 parts of Zn-doped modified nano-titanium dioxide, 10 parts of calcium-aluminum composite filler, 6 parts of maleic anhydride grafted polyethylene, 0.6 parts of lubricant polyethylene wax, and 1 part of antioxidant 168; Among them, the preparation method of Zn-doped modified nano titanium dioxide includes: fully mixing tetrabutyl titanate and anhydrous ethanol in a volume ratio of 1:3, adding 0.5 mol / L nitric acid to adjust the pH to 3 to obtain a mixed solution A, slowly adding a 0.1 mol / L Zn(NO3)3 solution to the mixed solution A at a rate of 2 seconds / drop, stirring for 100 minutes to obtain a transparent colloid, aging for 24 hours, and drying at a temperature of 80°C to obtain a solid, grinding, and then placing it in a muffle furnace at a temperature of 340°C for calcination for 4 hours.
[0026] The preparation method of the calcium-aluminum composite filler comprises: ultrasonically dispersing nano calcium carbonate in ethanol, adding aluminate coupling agent DL2411 when the temperature is controlled to be 70°C, stirring for 30 minutes, adding aluminum hydroxide when heated to 85°C, continuing to stir for 80 minutes, and continuing to stir for 30 minutes after cooling to room temperature; the weight ratio of nano calcium carbonate, ethanol, aluminate coupling agent and aluminum hydroxide is 40:55:0.2:30; The preparation steps of the cable sheath include: weighing raw materials in proportion and mixing them, and sending the mixture into a twin-screw extruder for melt extrusion and granulation, wherein the screw speed is 520r / min, the temperature of the first zone of the extruder is 120°C, the temperature of the second zone is 135°C, and the head discharge temperature is 150°C.
[0027] Example 4 The present embodiment provides a highly flame-retardant and environmentally friendly cable, wherein the cable sheath is composed of the following raw materials in parts by weight: 45 parts of polyvinyl chloride, 20 parts of ethylene-vinyl acetate copolymer, 4 parts of Zn-doped modified nano-titanium dioxide, 10 parts of calcium-aluminum composite filler, 4 parts of maleic anhydride grafted polyethylene, 0.6 parts of lubricant polyethylene wax, and 0.5 parts of antioxidant 168; Among them, the preparation method of Zn-doped modified nano-titanium dioxide includes: fully mixing tetrabutyl titanate and anhydrous ethanol in a volume ratio of 1:2, adding 0.5 mol / L nitric acid to adjust the pH to 3 to obtain a mixed solution A, slowly adding a Zn(NO3)3 solution with a concentration of 0.08 mol / L to the mixed solution A at a rate of 2 seconds / drop, stirring for 100 minutes to obtain a transparent colloid, aging for 20 hours, drying at a temperature of 80°C to obtain a solid, grinding, and then placing it in a muffle furnace at a temperature of 300°C for calcination for 4 hours.
[0028] The preparation method of the calcium-aluminum composite filler comprises: ultrasonically dispersing nano calcium carbonate in ethanol, adding aluminate coupling agent DL2411 when the temperature is controlled to be 70°C, stirring for 20 minutes, adding aluminum hydroxide when heated to 85°C, continuing to stir for 60 minutes, and continuing to stir for 30 minutes after cooling to room temperature to obtain the composite filler; the weight ratio of nano calcium carbonate, ethanol, aluminate coupling agent and aluminum hydroxide is 30:55:0.15:30; The preparation steps of the cable sheath include: weighing raw materials in proportion and mixing them, and sending the mixture into a twin-screw extruder for melt extrusion and granulation, wherein the screw speed is 500r / min, the temperature of the first zone of the extruder is 120°C, the temperature of the second zone is 125°C, and the head discharge temperature is 150°C.
