UV structural adhesive as well as preparation method and application thereof

By introducing silicone modified acrylate and modified mica powder into UV structural glue, combined with polyurethane modified acrylic resin and other additives, the problem of high vapor transmission rate of UV structural glue is solved, and the water vapor of OLED display devices is significantly improved Isolation performance and service life.

CN119060680APending Publication Date: 2024-12-03HUNAN CHUANGJIN TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411079654.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The water vapor transmission rate of existing UV structural adhesives is too high, resulting in OLED display devices being susceptible to moisture corrosion and have a short service life.

Method used

Introduce silicone modified acrylate and modified mica powder into the formulation of UV structural glue, using its hydrophobicity and high-diameter thickness ratio structure to improve water vapor isolation and water resistance, and enhance the attachment of the substrate by polyurethane modified acrylic resin Focus and bond strength, dilute monomer to adjust viscosity and curing speed, coupling agent promotes component binding, thixotropic agent adjusts rheology properties, and initiator achieves rapid curing.

Benefits of technology

It significantly reduces the water vapor transmission rate, improves the water resistance, corrosion and permeability of UV glue, extends the service life of OLED display devices, enhances its stability and reliability, and optimizes the packaging process and display effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004983336720000201
    Figure BDA0004983336720000201
Patent Text Reader

Abstract

The invention provides a UV structural adhesive as well as a preparation method and application thereof. The UV structural adhesive is prepared from the following raw materials: polyurethane modified acrylic resin, a diluting monomer, organic silicon modified acrylate, modified mica powder, a coupling agent, an adhesion promoter, a thixotropic agent and an initiator. The organosilicone modified acrylate is introduced into the formula, and organosilicone has strong hydrophobicity and flexibility, so that the water vapor isolation and water resistance of the UV adhesive can be effectively improved. The invention also provides a preparation method and application of the UV structural adhesive.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of OLED manufacturing, and in particular relates to a UV structural adhesive and a preparation method and application thereof. Background Art

[0002] In the process of manufacturing OLED display devices, packaging technology plays a vital role. Packaging is not only about wrapping electronic components in protective materials, but also a key step to prevent water vapor and oxygen from invading the inside of the device, thereby preventing device aging and failure. Especially for electronic and semiconductor devices, the water vapor transmission rate (WVIR) of the packaging material is a crucial indicator.

[0003] At present, UV structural adhesive is widely used as a commonly used packaging material due to its excellent curing performance and chemical stability. However, due to its inherent characteristics, the existing UV structural adhesive has the problem of too high water vapor transmission rate, which makes the display device susceptible to moisture corrosion, thus greatly shortening its service life. In order to solve this problem, it is urgent to develop a UV structural adhesive with low water vapor transmission rate to improve the long-term stability and reliability of display devices. Summary of the invention

[0004] The present invention aims to solve at least one of the above technical problems existing in the prior art. To this end, the present invention provides a UV structural adhesive, which effectively improves the water vapor isolation and water resistance performance of the UV adhesive.

[0005] The invention also provides a method for preparing the UV structural adhesive.

[0006] The invention also provides an application of UV structural adhesive.

[0007] The first aspect of the present invention provides a UV structural adhesive, the preparation raw materials of which include polyurethane modified acrylic resin, diluent monomer, organosilicon modified acrylate, modified mica powder, coupling agent, adhesion promoter, thixotropic agent and initiator.

[0008] One of the technical solutions of the present invention regarding UV structural adhesive has at least the following beneficial effects:

[0009] The water vapor permeability of UV glue itself is relatively high, resulting in a short product life after packaging. There are two reasons for this. One is that the wettability with the substrate is poor and the interfacial bonding strength at the substrate is weak; the other is that the water vapor permeability of the material itself is relatively high. To improve this phenomenon, the present invention introduces silicone-modified acrylate and modified mica powder into the formula, utilizing the hydrophobicity of silicone and the high diameter-to-thickness ratio of mica, thereby effectively improving the above problems. Specifically,

