PC / ASA / PMMA ternary alloy material with scratch resistance and self-cleaning performance and preparation method of PC / ASA / PMMA ternary alloy material

Through the preparation of PC/ASA/PMMA ternary alloy materials, combined with special additives and process treatment, the high-temperature curing and friction risks of self-cleaning and scratch resistance of automotive exterior parts materials is solved, and efficient self-cleaning and resistance to achieve Scratch effect, suitable for large and complex parts, reduces production costs and expands the scope of application.

CN119060519APending Publication Date: 2024-12-03JIANGSU ZHAOWEI PLASTICS TECH CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411306307.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-19
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Existing automotive exterior materials have high temperature curing requirements in terms of self-cleaning and scratch resistance, easy aging and falling off, and increased friction coefficient, which limits their application and durability.

Method used

Using PC/ASA/PMMA ternary alloy material, the superhydrophobicity and low friction coefficient are prepared by adding perfluoropolymer, nanosilicon dioxide and silicone, combined with high-speed mixing and melt blending extrusion technology. Material for self-cleaning and scratch-resistant effects.

Benefits of technology

It improves the durability and scratch resistance of the material, reduces production costs, is suitable for large and complex parts, expands the scope of application, and avoids the risks of high-temperature curing and friction of traditional technologies.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of high polymer materials, in particular to a PC / ASA / PMMA ternary alloy material with scratch resistance and self-cleaning performance and a preparation method of the PC / ASA / PMMA ternary alloy material, and the PC / ASA / PMMA ternary alloy material is prepared from the following raw materials in parts by weight: 280-320 parts of PC, 180-220 parts of ASA, 80-120 parts of PMMA, 7-11 parts of a perfluoropolymer, 7-11 parts of nano silicon dioxide and 5-7 parts of silicone. Through the special additive, the material surface is endowed with the characteristics of super-hydrophobicity, pollution resistance, hardness enhancement and the like, so that water drops show a high contact angle on the surface, and the material has excellent hydrophobicity and self-cleaning capability. By means of the design, attachment of dust and stains can be effectively reduced, the self-cleaning effect is achieved, the problems that a traditional self-cleaning coating needs high-temperature curing and is prone to aging and falling off can be solved, and the durability of the self-cleaning effect is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer materials, and in particular to a PC / ASA / PMMA ternary alloy material with scratch resistance and self-cleaning properties and a preparation method thereof. Background Art

[0002] With the development of the automobile industry, the demand for automobile exterior parts is growing. They are not only required to have beautiful appearance, but also to have good weather resistance, scratch resistance and self-cleaning performance. Among them, the self-cleaning performance can make the exterior parts automatically clean under the scouring of rain, which greatly improves the cleaning efficiency and reduces the maintenance cost. The scratch resistance can ensure the durability of the exterior parts in daily use and extend their service life.

[0003] At present, the market mainly improves the self-cleaning and scratch resistance of automotive exterior parts by applying self-cleaning coatings on the surface of materials. For example, some technologies achieve self-cleaning effects by coating fluorinated compounds on the surface of materials and using their low surface energy characteristics to form a high contact angle for water droplets on the surface. In addition, some technologies improve the surface hardness of materials by adding hard particles, such as calcium sulfate whiskers, to improve their scratch resistance.

[0004] However, there are still some problems with existing technologies in practical applications. First, existing self-cleaning coatings often require higher curing temperatures and longer curing times, which not only increases production costs but also limits their application on large and complex parts. Secondly, existing self-cleaning coatings may age and fall off during use, affecting the durability of their self-cleaning effects. In addition, although existing scratch-resistant technologies can improve the surface hardness of materials, they often increase the surface friction coefficient of the material, thereby increasing the risk of scratches. Summary of the invention

[0005] In view of the problems existing in the prior art, the present invention provides a PC / ASA / PMMA ternary alloy material with scratch resistance and self-cleaning performance and a preparation method thereof. The powder particle size distribution is uniform and stable, the powder reuse rate is high, the sintered product is not easy to yellow, and has good tensile strength and impact strength.

[0006] In order to achieve the above object, the present invention adopts the following technical solutions:

[0007] A PC / ASA / PMMA ternary alloy material with scratch resistance and self-cleaning properties comprises the following raw materials in parts by weight: 280-320 parts of PC, 180-220 parts of ASA, 80-120 parts of PMMA, 7-11 parts of perfluoropolymer, 7-11 parts of nano silicon dioxide and 5-7 parts of silicone.