[0029] Comparative Example 1 In this comparative example, a highly flame-retardant and environmentally friendly cable is provided, wherein the cable sheath is composed of the following raw materials in parts by weight: 50 parts of polyvinyl chloride, 17 parts of ethylene-vinyl acetate copolymer, 5 parts of Ni-doped modified nano titanium dioxide, 9 parts of calcium-aluminum composite filler, 5 parts of maleic anhydride grafted polyethylene, 0.5 parts of lubricant polyethylene wax, and 0.7 parts of antioxidant 168; Among them, the preparation method of Ni-doped modified nano titanium dioxide includes: fully mixing tetrabutyl titanate and anhydrous ethanol in a volume ratio of 1:2.5, adding 0.5 mol / L nitric acid to adjust the pH to 2.5 to obtain a mixed solution A, slowly adding a Ni(NO3)3 solution with a concentration of 0.09 mol / L to the mixed solution A at a rate of 2 seconds / drop, stirring for 90 minutes to obtain a transparent colloid, aging for 22 hours, and drying at a temperature of 75°C to obtain a solid, grinding, and then placing it in a muffle furnace at a temperature of 320°C for calcination for 3.5 hours.
[0030] The preparation method of the calcium-aluminum composite filler comprises: ultrasonically dispersing nano calcium carbonate in ethanol, adding aluminate coupling agent DL2411 when the temperature is controlled to be 65°C, stirring for 25 minutes, adding aluminum hydroxide when heated to 80°C, continuing to stir for 70 minutes, and continuing to stir for 25 minutes after cooling to room temperature; the weight ratio of nano calcium carbonate, ethanol, aluminate coupling agent and aluminum hydroxide is 35:50:0.17:25; The preparation steps of the cable sheath include: weighing raw materials in proportion and mixing them, and sending the mixture into a twin-screw extruder for melt extrusion and granulation, wherein the screw speed is 510r / min, the temperature of the first zone of the extruder is 115°C, the temperature of the second zone is 130°C, and the head discharge temperature is 145°C.
[0031] Comparative Example 2 In this comparative example, a highly flame-retardant and environmentally friendly cable is provided, wherein the cable sheath is composed of the following raw materials in parts by weight: 50 parts of polyvinyl chloride, 17 parts of ethylene-vinyl acetate copolymer, 5 parts of nano titanium dioxide, 9 parts of calcium aluminum composite filler, 5 parts of maleic anhydride grafted polyethylene, 0.5 parts of lubricant polyethylene wax, and 0.7 parts of antioxidant 168; The preparation method of the calcium-aluminum composite filler comprises: ultrasonically dispersing nano calcium carbonate in ethanol, adding aluminate coupling agent DL2411 when the temperature is controlled to be 65°C, stirring for 25 minutes, adding aluminum hydroxide when heated to 80°C, continuing to stir for 70 minutes, and continuing to stir for 25 minutes after cooling to room temperature; the weight ratio of nano calcium carbonate, ethanol, aluminate coupling agent and aluminum hydroxide is 35:50:0.17:25; The preparation steps of the cable sheath include: weighing raw materials in proportion and mixing them, and sending the mixture into a twin-screw extruder for melt extrusion and granulation, wherein the screw speed is 510r / min, the temperature of the first zone of the extruder is 115°C, the temperature of the second zone is 130°C, and the head discharge temperature is 145°C.
[0032] Comparative Example 3 In this comparative example, a highly flame-retardant and environmentally friendly cable is provided, wherein the cable sheath is composed of the following raw materials in parts by weight: 50 parts of polyvinyl chloride, 17 parts of ethylene-vinyl acetate copolymer, 9 parts of calcium-aluminum composite filler, 5 parts of maleic anhydride grafted polyethylene, 0.5 parts of lubricant polyethylene wax, and 0.7 parts of antioxidant 168; The preparation method of the calcium-aluminum composite filler comprises: ultrasonically dispersing nano calcium carbonate in ethanol, adding aluminate coupling agent DL2411 when the temperature is controlled to be 65°C, stirring for 25 minutes, adding aluminum hydroxide when heated to 80°C, continuing to stir for 70 minutes, and continuing to stir for 25 minutes after cooling to room temperature; the weight ratio of nano calcium carbonate, ethanol, aluminate coupling agent and aluminum hydroxide is 35:50:0.17:25; The preparation steps of the cable sheath include: weighing raw materials in proportion and mixing them, and sending the mixture into a twin-screw extruder for melt extrusion and granulation, wherein the screw speed is 510r / min, the temperature of the first zone of the extruder is 115°C, the temperature of the second zone is 130°C, and the head discharge temperature is 145°C.
