High-thermal-conductivity sample disc for liquid chromatography and preparation method of high-thermal-conductivity sample disc

By using modified thermal conductivity fillers and styrene-maleic anhydride copolymer in the sample plate of the liquid chromatograph, the thermal conductivity and toughness of the PTFE material are improved, and the problem of uneven temperature of the sample plate is solved, achieving more accurate and reliable test results.

CN119060478AInactive Publication Date: 2024-12-03ZHEJIANG UNIV +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411393984.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-08
Publication Date
2024-12-03
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing liquid chromatograph sample disks have insufficient thermal conductivity of PTFE materials used, resulting in uneven temperature in the sample chamber, which affects the accuracy of the detection results.

Method used

By adding modified thermally conductive filler to PTFE materials, and improving the compatibility and interface contact area between fillers and resins through free radical copolymerization and secondary polymerization technology, the toughness of the material is increased by combining styrene-maleic anhydride copolymer, preparation Extract a sample plate for high thermal conductivity liquid chromatography.

Benefits of technology

It effectively reduces the interface thermal resistance of the sample disk, improves thermal conductivity and impact strength, ensures the consistency of sample storage temperature and the accuracy of detection results, and controls the temperature fluctuation within 5℃.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses a high-thermal-conductivity sample disc for liquid chromatography and a preparation method of the high-thermal-conductivity sample disc. The sample disc is made of a PTFE (Polytetrafluoroethylene) material. The PTFE material is prepared from the following raw materials in percentage by mass: 70 to 80 percent of PTFE dispersion resin and 10 to 30 percent of modified heat-conducting filler, the modified heat-conducting filler is prepared from the following raw materials in parts by mass: 10 parts of heat-conducting filler, 5 to 12 parts of PTFE (Polytetrafluoroethylene) emulsion, 15 to 25 parts of fluorine-containing acrylate monomer and 13 to 18 parts of methyl methacrylate. The PTFE sample disc for the liquid chromatography, which has outstanding heat-conducting property, has the characteristics of good chemical reagent resistance, corrosion resistance, insulation and heat conduction, is suitable for automatic sample injection of various samples, and can effectively reduce the temperature difference of different sample injection ports and improve the accuracy and reliability of a detection result.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of liquid chromatograph accessories, and in particular to a sample tray for high thermal conductivity liquid chromatography and a preparation method thereof. Background Art

[0002] The automation level of liquid chromatographs used for scientific research and analysis is constantly improving, especially in the injection system. The application of automatic sample injectors has significantly improved the detection efficiency and accuracy, and effectively solved many drawbacks of traditional manual injection, such as inconsistent injection volume, low efficiency and operation errors. It is particularly noteworthy that by integrating the sample chamber temperature control function, the automatic sample injector can meet the processing requirements of temperature-sensitive samples, which is crucial to maintaining sample stability and ensuring the accuracy of analysis results.

[0003] However, this temperature control technology has encountered challenges in practical applications. Specifically, in the actual operation of high-end liquid chromatographs, it was found that the temperature in the sample chamber was uneven, and the temperature fluctuation range of different sample ports reached 8°C to 11°C, far exceeding the set temperature control requirement of 5°C. Analysis found that the root cause of this phenomenon lies in the limitations of the sample plate material. The commonly used PTFE (polytetrafluoroethylene) material, although widely selected due to its excellent chemical stability and corrosion resistance, also sacrificed good thermal conductivity, which in turn affected the consistency of sample storage conditions and the reliability of test results. Summary of the invention

[0004] In order to solve the problem that the thermal conductivity of the current sample tray is low and affects the accuracy of the sample detection results, the present application provides a high thermal conductivity sample tray for liquid chromatography and a preparation method thereof.

[0005] In a first aspect, the present application provides a sample plate for high thermal conductivity liquid chromatography, which is made of PTFE material; the raw materials of the PTFE material include, in terms of mass percentage: 70-80% PTFE dispersed resin and 10-30% modified thermal conductive filler; the modified thermal conductive filler includes the following raw materials in parts by mass: 10 parts of thermal conductive filler, 5-12 parts of PTFE emulsion, 15-25 parts of fluorine-containing acrylate monomer, and 13-18 parts of methyl methacrylate.