[0008] Further, the following raw materials are included in parts by weight: 280 parts of PC, 180 parts of ASA, 80 parts of PMMA, 7 parts of perfluoropolymer, 7 parts of nano-silicon dioxide and 5 parts of silicone.

[0009] Further, the following raw materials are included in parts by weight: 300 parts of PC, 200 parts of ASA, 100 parts of PMMA, 9 parts of perfluoropolymer, 9 parts of nano-silicon dioxide and 6 parts of silicone.

[0010] Furthermore, the following raw materials are included in parts by weight: 320 parts of PC, 220 parts of ASA, 120 parts of PMMA, 11 parts of perfluoropolymer, 11 parts of nano-silicon dioxide and 7 parts of silicone.

[0011] Furthermore, the particle size of the nano-silicon dioxide is 100 to 200 μm.

[0012] A method for preparing a PC / ASA / PMMA ternary alloy material with scratch resistance and self-cleaning properties, characterized in that it comprises the following steps:

[0013] Step 1, preparing the above raw materials in parts by weight, including PC, ASA, PMMA, perfluoropolymer, nano-silicon dioxide and silicone;

[0014] Step 2: Put PC, ASA and PMMA into a high-speed mixer and mix them evenly. The mixing time is 25-35 minutes and the mixing temperature is 70-90°C.

[0015] Step 3: Add the mixed raw materials into a twin-screw extruder, and add perfluoropolymer and silica for melt blending and extrusion at a temperature of 190-210°C and a screw speed of 90-110rpm;

[0016] Step 4: Cooling and drying the extruded material, and then pelletizing it to obtain PC / ASA / PMMA ternary alloy material particles;

[0017] Step 5: Mix the obtained PC / ASA / PMMA ternary alloy material with silicone, put it into the high-speed mixer again, mix it evenly, the mixing time is 3 minutes, and the mixing temperature is 60°C;

[0018] Step 6: Add the mixed raw materials into a twin-screw extruder for melt blending and extrusion at an extrusion temperature of 175-185°C and a screw speed of 80 rpm;

[0019] Step 7: Cooling and drying the extruded material, and then granulating it to obtain the final scratch-resistant self-cleaning PC / ASA / PMMA ternary alloy material;

[0020] Furthermore, in the step 2, PC, ASA and PMMA are put into a high-speed mixer and mixed evenly. The mixing time is 30 minutes and the mixing temperature is 80°C.

[0021] Furthermore, in the step three, the mixed raw materials are added into a twin-screw extruder, and the perfluoropolymer and silica are added at the same time for melt blending and extrusion. The extrusion temperature is 200° C. and the screw speed is 100 rpm.

[0022] Furthermore, the method also includes step eight: applying the obtained scratch-resistant self-cleaning PC / ASA / PMMA ternary alloy material to automobile exterior trims, and forming automobile exterior trims through injection molding.

[0023] Compared with the existing technology, the beneficial effects of this technical solution are as follows:

[0024] 1. The scratch-resistant self-cleaning PC / ASA / PMMA ternary alloy material of the present invention has the properties of super hydrophobicity, anti-pollution and hardness enhancement on the surface of the material through special additives, so that water droplets present a high contact angle on the surface, thus having excellent hydrophobicity and self-cleaning ability. This design can not only effectively reduce the adhesion of dust and stains and achieve a self-cleaning effect, but also avoid the problems of traditional self-cleaning coatings requiring high temperature curing and easy aging and shedding, thereby improving the durability of the self-cleaning effect.

[0025] 2. The scratch-resistant self-cleaning PC / ASA / PMMA ternary alloy material of the present invention uses silicone to significantly reduce the friction coefficient of the material surface, thereby resisting scratches and wear during daily use and ensuring the durability of the high gloss effect. This design can not only improve the scratch resistance of the material, but also avoid the problem of traditional scratch-resistant technology increasing the friction coefficient of the material surface and increasing the risk of scratches.