[0033] Comparative Example 4 In this comparative example, a highly flame-retardant and environmentally friendly cable is provided, wherein the cable sheath is composed of the following raw materials in parts by weight: 50 parts of polyvinyl chloride, 17 parts of ethylene-vinyl acetate copolymer, 5 parts of Zn-doped modified nano-titanium dioxide, 9 parts of calcium-aluminum composite filler, 5 parts of maleic anhydride grafted polyethylene, 0.5 parts of lubricant polyethylene wax, and 0.7 parts of antioxidant 168; Among them, the preparation method of Zn-doped modified nano titanium dioxide includes: fully mixing tetrabutyl titanate and anhydrous ethanol in a volume ratio of 1:2.5, adding 0.5 mol / L nitric acid to adjust the pH to 2.5 to obtain a mixed solution A, slowly adding a Zn(NO3)3 solution with a concentration of 0.09 mol / L to the mixed solution A at a rate of 2 seconds / drop, stirring for 90 minutes to obtain a transparent colloid, aging for 22 hours, and drying at a temperature of 75°C to obtain a solid, grinding, and then placing it in a muffle furnace at a temperature of 320°C for calcination for 3.5 hours.
[0034] The preparation method of the calcium-aluminum composite filler comprises: ultrasonically dispersing nano calcium carbonate in ethanol, adding silane coupling agent KH560 when the temperature is controlled to be 65°C, stirring for 25 minutes, adding aluminum hydroxide when heated to 80°C, continuing to stir for 70 minutes, and continuing to stir for 25 minutes after cooling to room temperature; the weight ratio of nano calcium carbonate, ethanol, aluminate coupling agent and aluminum hydroxide is 35:50:0.17:25; The preparation steps of the cable sheath include: weighing raw materials in proportion and mixing them, and sending the mixture into a twin-screw extruder for melt extrusion and granulation, wherein the screw speed is 510r / min, the temperature of the first zone of the extruder is 115°C, the temperature of the second zone is 130°C, and the head discharge temperature is 145°C.
[0035] Comparative Example 5 In this comparative example, a highly flame-retardant and environmentally friendly cable is provided, wherein the cable sheath is composed of the following raw materials in parts by weight: 50 parts of polyvinyl chloride, 17 parts of ethylene-vinyl acetate copolymer, 5 parts of Zn-doped modified nano titanium dioxide, 9 parts of calcium-based filler, 5 parts of maleic anhydride grafted polyethylene, 0.5 parts of lubricant polyethylene wax, and 0.7 parts of antioxidant 168; Among them, the preparation method of Zn-doped modified nano titanium dioxide includes: fully mixing tetrabutyl titanate and anhydrous ethanol in a volume ratio of 1:2.5, adding 0.5 mol / L nitric acid to adjust the pH to 2.5 to obtain a mixed solution A, slowly adding a Zn(NO3)3 solution with a concentration of 0.09 mol / L to the mixed solution A at a rate of 2 seconds / drop, stirring for 90 minutes to obtain a transparent colloid, aging for 22 hours, and drying at a temperature of 75°C to obtain a solid, grinding, and then placing it in a muffle furnace at a temperature of 320°C for calcination for 3.5 hours.
[0036] The preparation method of the calcium-based filler comprises: ultrasonically dispersing nano calcium carbonate in ethanol, adding aluminate coupling agent DL2411 when the temperature is controlled to be 65°C, stirring for 25 minutes, heating to 80°C, continuing to stir for 70 minutes, cooling to room temperature and continuing to stir for 25 minutes to obtain the filler; the weight ratio of nano calcium carbonate, ethanol and aluminate coupling agent is 35:50:0.17; The preparation steps of the cable sheath include: weighing raw materials in proportion and mixing them, and sending the mixture into a twin-screw extruder for melt extrusion and granulation, wherein the screw speed is 510r / min, the temperature of the first zone of the extruder is 115°C, the temperature of the second zone is 130°C, and the head discharge temperature is 145°C.