[0006] Preferably, the modified thermally conductive filler comprises 9 to 16 parts by mass of sulfonate acrylic acid monomer.

[0007] Preferably, the method for preparing the modified thermally conductive filler comprises the following steps: Add thermal conductive filler, 50-70wt% fluorinated acrylate monomer, 40-60wt% methyl methacrylate, and 30-50wt% sulfonate acrylic monomer to the emulsifier solution, stir evenly, add initiator, heat up for primary polymerization, and obtain a premixed solution; The PTFE emulsion and the premixed liquid are mixed evenly, the remaining fluorinated acrylate monomer, methyl methacrylate and sulfonate acrylate monomer are added, the initiator is added after stirring evenly, the temperature is raised for secondary polymerization, the temperature is lowered, separation and filtration are performed, washing and drying are performed, and a modified thermal conductive filler is obtained; Preferably, the temperature of the primary polymerization and the secondary polymerization is 65-75°C.

[0008] Preferably, the initiator is selected from one or more of benzoyl peroxide, potassium persulfate, sodium persulfate, and ammonium persulfate.

[0009] In order to improve the thermal conductivity of the PTFE sample tray, improve the consistency of the sample storage temperature and the accuracy of the test results, the present application adds a large amount of thermally conductive fillers to the PTFE resin substrate in order to improve its thermal conductivity. It should be noted that in order to improve the compatibility of the thermally conductive filler with the non-polar PTFE resin, the present application pre-treats the filler on the surface. Specifically, firstly, through free radical copolymerization, the fluorinated acrylate monomer, methyl methacrylate and sulfonate acrylic monomer are in situ polymerized on the surface of the thermally conductive filler. On the one hand, it can significantly improve the compatibility of the thermally conductive filler with the PTFE material and increase the interfacial force; on the other hand, it can increase the steric hindrance and charge density on the surface of the filler, which helps to disperse the filler, inhibit agglomeration, and form a good thermal conductive path in the resin.

[0010] However, the thermal conductive filler obtained by the primary polymerization still has the problem of weak contact interface bonding with the resin and large interface thermal resistance. To overcome this problem, the present application mixes the thermal conductive filler modified by the primary polymerization with the PTFE emulsion to form mixed emulsion particles, and performs secondary graft polymerization on the surface of the mixed emulsion particles. The modified thermal conductive filler obtained by the secondary polymerization has a multi-core core layer of PTFE and thermal conductive filler composite, and a shell layer of fluorine-containing acrylate polymer, which further improves the compatibility while effectively increasing the interface contact area between the thermal conductive filler and PTFE, reducing the thermal resistance of the interface layer, and improving the thermal conductivity and strength properties of the material.

[0011] Preferably, the emulsifier solution is obtained by mixing a nonionic surfactant, carboxymethyl cellulose, calcium carbonate and water in a mass ratio of 2 to 4:1 to 3:0.5 to 1.5:100.

[0012] The emulsifier solution helps to promote the effective suspension of the mixed emulsion particles and ensure the effective grafting modification of the two polymerizations. Specifically, the nonionic surfactant forms a protective layer on the particle surface through surface adsorption to reduce agglomeration; carboxymethyl cellulose can increase the viscosity of the emulsion, exert a stronger support effect on the mixed emulsion particles, and inhibit sedimentation; and calcium carbonate can act as a physical barrier to increase the steric hindrance between particles, further hindering particle aggregation. Through the synergistic cooperation of the three, the stable suspension of the thermal conductive filler and its composite emulsion with PTFE emulsion is achieved, ensuring the progress of the polymerization modification reaction.

[0013] It should be noted that the participation of methyl methacrylate and sulfonate acrylic acid monomer in the modification reaction helps to promote the dispersion of the thermal conductive filler in the PTFE emulsion.