[0026] 3. The scratch-resistant self-cleaning PC / ASA / PMMA ternary alloy material of the present invention has a simple preparation method, is suitable for large-scale production, is conducive to reducing production costs and improving production efficiency. At the same time, the material is suitable for large and complex parts, which expands its application range. In general, the scratch-resistant self-cleaning PC / ASA / PMMA ternary alloy material of the present invention and its preparation method have higher self-cleaning effect durability, better scratch resistance, lower production cost and wider application range compared with the prior art, and have obvious advantages. DETAILED DESCRIPTION

[0027] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0028] Embodiment 1:

[0029] Step 1, prepare raw materials, including PC 280g, ASA 180g, PMMA 80g, perfluoropolymer 7g, nano-silicon dioxide 7g and silicone 5g;

[0030] Step 2: Put PC, ASA and PMMA into a high-speed mixer and mix them evenly. The mixing time is 25 minutes and the mixing temperature is 70°C.

[0031] Step 3: Add the mixed raw materials into a twin-screw extruder, and add perfluoropolymer and silica for melt blending and extrusion at a temperature of 190°C and a screw speed of 90 rpm;

[0032] Step 4: Cooling and drying the extruded material, and then pelletizing it to obtain PC / ASA / PMMA ternary alloy material particles;

[0033] Step 5: Mix the obtained PC / ASA / PMMA ternary alloy material with silicone, put it into the high-speed mixer again, mix it evenly, the mixing time is 3 minutes, and the mixing temperature is 60°C;

[0034] Step 6: Add the mixed raw materials into a twin-screw extruder for melt blending and extrusion at an extrusion temperature of 175° C. and a screw speed of 80 rpm;

[0035] Step 7: Cool and dry the extruded material, and then granulate it to obtain the final scratch-resistant self-cleaning PC / ASA / PMMA ternary alloy material.

[0036] Embodiment 2:

[0037] Step 1, prepare raw materials, including PC 290g, ASA 190g, PMMA 90g, perfluoropolymer 8g, nano-silicon dioxide 8g and silicone 5.5g;

[0038] Step 2: Put PC, ASA and PMMA into a high-speed mixer and mix them evenly. The mixing time is 28 minutes and the mixing temperature is 75°C.

[0039] Step 3: Add the mixed raw materials into a twin-screw extruder, and add perfluoropolymer and silica for melt blending and extrusion at a temperature of 195°C and a screw speed of 95 rpm;

[0040] Step 4: Cooling and drying the extruded material, and then pelletizing it to obtain PC / ASA / PMMA ternary alloy material particles;

[0041] Step 5: Mix the obtained PC / ASA / PMMA ternary alloy material with silicone, put it into the high-speed mixer again, mix it evenly, the mixing time is 3 minutes, and the mixing temperature is 60°C;

[0042] Step 6: Add the mixed raw materials into a twin-screw extruder for melt blending and extrusion at an extrusion temperature of 178°C and a screw speed of 80 rpm;

[0043] Step 7: Cool and dry the extruded material, and then granulate it to obtain the final scratch-resistant self-cleaning PC / ASA / PMMA ternary alloy material.

[0044] Embodiment 3:

[0045] Step 1, prepare raw materials, including 300g PC, 200g ASA, 100g PMMA, 9g perfluoropolymer, 9g nano-silicon dioxide and 6g silicone;

[0046] Step 2: Put PC, ASA and PMMA into a high-speed mixer and mix them evenly. The mixing time is 30 minutes and the mixing temperature is 80°C.

[0047] Step 3: Add the mixed raw materials into a twin-screw extruder, and add perfluoropolymer and silica for melt blending and extrusion at a temperature of 200° C. and a screw speed of 100 rpm;

[0048] Step 4: Cooling and drying the extruded material, and then pelletizing it to obtain PC / ASA / PMMA ternary alloy material particles;

[0049] Step 5: Mix the obtained PC / ASA / PMMA ternary alloy material with silicone, put it into the high-speed mixer again, mix it evenly, the mixing time is 3 minutes, and the mixing temperature is 60°C;

[0050] Step 6: Add the mixed raw materials into a twin-screw extruder for melt blending and extrusion at an extrusion temperature of 180°C and a screw speed of 80 rpm;

[0051] Step 7: Cool and dry the extruded material, and then granulate it to obtain the final scratch-resistant self-cleaning PC / ASA / PMMA ternary alloy material.