[0037] Comparative Example 6 In this comparative example, a highly flame-retardant and environmentally friendly cable is provided, wherein the cable sheath is composed of the following raw materials in parts by weight: 50 parts of polyvinyl chloride, 17 parts of ethylene-vinyl acetate copolymer, 5 parts of Zn-doped modified nano-titanium dioxide, 9 parts of calcium-aluminum composite filler, 5 parts of maleic anhydride grafted polyethylene, 0.5 parts of lubricant polyethylene wax, and 0.7 parts of antioxidant 168; Among them, the preparation method of Zn-doped modified nano titanium dioxide includes: fully mixing tetrabutyl titanate and anhydrous ethanol in a volume ratio of 1:2.5, adding 0.5 mol / L nitric acid to adjust the pH to 2.5 to obtain a mixed solution AA, slowly adding a Zn(NO3)3 solution with a concentration of 0.09 mol / L to the mixed solution A at a rate of 2 seconds / drop, stirring for 90 minutes to obtain a transparent colloid, aging for 22 hours, and drying at a temperature of 75°C to obtain a solid, grinding, and then placing it in a muffle furnace at a temperature of 320°C for calcination for 3.5 hours.
[0038] The preparation method of the calcium-aluminum composite filler comprises: ultrasonically dispersing nano calcium carbonate in ethanol, adding aluminate coupling agent DL2411 when the temperature is controlled to be 65°C, stirring for 25 minutes, adding magnesium hydroxide when heated to 80°C, continuing to stir for 70 minutes, and continuing to stir for 25 minutes after cooling to room temperature; the weight ratio of nano calcium carbonate, ethanol, aluminate coupling agent and magnesium hydroxide is 35:50:0.17:25; The preparation steps of the cable sheath include: weighing raw materials in proportion and mixing them, and sending the mixture into a twin-screw extruder for melt extrusion and granulation, wherein the screw speed is 510r / min, the temperature of the first zone of the extruder is 115°C, the temperature of the second zone is 130°C, and the head discharge temperature is 145°C.
[0039] Comparative Example 7 In this comparative example, a highly flame-retardant and environmentally friendly cable is provided, wherein the cable sheath is composed of the following raw materials in parts by weight: 50 parts of polyvinyl chloride, 17 parts of ethylene-vinyl acetate copolymer, 5 parts of Zn-doped modified nano titanium dioxide, 9 parts of aluminum-based filler, 5 parts of maleic anhydride grafted polyethylene, 0.5 parts of lubricant polyethylene wax, and 0.7 parts of antioxidant 168; Among them, the preparation method of Zn-doped modified nano titanium dioxide includes: fully mixing tetrabutyl titanate and anhydrous ethanol in a volume ratio of 1:2.5, adding 0.5 mol / L nitric acid to adjust the pH to 2.5 to obtain a mixed solution A, slowly adding a Zn(NO3)3 solution with a concentration of 0.09 mol / L to the mixed solution A at a rate of 2 seconds / drop, stirring for 90 minutes to obtain a transparent colloid, aging for 22 hours, and drying at a temperature of 75°C to obtain a solid, grinding, and then placing it in a muffle furnace at a temperature of 320°C for calcination for 3.5 hours.
[0040] The preparation method of the aluminum-based filler comprises: adding aluminate coupling agent DL2411 to ethanol at a controlled temperature of 65°C, stirring for 25 minutes, adding aluminum hydroxide when heated to 80°C, continuing to stir for 70 minutes, and continuing to stir for 25 minutes after cooling to room temperature; the weight ratio of ethanol, aluminate coupling agent and aluminum hydroxide is 50:0.17:25; The preparation steps of the cable sheath include: weighing raw materials in proportion and mixing them, and sending the mixture into a twin-screw extruder for melt extrusion and granulation, wherein the screw speed is 510r / min, the temperature of the first zone of the extruder is 115°C, the temperature of the second zone is 130°C, and the head discharge temperature is 145°C.
[0041] Comparative Example 8 In this comparative example, a highly flame-retardant and environmentally friendly cable is provided, wherein the cable sheath is composed of the following raw materials in parts by weight: 50 parts of polyvinyl chloride, 17 parts of ethylene-vinyl acetate copolymer, 5 parts of Zn-doped modified nano titanium dioxide, 5 parts of maleic anhydride grafted polyethylene, 0.5 parts of lubricant polyethylene wax, and 0.7 parts of antioxidant 168; Among them, the preparation method of Zn-doped modified nano titanium dioxide includes: fully mixing tetrabutyl titanate and anhydrous ethanol in a volume ratio of 1:2.5, adding 0.5 mol / L nitric acid to adjust the pH to 2.5 to obtain a mixed solution A, slowly adding a Zn(NO3)3 solution with a concentration of 0.09 mol / L to the mixed solution A at a rate of 2 seconds / drop, stirring for 90 minutes to obtain a transparent colloid, aging for 22 hours, and drying at a temperature of 75°C to obtain a solid, grinding, and then placing it in a muffle furnace at a temperature of 320°C for calcination for 3.5 hours.