[0014] Preferably, the sulfonate acrylic acid monomer is selected from one or more of sodium allyl sulfonate, sodium 2-propylene sulfonate, and sodium methyl propylene sulfonate.

[0015] Preferably, the fluorine-containing acrylate monomer is selected from one or more of perfluoroalkylethyl methacrylate, trifluoroethyl methacrylate, and perfluoroalkyl acrylate.

[0016] Preferably, the thermally conductive filler includes one or more of aluminum oxide, zinc oxide, aluminum nitride, boron nitride, silicon carbide, and graphite.

[0017] The above-mentioned thermally conductive filler has both good insulation properties and thermal conductivity.

[0018] Preferably, the raw material of the PTFE material also includes 5-10% styrene-maleic anhydride copolymer.

[0019] The addition of a large amount of thermally conductive fillers, while improving the thermal conductivity of PTFE materials, also significantly increases the rigidity and brittleness of the materials, which is not conducive to ensuring the impact strength of the product. To this end, the present application adds an appropriate amount of styrene-maleic anhydride copolymer, which helps to compensate for the toughness of the material and improves the impact strength of the product.

[0020] In a second aspect, the present application provides a method for preparing a sample disk for high thermal conductivity liquid chromatography, comprising the following steps: Mixing: Add the modified thermal conductive filler into a mixing container, add PTFE dispersion resin and lubricant, and mix evenly to obtain PTFE material; Preforming: Put the PTFE material into the mold and make the preform by cold pressing; Sintering: sinter the preform at 370-390℃, and grind it after cooling; Preferably, the amount of the lubricant is 5-10% of the PTFE dispersed resin; Preferably, the lubricant is selected from silicone oil, mineral oil or paraffin oil.

[0021] Preferably, in the mixing step, 5 to 10% of the mass of the raw materials is added with styrene-maleic anhydride copolymer.

[0022] In summary, this application has the following beneficial effects: By adding a thermally conductive filler mixed with PTFE emulsion and subjected to secondary polymerization into the PTFE resin, the compatibility of the thermally conductive filler with the resin is improved and its full dispersion is promoted, while the interfacial thermal resistance of the thermally conductive filler and the resin is effectively reduced, giving full play to the thermal conductivity of the filler. The application of this material in the preparation of the sample tray of the automatic sampler helps to improve the consistency of the sample storage temperature, thereby improving the accuracy and reliability of the liquid chromatography test results. The test shows that the thermal conductivity of the PTFE material with the above-mentioned thermally conductive filler is greater than 7.0 W / (m•K); at the same time, when the sample tray is used for liquid chromatography detection, the temperature fluctuation of each sample port can be controlled within 5°C. DETAILED DESCRIPTION Preparation Example

[0023] Preparation Example 1 The modified thermal conductive filler is prepared according to the following steps: Preparation of emulsion: 28g nonionic surfactant, 12g carboxymethyl cellulose and 10g calcium carbonate were added into 1000g water and stirred evenly to obtain an emulsifier solution for use. The nonionic surfactant was Span 60 and the calcium carbonate particle size was 1250 mesh.

[0024] Primary polymerization: add 100g of aluminum oxide (D50 particle size is 40 microns), 120g of trifluoroethyl methacrylate, 70g of methyl methacrylate, and 50g of sodium methyl methacrylate sulfonate to the emulsifier solution, stir evenly, add 2g of benzoyl peroxide, heat to 65°C for primary polymerization, and react for 3h to obtain a premixed solution.

[0025] Secondary polymerization: Mix 100g PTFE emulsion and premix evenly, add the remaining 80g trifluoroethyl methacrylate, 70g methyl methacrylate and 60g sodium methyl methacrylate sulfonate, stir evenly, add 2.2g benzoyl peroxide, heat to 65°C for secondary polymerization, react for 2h, cool, centrifuge, filter, wash with deionized water, and dry to obtain a modified thermal conductive filler.