[0010] The present invention introduces silicone-modified acrylate into the formula. Due to its strong hydrophobicity and flexibility, silicone can effectively improve the water vapor isolation and water resistance of the UV glue itself. The structure of the modified mica powder is a compound silicon oxide layer composed of two layers of silicon oxide tetrahedrons sandwiching a layer of aluminum oxide octahedron. It can be split into extremely thin sheets with a large diameter-to-thickness ratio, a two-dimensional sheet structure, and stacked sheets, which greatly improves the water resistance, corrosion resistance, and penetration resistance of the paint film. The modified mica powder further improves its dispersibility in the system. The mica powder is evenly arranged in the colloid to form a barrier. When water vapor wants to penetrate, it needs to greatly increase its penetration path, thereby reducing water vapor penetration. Secondly, the synthetic mica powder has high transparency and its curing speed will not be reduced due to the addition of fillers.

[0011] The role of polyurethane modified acrylic resin is mainly to provide the main properties and characteristics of the colloid as a base resin. Specifically, polyurethane modified acrylic resin provides basic performance and colloid structure: polyurethane modified acrylic resin, as the main base resin, provides the necessary fluidity, curing performance and weather resistance for UV structural adhesive. Its selection is based on its good compatibility with other ingredients in the formula (such as diluent monomers, silicone modified acrylates, modified mica powder, etc.) to form a stable colloid structure. In addition, during the use of UV structural adhesive, polyurethane modified acrylic resin can improve the wettability with the substrate, thereby enhancing its adhesion and bonding strength on the surface of the substrate. This is crucial to ensure the stability and durability of the encapsulated product. Further, as the main curing basis, the selection of polyurethane modified acrylic resin directly affects the curing speed and final physical properties of UV adhesive. This includes aspects such as the hardness, flexibility and chemical stability of the colloid. Further, through polyurethane modification, UV structural adhesive can obtain better water resistance, thereby extending the service life of the encapsulated product. This is particularly important for applications in high-demand environments such as OLED display devices, which can effectively prevent the penetration of water vapor and device aging caused by chemical reactions. Therefore, the polyurethane-modified acrylic resin in the above formula is not only the main component of the colloid, but also plays an important role in adjusting and optimizing the compatibility of other ingredients, providing basic performance, and enhancing the durability and stability of the product.

[0012] The main function of the diluent monomer is to adjust the viscosity and fluidity of the colloid, as well as to affect the curing speed and final performance of the colloid. Specifically, the diluent monomer can significantly affect the viscosity and fluidity of the UV colloid through its molecular structure and the amount of addition. This is very important for the operability of the colloid during construction and coating. The appropriate diluent monomer can make the colloid easier to be evenly coated on the surface of the substrate, ensuring the flatness and uniformity of the coating. It can be understood that UV structural adhesives need to be cured by ultraviolet light to form a stable encapsulation layer. The selection of diluent monomers can adjust the curing speed of the colloid. Generally, appropriate diluent monomers can help optimize the curing speed, so that the colloid can be quickly cured after ultraviolet light irradiation, and ensure that the physical properties after curing meet the requirements. In addition, the addition of diluent monomers can improve the optical transparency and surface quality of UV structural adhesives, ensuring that the encapsulated products meet good visual effects and performance requirements. In addition, it can also affect the flexibility and durability of the colloid, thereby improving the service life and environmental adaptability of the product. Further, the appropriately selected diluent monomer can help improve the chemical stability of the UV adhesive, making it less likely to deteriorate or degrade during long-term use, thereby ensuring the stability and reliability of the encapsulated product. Therefore, the diluent monomer in UV structural adhesive is not only to adjust its rheological properties and operability, but also to affect the curing speed, optical properties and long-term stability of the colloid. It is one of the indispensable and important components in the formula.