[0042] The preparation steps of the cable sheath include: weighing raw materials in proportion and mixing them, and sending the mixture into a twin-screw extruder for melt extrusion and granulation, wherein the screw speed is 510r / min, the temperature of the first zone of the extruder is 115°C, the temperature of the second zone is 130°C, and the head discharge temperature is 145°C.
[0043] Test Example 1: The cable sheath materials prepared in the above-mentioned Examples 1-4 and Comparative Examples 1-8 were tested as follows: Oxygen index: Determine the oxygen index according to GB / T 2406.2-2009; Tensile strength: tensile strength was measured according to GB / T32129-2015; aging conditions: 100℃×48h; Salt resistance: The test temperature is 25℃. Soak the protective layer in 4g / L sodium chloride solution for one month and observe whether the surface is bubbling or damaged. The test results are shown in Table 1 below: Table 1
[0044] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A highly flame-retardant and environmentally friendly cable, It is characterized in that The cable sheath is composed of the following raw materials in parts by weight: 45-55 parts of polyvinyl chloride, 15-20 parts of ethylene-vinyl acetate copolymer, 4-6 parts of Zn-doped modified nano titanium dioxide, 8-10 parts of calcium-aluminum composite filler, 4-6 parts of maleic anhydride grafted polyethylene, 0.4-0.6 parts of lubricant, and 0.5-1 parts of antioxidant.
2. A highly flame-retardant and environmentally friendly cable according to claim 1, It is characterized in that The preparation method of the calcium aluminum composite filler comprises: ultrasonically dispersing nano calcium carbonate in ethanol, adding an aluminate coupling agent when the temperature is controlled to be 60-70° C., stirring for 20-30 minutes, adding aluminum hydroxide when heated to 75-85° C., continuing to stir for 60-80 minutes, and continuing to stir for 20-30 minutes after cooling to room temperature.
3. A highly flame-retardant and environmentally friendly cable according to claim 2, It is characterized in that The weight ratio of the nano calcium carbonate, ethanol, aluminate coupling agent and aluminum hydroxide is (30-40): (45-55): (0.15-0.2): (20-30).
4. A highly flame-retardant and environmentally friendly cable according to claim 2, It is characterized in that The aluminate coupling agent is aluminate coupling agent DL2411.
5. A highly flame-retardant and environmentally friendly cable according to claim 1, It is characterized in that The preparation method of Zn-doped modified nano titanium dioxide comprises: after tetrabutyl titanate and anhydrous ethanol are fully mixed, 0.5 mol / L nitric acid is added to adjust the pH to 2-3 to obtain a mixed solution A, and Zn (NO) is slowly added to the mixed solution A at a speed of 2 seconds per drop. 3 ) 3 The solution is stirred for 80-100 minutes to obtain a transparent colloid, which is aged for 20-24 hours and then dried at 70-80°C to obtain a solid, which is then ground and calcined in a muffle furnace at 300-340°C for 3-4 hours.
6. A highly flame-retardant and environmentally friendly cable according to claim 5, It is characterized in that The volume ratio of tetrabutyl titanate to anhydrous ethanol is 1:(2-3).
7. A highly flame-retardant and environmentally friendly cable according to claim 5, It is characterized in that The Zn(NO 3 ) 3 The concentration of the solution is 0.08-0.1 mol / L.
8. A highly flame-retardant and environmentally friendly cable according to claim 1, It is characterized in that The antioxidant includes antioxidant 168 or antioxidant 2246.
9. A highly flame-retardant and environmentally friendly cable according to claim 1, It is characterized in that The lubricant is polyethylene wax.
10. A highly flame-retardant and environmentally friendly cable according to claim 1, It is characterized in that The preparation steps of the cable sheath include: weighing raw materials according to a proportion and mixing them, and sending the mixed materials into a twin-screw extruder for melt extrusion and granulation, wherein the screw speed is 500-520r / min, the temperature of the first zone of the extruder is 110-120°C, the temperature of the second zone is 125-135°C, and the head discharge temperature is 140-150°C.
Citation Information
Cited By
Environment-friendly insulated cable material and preparation method thereof
CN120173383A