[0026] Preparation Example 2 The modified thermal conductive filler is prepared according to the following steps: Preparation of emulsion: 20g nonionic surfactant, 25g carboxymethyl cellulose and 5g calcium carbonate were added into 1000g water and stirred evenly to obtain an emulsifier solution for use. The nonionic surfactant was Span 60 and the calcium carbonate particle size was 1250 mesh.

[0027] Primary polymerization: add 100g of aluminum oxide (D50 particle size is 40 microns), 75g of trifluoroethyl methacrylate, 55g of methyl methacrylate, and 35g of sodium methacrylate sulfonate to the emulsifier solution, stir evenly, add 1.6g of benzoyl peroxide, heat to 70°C for primary polymerization, and react for 3h to obtain a premixed solution.

[0028] Secondary polymerization: Mix 60g of PTFE emulsion and the premixed liquid evenly, add the remaining 75g of trifluoroethyl methacrylate, 75g of methyl methacrylate and 55g of sodium methacrylate sulfonate, stir evenly, add 2g of benzoyl peroxide, heat to 70°C for secondary polymerization, react for 2h, cool, centrifuge, filter, wash with deionized water, and dry to obtain a modified thermal conductive filler.

[0029] Preparation Example 3 The modified thermal conductive filler is prepared according to the following steps: Preparation of emulsion: 35g nonionic surfactant, 10g carboxymethyl cellulose and 10g calcium carbonate were added into 1000g water and stirred evenly to obtain an emulsifier solution for use. The nonionic surfactant was Span 60 and the calcium carbonate particle size was 1250 mesh.

[0030] Primary polymerization: add 100g of aluminum oxide (D50 particle size is 40 microns), 150g of trifluoroethyl methacrylate, 90g of methyl methacrylate, and 80g of sodium methyl methacrylate sulfonate to the emulsifier solution, stir evenly, add 3.5g of benzoyl peroxide, heat to 65°C for primary polymerization, and react for 3h to obtain a premixed solution.

[0031] Secondary polymerization: 120g PTFE emulsion was mixed evenly with the premixed liquid, and the remaining 100g trifluoroethyl methacrylate, 90g methyl methacrylate and 80g sodium methacrylate sulfonate were added, and 3g benzoyl peroxide was added after stirring, and the temperature was raised to 65°C for secondary polymerization, and the reaction was carried out for 3h. The mixture was cooled, centrifuged, filtered, washed with deionized water, and dried to obtain a modified thermal conductive filler.

[0032] Preparation Example 4 The modified thermal conductive filler, in which no sulfonate acrylic acid monomer is added to the raw materials, has the following specific preparation steps: Preparation of emulsion: 28g nonionic surfactant, 12g carboxymethyl cellulose and 10g calcium carbonate were added into 1000g water and stirred evenly to obtain an emulsifier solution for use. The nonionic surfactant was Span 60 and the calcium carbonate particle size was 1250 mesh.

[0033] Primary polymerization: add 100g of aluminum oxide (D50 particle size is 40 microns), 130g of trifluoroethyl methacrylate, and 80g of methyl methacrylate to the emulsifier solution, stir evenly, add 2g of benzoyl peroxide, heat to 65°C for primary polymerization, and react for 3h to obtain a premixed solution.

[0034] Secondary polymerization: Mix 100g PTFE emulsion and premix evenly, add the remaining 90g trifluoroethyl methacrylate and 80g methyl methacrylate, stir evenly, add 1.7g benzoyl peroxide, heat to 65°C for secondary polymerization, react for 2h, cool, centrifuge, filter, wash with deionized water, and dry to obtain a modified thermal conductive filler.

[0035] Preparation Example 5 The modified thermal conductive filler is different from Preparation Example 1 in that no polymerization is performed. The specific preparation steps are as follows: Preparation of emulsion: 28g nonionic surfactant, 12g carboxymethyl cellulose and 10g calcium carbonate were added into 1000g water and stirred evenly to obtain an emulsifier solution for use. The nonionic surfactant was Span 60 and the calcium carbonate particle size was 1250 mesh.