[0013] The role of coupling agents is to promote chemical bonding and interaction between different components to enhance the performance and stability of the overall colloid. UV structural adhesives usually contain fillers such as modified mica powder, and coupling agents can enhance the bonding between fillers and resins. This chemical bonding can effectively reduce the movement and deposition of fillers in the colloid, thereby improving the uniformity and stability of the colloid. Coupling agents can also improve the dispersibility of fillers in the resin system and ensure that the fillers are evenly distributed throughout the colloid. Especially for nano-scale fillers such as modified mica powder, the role of coupling agents can prevent their agglomeration in the colloid, thereby maintaining the physical and chemical properties they provide. By promoting good bonding between fillers and resins, coupling agents help enhance the mechanical strength, wear resistance and tensile resistance of UV structural adhesives. This is crucial for the long-term stability and reliability of encapsulated products. In addition, the addition of coupling agents can make UV structural adhesives show better heat resistance, chemical corrosion resistance and water resistance under various environmental conditions. This is very important for long-term reliability in high-demand applications such as display devices. Therefore, the use of coupling agents in UV structural adhesives is not only to enhance the bonding strength and dispersibility between fillers and resins, but also to improve the overall physical properties and environmental resistance of the colloid. It is an important component to ensure the stability of the colloid and optimize its performance.

[0014] The role of adhesion promoters is mainly to improve the bonding strength and adhesion between UV colloids and substrates. UV colloids need to be able to firmly adhere to various substrate surfaces, including glass, metal, plastic, etc. Adhesion promoters can effectively improve their adhesion by improving the affinity of the colloid to the substrate surface. This is very important to ensure the stability and reliability of the encapsulated product under various stress and environmental conditions. The adhesion performance of UV colloids is affected by surface tension and wettability. Adhesion promoters can adjust the contact angle between the colloid and the substrate surface, so that the colloid can wet the substrate surface more evenly and adhere to it more firmly. It can be understood that a properly selected adhesion promoter can reduce the gaps and bubbles between the colloid and the substrate, ensuring the integrity and uniformity of the contact surface. This is very important to prevent water vapor and other harmful substances from penetrating into the interface between the colloid and the substrate, thereby protecting the product from damage and aging. By enhancing the adhesion of UV colloids to the substrate, adhesion promoters can significantly improve the weather resistance and durability of the product. This is particularly critical for outdoor environments or applications that require long-term stability. Therefore, the role of adhesion promoter in UV structural adhesive is to enhance the bonding strength and adhesion between the colloid and various substrates, thereby improving the performance and stability of the packaged product. Selecting a suitable adhesion promoter is of great significance to ensure that the UV colloid can achieve the expected technical performance in practical applications.

[0015] The role of thixotropic agents is to adjust the rheological properties of the colloid, especially during the construction and curing process, as well as the stability of performance under different environmental conditions. Specifically, thixotropic agents are able to change their rheological properties according to the applied shear force, thereby controlling the viscosity of the colloid. In a static state, the viscosity of the colloid is high, which helps in precise control and curing during coating and coating. When subjected to shear force, thixotropic agents significantly reduce the viscosity of the colloid, facilitating coating and fluidity. Since UV structural adhesives require precise control during coating or injection, thixotropic agents can make them easier to handle and operate during construction. This property is essential to ensure that the colloid is evenly coated on the surface of the substrate and fill small holes and depressions. The addition of thixotropic agents can also optimize the curing speed and efficiency of UV colloids. It can adjust the reaction speed of the colloid under UV light irradiation to ensure that the curing process is completed in an appropriate time to obtain the desired physical and chemical properties. By adjusting the rheological properties of the colloid, the thixotropic agent can improve the stability of UV structural adhesives under different temperature and humidity conditions, which is very important for ensuring the stability of the product under long-term use and in various environments. Choosing a suitable thixotropic agent can significantly improve the application performance and market competitiveness of UV colloids.