[0052] Embodiment 4:

[0053] Step 1, prepare raw materials, including 310g PC, 210g ASA, 110g PMMA, 10g perfluoropolymer, 10g nano-silicon dioxide and 6.5g silicone;

[0054] Step 2: Put PC, ASA and PMMA into a high-speed mixer and mix them evenly. The mixing time is 33 minutes and the mixing temperature is 85°C.

[0055] Step 3: Add the mixed raw materials into a twin-screw extruder, and add perfluoropolymer and silica for melt blending and extrusion at a temperature of 205°C and a screw speed of 105 rpm;

[0056] Step 4: Cooling and drying the extruded material, and then pelletizing it to obtain PC / ASA / PMMA ternary alloy material particles;

[0057] Step 5: Mix the obtained PC / ASA / PMMA ternary alloy material with silicone, put it into the high-speed mixer again, mix it evenly, the mixing time is 3 minutes, and the mixing temperature is 60°C;

[0058] Step 6: Add the mixed raw materials into a twin-screw extruder for melt blending and extrusion at an extrusion temperature of 182° C. and a screw speed of 80 rpm;

[0059] Step 7: Cool and dry the extruded material, and then granulate it to obtain the final scratch-resistant self-cleaning PC / ASA / PMMA ternary alloy material.

[0060] Embodiment 5:

[0061] Step 1, prepare raw materials, including 320g PC, 220g ASA, 120g PMMA, 11g perfluoropolymer, 11g nano-silicon dioxide and 7g silicone;

[0062] Step 2: Put PC, ASA and PMMA into a high-speed mixer and mix them evenly. The mixing time is 35 minutes and the mixing temperature is 90°C.

[0063] Step 3: Add the mixed raw materials into a twin-screw extruder, and add perfluoropolymer and silica for melt blending and extrusion at a temperature of 210° C. and a screw speed of 110 rpm;

[0064] Step 4: Cooling and drying the extruded material, and then pelletizing it to obtain PC / ASA / PMMA ternary alloy material particles;

[0065] Step 5: Mix the obtained PC / ASA / PMMA ternary alloy material with silicone, put it into the high-speed mixer again, mix it evenly, the mixing time is 3 minutes, and the mixing temperature is 60°C;

[0066] Step 6: Add the mixed raw materials into a twin-screw extruder for melt blending and extrusion at an extrusion temperature of 185°C and a screw speed of 80 rpm;

[0067] Step 7: Cool and dry the extruded material, and then granulate it to obtain the final scratch-resistant self-cleaning PC / ASA / PMMA ternary alloy material.

[0068] The scratch-resistant self-cleaning PC / ASA / PMMA ternary alloy material of the present invention has the properties of super hydrophobicity, anti-pollution and hardness enhancement on the surface of the material through special additives, so that water droplets present a high contact angle on the surface, thus having excellent hydrophobicity and self-cleaning ability. This design can not only effectively reduce the adhesion of dust and stains and achieve a self-cleaning effect, but also avoid the problems of traditional self-cleaning coatings requiring high temperature curing and easy aging and shedding, thereby improving the durability of the self-cleaning effect.

[0069] The scratch-resistant self-cleaning PC / ASA / PMMA ternary alloy material of the present invention uses silicone to significantly reduce the friction coefficient of the material surface, thereby resisting scratches and wear during daily use and ensuring the durability of the high gloss effect. This design can not only improve the scratch resistance of the material, but also avoid the problem that traditional scratch-resistant technology increases the friction coefficient of the material surface and increases the risk of scratches.

[0070] The scratch-resistant self-cleaning PC / ASA / PMMA ternary alloy material of the present invention has a simple preparation method, is suitable for large-scale production, is conducive to reducing production costs and improving production efficiency. At the same time, the material is suitable for large and complex parts, which expands its application range. In general, the scratch-resistant self-cleaning PC / ASA / PMMA ternary alloy material of the present invention and its preparation method have higher self-cleaning effect durability, better scratch resistance, lower production cost and wider application range compared with the prior art, and have obvious advantages.

[0071] Due to the advanced nature of this technical solution, it can be widely used in the field of automobile manufacturing. First, the automobile manufacturing industry can use this scratch-resistant and self-cleaning PC / ASA / PMMA ternary alloy material in large quantities to manufacture automobile exterior parts, such as bumpers, headlight covers, grilles, outer triangular decorative panels, etc., which can not only improve the beauty and durability of the car, reduce maintenance costs, but also enhance the overall image and brand value of the car.