[0036] Premixing: Add 100 g of alumina (D50 particle size: 40 μm) into the emulsifier solution, stir evenly, heat to 65°C for primary polymerization, and react for 3 hours to obtain a premixed solution.

[0037] Polymerization: Mix 100g PTFE emulsion and premix evenly, add 200g trifluoroethyl methacrylate, 140g methyl methacrylate and 110g sodium methyl methacrylate sulfonate, stir evenly, add 4.2g benzoyl peroxide, heat to 65°C for polymerization, react for 5h, cool, centrifuge, filter, wash with deionized water, and dry to obtain a modified thermal conductive filler.

[0038] Preparation Example 6 The modified thermally conductive filler is different from Preparation Example 1 in that, in the emulsion preparation step, the carboxymethyl cellulose is replaced by an equal amount of nonionic surfactant.

[0039] Preparation Example 7 The modified thermally conductive filler is different from Preparation Example 1 in that in the emulsion preparation step, calcium carbonate is replaced by an equal amount of nonionic surfactant.

[0040] Preparation Example 8 The modified thermal conductive filler is different from Preparation Example 1 in that no PTFE emulsion is added in the secondary polymerization step. The specific preparation operation is as follows: Add the remaining 80g of trifluoroethyl methacrylate, 70g of methyl methacrylate and 60g of sodium methyl propylene sulfonate to the premixed liquid, stir evenly, add 2.2g of benzoyl peroxide, heat to 65°C for secondary polymerization, react for 2h, cool, centrifuge, filter, wash with deionized water, and dry to obtain a modified thermal conductive filler.

[0041] Preparation Example 9 The modified thermally conductive filler is different from that of Preparation Example 1 in that in the first polymerization and the second polymerization steps, trifluoroethyl methacrylate is replaced by an equal amount of sodium methacrylic acid sulfonate. Example

[0042] Example Raw material selection: PTFE dispersion resin is Japan Daikin F-201 polytetrafluoroethylene dispersion resin; styrene-maleic anhydride copolymer model is Kumho Rili HSG5415; lubricant is No. 5 white mineral oil.

[0043] Example 1

[0044] A high thermal conductivity liquid chromatography sample plate is prepared according to the following steps: Mixing: 2.15 kg of the modified thermally conductive filler of Preparation Example 1 is added into a mixing container, and then 7 kg of PTFE dispersion resin, 0.85 kg of styrene-maleic anhydride copolymer and 0.6 kg of lubricant are added, and mixed evenly to obtain a PTFE material.

[0045] Preforming: The PTFE material is placed in a sample tray mold and cold-pressed at 40°C and 60MPa to obtain a preform.

[0046] Sintering: sinter the preform at 380-390℃, take it out after 10 hours and cool it at room temperature, then grind and modify it.

[0047] Example 2

[0048] A high thermal conductivity liquid chromatography sample plate is prepared according to the following steps: Mixing: 1.6 kg of the modified thermally conductive filler of Preparation Example 2 is added into a mixing container, and then 7.8 kg of PTFE dispersion resin, 0.6 kg of styrene-maleic anhydride copolymer and 0.7 kg of lubricant are added, and mixed evenly to obtain a PTFE material.

[0049] Preforming: The PTFE material is placed in a sample tray mold and cold-pressed at 50°C and 55MPa to obtain a preform.

[0050] Sintering: sinter the preform at 380-390℃, take it out after 10 hours and cool it at room temperature, then grind and modify it.

[0051] Example 3

[0052] A high thermal conductivity liquid chromatography sample plate is prepared according to the following steps: Mixing: 2.4 kg of the modified thermally conductive filler of Preparation Example 3 is added into a mixing container, and then 7.1 kg of PTFE dispersion resin, 0.5 kg of styrene-maleic anhydride copolymer and 0.5 kg of lubricant are added, and mixed evenly to obtain a PTFE material.

[0053] Preforming: The PTFE material is placed in a sample tray mold and cold-pressed at 40°C and 60MPa to obtain a preform.

[0054] Sintering: sinter the preform at 380-390℃, take it out after 10 hours and cool it at room temperature, then grind and modify it.