[0016] The role of the initiator is to promote the rapid polymerization reaction, thereby achieving the curing or cross-linking of the UV colloid. The initiator in the UV structural adhesive will undergo a chemical reaction under ultraviolet light to generate free radicals or ions. These active species can initiate the polymerization reaction between monomer molecules. Through the action of the initiator, the liquid UV colloid can be quickly converted into a solid state to achieve curing and cross-linking, thereby forming a colloid with the desired physical properties. Selecting a suitable initiator can adjust the curing speed of the UV colloid so that it can reach the ideal degree of hardening within the required time. This is crucial for the control of production efficiency and product quality, and can ensure precise operation and stability during the production process. In addition, the role of the initiator is not only to start the polymerization reaction, but also to ensure that the polymer chains in the entire colloid system are fully cross-linked and cured. This helps to improve the mechanical strength, wear resistance and environmental corrosion resistance of the colloid. Further, the selection and amount of initiator used can affect the final physical and chemical properties of the UV structural adhesive, such as hardness, heat resistance, chemical resistance, etc. Therefore, engineers need to select the appropriate initiator according to the specific application requirements and environmental conditions to achieve the best product performance. It can be understood that the role of the initiator in UV structural adhesive is to achieve the curing and cross-linking of the colloid by initiating polymerization reactions, thereby ensuring that the product has the required physical and chemical properties. The correct selection and use of initiators is one of the key factors to ensure that UV colloids can achieve the expected performance in practical applications.

[0017] According to some embodiments of the present invention, the preparation raw materials include, by weight:

[0018] Polyurethane modified acrylic resin: 45 to 55 parts,

[0019] Diluent: 20 to 30 parts,

[0020] Silicone modified acrylate: 2 to 7 parts,

[0021] Modified mica powder: 10 to 25 parts,

[0022] Coupling agent: 0.5 to 2 parts,

[0023] Adhesion promoter: 0.5 to 2 parts,

[0024] Thixotropic agent: 1 to 5 parts,

[0025] Initiator: 2 to 6 parts.

[0026] According to some embodiments of the present invention, the preparation raw materials include, by weight:

[0027] Polyurethane modified acrylic resin: 48 to 53 parts,

[0028] Diluent: 20 to 25 parts,

[0029] Silicone modified acrylate: 3 to 7 parts,

[0030] Modified mica powder: 15 to 20 parts,

[0031] Coupling agent: 1 to 1.5 parts,

[0032] Adhesion promoter: 1 to 1.5 parts,

[0033] Thixotropic agent: 2 to 5 parts,

[0034] Initiator: 4 to 6 parts.

[0035] According to some embodiments of the present invention, the polyurethane modified acrylic resin includes at least one of L-8402, L-8403, L-8405C, L-8412A, L-8414, L-8442, BASF Laromer UA9065, allnex EBECRYL246 and allnex EBECRYL8894.

[0036] According to some embodiments of the present invention, the method for preparing the organosilicon-modified acrylate comprises: adding γ-methacryloxypropyltrimethoxysilane to terminal methyl dimethoxy silicone oil, heating the reaction, and then adding dibutyltin dilaurate for reaction.

[0037] According to some embodiments of the present invention, the preparation method of the organosilicon-modified acrylate may be:

[0038] Weigh 1 mol of terminal methyl dimethoxy silicone oil (viscosity 1000-2000cps) in a three-necked flask, gradually add 2.2 mol of γ-methacryloxypropyltrimethoxysilane, after the addition is completed, heat to 40°C, react for 2 hours, then add 0.2% dibutyltin dilaurate, and react for another hour. After the reaction is completed, cool to room temperature, wash with petroleum ether, and dry to obtain the final product KH-SJ.

[0039] According to some embodiments of the present invention, the method for preparing the modified mica powder comprises:

[0040] (1) dissolving a silane modifier in an alcohol solution, adjusting the pH, and then heating to obtain a pre-hydrolyzed silane modifier;

[0041] (2) After the mica powder is dispersed, the pre-hydrolyzed silane modifier is added, mixed at high speed, and then dried.

[0042] In step (1), the preparation method of the pre-hydrolyzed silane modifier can be: a certain amount of deionized water and anhydrous ethanol are prepared in a ratio of 1:1, the solution is placed in a 200mL beaker, and then the alkane modifier is weighed and placed therein, wherein the mass proportion of the modifier is 25%, the pH of the solution is adjusted to 4-5 using glacial acetic acid, and the solution is placed in a 60°C water bath with stirring and heating to promote the pre-hydrolysis of the modifier for standby use.