[0072] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A PC / ASA / PMMA ternary alloy material with scratch resistance and self-cleaning properties, characterized in that: The invention comprises the following raw materials in parts by weight: 280-320 parts of PC, 180-220 parts of ASA, 80-120 parts of PMMA, 7-11 parts of perfluoropolymer, 7-11 parts of nano silicon dioxide and 5-7 parts of silicone.

2. The PC / ASA / PMMA ternary alloy material with scratch resistance and self-cleaning properties according to claim 1, characterized in that: The invention comprises the following raw materials in parts by weight: 280 parts of PC, 180 parts of ASA, 80 parts of PMMA, 7 parts of perfluoropolymer, 7 parts of nano silicon dioxide and 5 parts of silicone.

3. The PC / ASA / PMMA ternary alloy material with scratch resistance and self-cleaning performance according to claim 1, characterized in that: The invention comprises the following raw materials in parts by weight: 300 parts of PC, 200 parts of ASA, 100 parts of PMMA, 9 parts of perfluoropolymer, 9 parts of nano silicon dioxide and 6 parts of silicone.

4. The PC / ASA / PMMA ternary alloy material with scratch resistance and self-cleaning performance according to claim 1, characterized in that: The invention comprises the following raw materials in parts by weight: 320 parts of PC, 220 parts of ASA, 120 parts of PMMA, 11 parts of perfluoropolymer, 11 parts of nano silicon dioxide and 7 parts of silicone.

5. The PC / ASA / PMMA ternary alloy material with scratch resistance and self-cleaning properties according to claim 1, characterized in that: The particle size of the nano silicon dioxide is 100-200 μm.

6. A method for preparing the PC / ASA / PMMA ternary alloy material with scratch resistance and self-cleaning properties as claimed in any one of claims 1 to 5, characterized in that: The steps include: Step 1, preparing the above raw materials in parts by weight, including PC, ASA, PMMA, perfluoropolymer, nano-silicon dioxide and silicone; Step 2: Put PC, ASA and PMMA into a high-speed mixer and mix them evenly. The mixing time is 25-35 minutes and the mixing temperature is 70-90°C. Step 3: Add the mixed raw materials into a twin-screw extruder, and add perfluoropolymer and silica for melt blending and extrusion at a temperature of 190-210°C and a screw speed of 90-110rpm; Step 4: Cooling and drying the extruded material, and then pelletizing to obtain PC / ASA / PMMA ternary alloy material particles; Step 5: Mix the obtained PC / ASA / PMMA ternary alloy material with silicone, put it into the high-speed mixer again, mix it evenly, the mixing time is 3 minutes, and the mixing temperature is 60°C; Step 6: Add the mixed raw materials into a twin-screw extruder for melt blending and extrusion at an extrusion temperature of 175-185°C and a screw speed of 80 rpm; Step 7: Cooling and drying the extruded material, and then granulating it to obtain the final scratch-resistant self-cleaning PC / ASA / PMMA ternary alloy material; 7. The method for preparing a PC / ASA / PMMA ternary alloy material with scratch resistance and self-cleaning properties according to claim 6, characterized in that: In the step 2, PC, ASA and PMMA are put into a high-speed mixer and mixed evenly. The mixing time is 30 minutes and the mixing temperature is 80°C.

8. The method for preparing a PC / ASA / PMMA ternary alloy material with scratch resistance and self-cleaning properties according to claim 6, characterized in that: In the step three, the mixed raw materials are added into a twin-screw extruder, and the perfluoropolymer and silicon dioxide are added at the same time for melt blending and extrusion. The extrusion temperature is 200° C. and the screw speed is 100 rpm.

9. The method for preparing a PC / ASA / PMMA ternary alloy material with scratch resistance and self-cleaning properties according to claim 6, characterized in that: The step also includes step eight: applying the obtained scratch-resistant self-cleaning PC / ASA / PMMA ternary alloy material to automobile exterior trims, and forming automobile exterior trims through injection molding.

Citation Information

Cited By

  • Ethanol-resistant spraying-free high-brightness black ASA / PMMA material and preparation method thereof

    CN120399378A

  • PC / PMMA alloy material and preparation method and application thereof

    CN121226643A