[0055] Example 4

[0056] A sample plate for high thermal conductivity liquid chromatography, which differs from Example 1 in that the modified thermal conductive filler of Preparation Example 1 is replaced by an equal amount of the modified thermal conductive filler of Preparation Example 4.

[0057] Example 5

[0058] A sample plate for high thermal conductivity liquid chromatography, which differs from Example 1 in that the modified thermal conductive filler of Preparation Example 1 is replaced by an equal amount of the modified thermal conductive filler of Preparation Example 5.

[0059] Example 6

[0060] A sample plate for high thermal conductivity liquid chromatography, which differs from Example 1 in that the modified thermal conductive filler of Preparation Example 1 is replaced by an equal amount of the modified thermal conductive filler of Preparation Example 6.

[0061] Example 7

[0062] A sample plate for high thermal conductivity liquid chromatography, which differs from Example 1 in that the modified thermal conductive filler of Preparation Example 1 is replaced by an equal amount of the modified thermal conductive filler of Preparation Example 7.

[0063] Example 8

[0064] A sample plate for high thermal conductivity liquid chromatography, which differs from Example 1 in that no styrene-maleic anhydride copolymer is added. Comparative Example

[0065] Comparative Example 1 A sample plate for high thermal conductivity liquid chromatography, which differs from Example 1 in that the modified thermal conductive filler of Preparation Example 1 is replaced by an equal amount of the modified thermal conductive filler of Preparation Example 8.

[0066] Comparative Example 2 A sample plate for high thermal conductivity liquid chromatography, which differs from Example 1 in that the modified thermal conductive filler of Preparation Example 1 is replaced by an equal amount of the modified thermal conductive filler of Preparation Example 9.

[0067] Comparative Example 3 A sample plate for high thermal conductivity liquid chromatography, which differs from Example 1 in that the modified thermal conductive filler of Preparation Example 1 is replaced by an equal amount of unmodified thermal conductive filler (alumina with a D50 particle size of 40 microns). Performance testing

[0068] Test 1: Thermal conductivity test The thermal conductivity of PTFE material is tested in accordance with the provisions of IS0 22007-2:2015 "Determination of thermal conductivity and thermal diffusivity of plastics Part 2: Transient plane heat source (hot disk) method".

[0069] Test 2: Impact strength test The notched Izod impact strength of the sample disc was measured according to ISO 180:2019 “Determination of Izod impact strength of plastic rigid materials”.

[0070] Table 1. Performance test results

[0071] Analysis of test results: 1. Combining Examples 1 to 8 and Comparative Examples 1 to 3 with Table 1, it can be seen that the surface modification of the thermal conductive filler using PTFE emulsion, fluorinated acrylate monomer, and methyl methacrylate significantly enhances the filler's effect on the thermal conductivity and impact strength of the PTFE resin matrix. The reason may be that for the non-polar PTFE resin substrate, the filler is difficult to disperse after being directly added, and a non-polar chain segment needs to be grafted on its surface to improve the compatibility of the filler with the resin substrate, so that it is fully dispersed and uniform, forming a good thermal conductivity path, and playing an excellent reinforcing role.

[0072] In addition, the present application mixes the surface-modified thermal conductive filler with PTFE emulsion for secondary surface modification, which effectively enhances the interfacial bonding force between the modified thermal conductive filler and the resin substrate, increases the interfacial contact area, reduces the interfacial thermal resistance, and further improves the thermal conductivity of the filled PTFE material.

[0073] 2. It can be seen from Example 1 and Example 4 and Table 1 that the introduction of sulfonate acrylic acid monomers to the surface of the heat-conducting filler in the primary polymerization and the secondary polymerization helps to improve the thermal conductivity and mechanical strength of the PTFE material. The reason may be that the introduction of sulfonate acrylic acid monomers can significantly increase the charge density on the surface of the filler, inhibit the agglomeration and sedimentation between particles through electrostatic action, promote the original flavor polymerization grafting reaction, and ensure the thermal conductivity and enhancement performance of the particle-modified filler in the PTFE resin. Similarly, the role of Examples 5 to 7 is to promote the dispersion of particles and ensure the progress of the polymerization grafting reaction, so as to fully improve the thermal conductivity and strength properties of the material.