[0043] Step (2) may specifically be: weigh mica powder and place it in a high-speed mixer, pre-disperse and mix for 5 minutes, weigh the silane modifier that has been pre-hydrolyzed in the above step (1) and add it thereto, add it in multiple times, mix at high speed for 20 minutes, dry the material, and test it for use, wherein the amount of silane modifier is 1.5%.

[0044] According to some embodiments of the present invention, the silane modifier includes at least one of methyltrimethoxysilane, hexadecyltrimethoxysilane, γ-methacryloxypropyltrimethoxysilane, and aminopropyltriethoxysilane.

[0045] According to some embodiments of the present invention, the modified mica powder: the mica powder raw material is synthetic mica powder or wet mica powder, with an average particle size of 6-15 μm and an aspect ratio of 80-120.

[0046] According to some embodiments of the present invention, the diluent monomer includes at least one of dimethyl acrylamide, hydroxyethyl methacrylate, hydroxypropyl methacrylate, isobornyl acrylate, lauryl acrylate and cyclohexyl methacrylate.

[0047] According to some embodiments of the present invention, the coupling agent includes at least one of vinyltrimethoxysilane, vinyltri(methoxyethoxy)silane, vinyltriethoxysilane and aminopropyltriethoxysilane.

[0048] According to some embodiments of the present invention, the adhesion promoter includes at least one of a phosphate compound, EM39 and Lencolo 4051.

[0049] According to some embodiments of the present invention, the thixotropic agent is silica.

[0050] According to some embodiments of the invention, the initiator includes at least one of 184, BP, Omnirad 500, TR-NPI-20400, 819, ITX and Lencolo 5032.

[0051] According to some embodiments of the invention, the adhesion promoter comprises a phosphate compound.

[0052] According to some embodiments of the invention, the adhesion promoter includes at least one of EM39 and Lencolo 4051.

[0053] The second aspect of the present invention provides a method for preparing a UV structural adhesive, comprising the following steps: mixing the polyurethane modified acrylic resin, diluent monomer, silicone modified acrylate and modified mica powder, stirring and dispersing them, adding the coupling agent, adhesion promoter and thixotropic agent, dispersing them evenly, and finally adding the initiator, stirring and degassing them evenly.

[0054] A technical solution in the preparation method of UV structural adhesive of the present invention has at least the following beneficial effects:

[0055] The preparation method of the present invention does not require expensive equipment and complicated process control, has undemanding reaction conditions, has readily available raw materials, has low production costs, and is easy to industrialize.

[0056] The preparation method of the present invention ensures uniform distribution of each component in the colloid by first mixing and stirring the polyurethane modified acrylic resin, the diluent monomer, the organosilicon modified acrylate and the modified mica powder. This step is the key in the preparation process and can effectively improve the homogeneity and stability of subsequent products.

[0057] Adding coupling agents and adhesion promoters can form stronger chemical bonds and physical adsorption between the colloid and the substrate, thereby significantly improving the adhesion and interfacial bonding strength of the UV structural adhesive on the substrate. This is crucial to enhancing the durability and service life of the product.

[0058] The introduction of thixotropic agents can adjust the rheological properties of the colloid during the construction process, so that it has appropriate viscosity and fluidity during construction, which helps to improve operability and coating uniformity, thereby reducing process difficulty and loss during product manufacturing.

[0059] The addition of initiator can quickly start the curing reaction of UV colloid, prompting the colloid to quickly cure and crosslink under ultraviolet light. This not only improves production efficiency, but also ensures that the product achieves the required physical and chemical properties in a short time, thereby reducing the manufacturing cycle and increasing product output.

[0060] The final step of vacuum degassing can effectively remove bubbles and tiny voids in the colloid, further improving the uniformity and density of the colloid. This helps reduce defects and quality problems that may occur during the use of the product, and improves the reliability and stability of the product.

[0061] According to some embodiments of the present invention, the polyurethane modified acrylic resin, diluent monomer, silicone modified acrylate and modified mica powder are mixed and stirred and dispersed. The stirring and dispersion can be carried out in a planetary mill. The stirring speed can be 10 rpm and the dispersion speed can be 300±10 rpm.

[0062] According to some embodiments of the present invention, the coupling agent, adhesion promoter and thixotropic agent are added and dispersed evenly, the stirring speed may be 50 rpm, and the dispersion speed may be 300±10 rpm.

[0063] According to some embodiments of the present invention, the initiator is finally added and stirred evenly, and the stirring speed may be 50 rpm.

[0064] After vacuum degassing, it can be packaged for later use.

[0065] A third aspect of the present invention provides an OLED display device, wherein the OLED display device comprises the UV structural adhesive of the present invention.

[0066] One of the technical solutions of the present invention regarding the OLED display device has at least the following beneficial effects:

[0067] When the UV structural adhesive of the present invention is applied to an OLED display device, the UV structural adhesive has excellent water vapor isolation performance and water resistance, and can effectively prevent water vapor and oxygen from entering the interior of the OLED display device. This protective ability can significantly extend the service life of the OLED display device, reduce device aging and failure caused by moisture, and improve the stability and reliability of the device. The high transparency and low dispersion properties of the UV structural adhesive prevent it from affecting the display effect of the OLED display device during the packaging process. After the colloid is cured, maintaining high transparency helps to maintain the high definition and color saturation of the OLED display device and enhance the user's visual experience. Since the UV structural adhesive has the characteristic of rapid curing, it can quickly complete the curing process under ultraviolet light irradiation. This characteristic reduces the manufacturing cycle in the packaging process, improves the efficiency and production capacity of the production line, helps to reduce manufacturing costs and enhance competitiveness. The application of the UV structural adhesive of the present invention to OLED display devices can not only improve the protection performance and display effect of its packaging, but also optimize the manufacturing process and product performance, thereby occupying a favorable position in market competition. DETAILED DESCRIPTION

[0068] The following are specific embodiments of the present invention, and the technical solutions of the present invention are further described in conjunction with the embodiments, but the present invention is not limited to these embodiments.

[0069] The following will be combined with the embodiments to clearly and completely describe the concept of the present invention and the technical effects produced, so as to fully understand the purpose, characteristics and effects of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, other embodiments obtained by those skilled in the art without creative work are all within the scope of protection of the present invention.

[0070] In the description of the present invention, the description with reference to the terms "one embodiment", "some embodiments", "illustrative embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.

[0071] Unless otherwise specified, "room temperature" in the present invention means 25°C±5°C.

[0072] Unless otherwise specified, "about" in the present invention means that the allowable error is within ±2%.

[0073] If the specific conditions are not specified in the examples, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. If the manufacturers of the reagents or instruments are not specified, they are all conventional products that can be purchased commercially.

[0074] Example 1

[0075] A UV structural adhesive was prepared, and the raw materials for preparation were:

[0076] Polyurethane modified acrylic resin: 48 parts,

[0077] Diluted monomer: 20 parts,

[0078] Silicone modified acrylate: 3 parts,

[0079] Modified wet mica powder: 15 parts,

[0080] Coupling agent: 1 part,

[0081] Adhesion promoter: 1 part,

[0082] Thixotropic agent: 2 parts,

[0083] Initiator: 4 parts.

[0084] In the preparation of raw materials:

[0085] The polyurethane modified acrylic resin is Lancolu L-8402.

[0086] The diluent monomer is dimethyl acrylamide.

[0087] The preparation method of silicone-modified acrylate is as follows: weigh 1 mol of terminal methyl dimethoxy silicone oil (viscosity 1000-2000 cps) in a three-necked flask, gradually add 2.2 mol of γ-methacryloxypropyltrimethoxysilane, and after the addition is completed, heat to 40° C., react for 2 hours, then add 0.2% of dibutyltin dilaurate, and react for another hour. After the reaction is completed, cool to room temperature, wash with petroleum ether, and dry to obtain the final product KH-SJ.