[0074] 3. It can be seen from Example 1 and Example 8 and Table 1 that adding styrene-maleic anhydride copolymer to PTFE resin can help improve the impact strength of the product. The reason may be that styrene-maleic anhydride copolymer can compensate for the problem of decreased material toughness caused by adding a large amount of filler. Thus, the impact strength of the product can be improved together with the thermal conductive filler.

[0075] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A sample tray for high thermal conductivity liquid chromatography, characterized in that: The sample plate is made of PTFE material; in terms of mass percentage, the raw materials of the PTFE material include: 70-80% PTFE dispersed resin and 10-30% modified thermal conductive filler; the modified thermal conductive filler includes the following raw materials in parts by mass: 10 parts of thermal conductive filler, 5-12 parts of PTFE emulsion, 15-25 parts of fluorine-containing acrylate monomer, and 13-18 parts of methyl methacrylate.

2. The sample tray according to claim 1, characterized in that: The modified thermally conductive filler includes 9 to 16 parts by mass of sulfonate acrylic acid monomer.

3. The sample tray according to claim 2, characterized in that: The modified thermally conductive filler preparation method comprises the following steps: Add thermal conductive filler, 50-70wt% fluorinated acrylate monomer, 40-60wt% methyl methacrylate, and 30-50wt% sulfonate acrylic monomer to the emulsifier solution, stir evenly, add initiator, heat up for primary polymerization, and obtain a premixed solution; The PTFE emulsion and the premixed liquid are mixed evenly, the remaining fluorinated acrylate monomer, methyl methacrylate and sulfonate acrylate monomer are added, the initiator is added after stirring evenly, the temperature is raised for secondary polymerization, the temperature is lowered, separation and filtration are performed, washing and drying are performed, and a modified thermal conductive filler is obtained; Preferably, the temperature of the primary polymerization and the secondary polymerization is 65-75°C.

4. The sample tray according to claim 3, characterized in that: The emulsifier solution is obtained by mixing a nonionic surfactant, carboxymethyl cellulose, calcium carbonate and water in a mass ratio of 2-4:1-3:0.5-1.5:

100.

5. The sample tray according to claim 1, characterized in that: The sulfonate acrylic acid monomer is selected from one or more of sodium allyl sulfonate, sodium 2-propylene sulfonate, and sodium methyl propylene sulfonate.

6. The sample tray according to claim 1, characterized in that: The fluorine-containing acrylate monomer is selected from one or more of perfluoroalkylethyl methacrylate, trifluoroethyl methacrylate, and perfluoroalkyl acrylate.

7. The sample tray according to claim 1, characterized in that: The thermal conductive filler includes one or more of aluminum oxide, zinc oxide, aluminum nitride, boron nitride, silicon carbide, and graphite.

8. The sample tray according to claim 1, characterized in that: In terms of mass percentage, the raw material of the PTFE material also includes 5-10% styrene-maleic anhydride copolymer.

9. The method for preparing a sample tray according to claim 1, characterized in that: The steps include: Mixing: Add the modified thermal conductive filler into a mixing container, add PTFE dispersion resin and lubricant, and mix evenly to obtain PTFE material; Preforming: Put the PTFE material into the mold and make the preform by cold pressing; Sintering: sinter the preform at 370-390℃, and grind it after cooling; Preferably, the amount of the lubricant is 5-10% of the PTFE dispersed resin; Preferably, the lubricant is selected from silicone oil, mineral oil or paraffin oil.

10. The sample tray according to claim 9, characterized in that In the mixing step, 5 to 10% of the raw material mass of styrene-maleic anhydride copolymer is also added.

Citation Information

Cited By

  • High-thermal-conductivity polytetrafluoroethylene insulating material and preparation method thereof

    CN121895697A