[0088] The preparation method of modified mica powder is:

[0089] 1. Prepare 50g solution of deionized water and anhydrous ethanol in a ratio of 1:1 and place it in a 200mL beaker. Then weigh 16.67g of hexadecyltrimethoxysilane and place it in it. Use glacial acetic acid to adjust the pH of the solution to 4-5. Place it in a 60℃ water bath with stirring and heating to promote the pre-hydrolysis of the modifier for standby use.

[0090] 2. Weigh 1 kg of wet mica powder and place it in a high-speed mixer. Pre-disperse and mix for 5 minutes. Weigh the silane modifier that has been pre-hydrolyzed in step 1 above and add it three times. Mix at high speed for 20 minutes. Dry the material and test it for later use. The amount of silane modifier is 1.5%.

[0091] The coupling agent is vinyltrimethoxysilane.

[0092] The adhesion promoter is EM39.

[0093] The thixotropic agent is silica.

[0094] The initiator is 184 initiator.

[0095] The preparation method of the UV structural adhesive in this embodiment is as follows: after mixing polyurethane modified acrylic resin, diluent monomer, organosilicon modified acrylate and modified mica powder, stirring and dispersing, adding coupling agent, adhesion promoter and thixotropic agent, dispersing evenly, and finally adding initiator, stirring evenly and vacuum degassing.

[0096] Polyurethane modified acrylic resin, diluent monomer, organosilicon modified acrylate and modified mica powder were mixed in a planetary mill with a stirring speed of 10 rpm and a dispersing speed of 300 rpm.

[0097] After adding coupling agent, adhesion promoter and thixotropic agent, the stirring speed was 50 rpm and the dispersion speed was 300 rpm.

[0098] The stirring speed when adding the initiator was 50 rpm.

[0099] The condition for vacuum degassing is that the vacuum degree is less than -90Kpa.

[0100] Example 2

[0101] A UV structural adhesive was prepared, and the raw materials for preparation were:

[0102] Polyurethane modified acrylic resin: 48 parts,

[0103] Diluted monomer: 20 parts,

[0104] Silicone modified acrylate: 3 parts,

[0105] Modified wet mica powder: 20 parts,

[0106] Coupling agent: 1 part,

[0107] Adhesion promoter: 1 part,

[0108] Thixotropic agent: 2 parts,

[0109] Initiator: 4 parts.

[0110] In the preparation of raw materials:

[0111] The polyurethane modified acrylic resin is Lancolu L-8405C.

[0112] The diluent monomer is dimethyl acrylamide.

[0113] The preparation method of silicone-modified acrylate is as follows: weigh 1 mol of terminal methyl dimethoxy silicone oil (viscosity 1000-2000 cps) in a three-necked flask, gradually add 2.2 mol of γ-methacryloxypropyltrimethoxysilane, and after the addition is completed, heat to 40° C., react for 2 hours, then add 0.2% of dibutyltin dilaurate, and react for another hour. After the reaction is completed, cool to room temperature, wash with petroleum ether, and dry to obtain the final product KH-SJ.

[0114] The preparation method of modified mica powder is:

[0115] 1. Prepare 50g solution of deionized water and anhydrous ethanol in a ratio of 1:1 and place it in a 200mL beaker. Then weigh 16.67g of hexadecyltrimethoxysilane and place it in it. Use glacial acetic acid to adjust the pH of the solution to 4-5. Place it in a 60℃ water bath with stirring and heating to promote the pre-hydrolysis of the modifier for standby use.

[0116] 2. Weigh 1 kg of wet mica powder and place it in a high-speed mixer. Pre-disperse and mix for 5 minutes. Weigh the silane modifier that has been pre-hydrolyzed in step 1 above and add it three times. Mix at high speed for 20 minutes. Dry the material and test it for later use. The amount of silane modifier is 1.5%.

[0117] The coupling agent is vinyltrimethoxysilane.

[0118] The adhesion promoter is EM39.

[0119] The thixotropic agent is silica.

[0120] The initiator is 2 parts of 184 initiator and 2 parts of 20400 initiator.

[0121] The preparation method of the UV structural adhesive in this embodiment is as follows: after mixing polyurethane modified acrylic resin, diluent monomer, organosilicon modified acrylate and modified mica powder, stirring and dispersing, adding coupling agent, adhesion promoter and thixotropic agent, dispersing evenly, and finally adding initiator, stirring evenly and vacuum degassing.

[0122] Polyurethane modified acrylic resin, diluent monomer, organosilicon modified acrylate and modified mica powder were mixed in a planetary mill with a stirring speed of 10 rpm and a dispersing speed of 300 rpm.

[0123] After adding coupling agent, adhesion promoter and thixotropic agent, the stirring speed was 50 rpm and the dispersion speed was 300 rpm.

[0124] The stirring speed when adding the initiator was 50 rpm.

[0125] The condition for vacuum degassing is that the vacuum degree is less than -90Kpa.

[0126] Example 3

[0127] A UV structural adhesive was prepared, and the raw materials for preparation were:

[0128] Polyurethane modified acrylic resin: 53 parts,

[0129] Diluted monomer: 20 parts,

[0130] Silicone modified acrylate: 5 parts,

[0131] Modified synthetic mica powder: 15 parts,

[0132] Coupling agent: 1 part,

[0133] Adhesion promoter: 1 part,

[0134] Thixotropic agent: 2 parts,

[0135] Initiator: 4 parts.

[0136] In the preparation of raw materials:

[0137] The polyurethane modified acrylic resin is Lancolu L-8405C.

[0138] The diluent monomer is dimethyl acrylamide.

[0139] The preparation method of silicone-modified acrylate is as follows: weigh 1 mol of terminal methyl dimethoxy silicone oil (viscosity 1000-2000 cps) in a three-necked flask, gradually add 2.2 mol of γ-methacryloxypropyltrimethoxysilane, and after the addition is completed, heat to 40° C., react for 2 hours, then add 0.2% of dibutyltin dilaurate, and react for another hour. After the reaction is completed, cool to room temperature, wash with petroleum ether, and dry to obtain the final product KH-SJ.

[0140] The preparation method of modified mica powder is:

[0141] 1. Prepare 50g solution of deionized water and anhydrous ethanol in a ratio of 1:1 and place it in a 200mL beaker. Then weigh 16.67g of methyltrimethoxysilane and place it in it. Use glacial acetic acid to adjust the pH of the solution to 4-5. Place it in a 60℃ water bath and stir and heat to promote the pre-hydrolysis of the modifier for use.

[0142] 2. Weigh 1 kg of synthetic mica powder and place it in a high-speed mixer. Pre-disperse and mix for 5 minutes. Weigh the silane modifier that has been pre-hydrolyzed in step 1 above and add it three times. Mix at high speed for 20 minutes. Dry the material and test it for later use. The amount of silane modifier is 1.5%.

[0143] The coupling agent is aminopropyltriethoxysilane.

[0144] The adhesion promoter is EM39.

[0145] The thixotropic agent is silica.

[0146] The initiator is 0500 initiator.

[0147] The preparation method of the UV structural adhesive in this embodiment is as follows: after mixing polyurethane modified acrylic resin, diluent monomer, organosilicon modified acrylate and modified mica powder, stirring and dispersing, adding coupling agent, adhesion promoter and thixotropic agent, dispersing evenly, and finally adding initiator, stirring evenly and vacuum degassing.

[0148] Polyurethane modified acrylic resin, diluent monomer, organosilicon modified acrylate and modified mica powder were mixed in a planetary mill with a stirring speed of 10 rpm and a dispersing speed of 300 rpm.

[0149] After adding coupling agent, adhesion promoter and thixotropic agent, the stirring speed was 50 rpm and the dispersion speed was 300 rpm.

[0150] The stirring speed when adding the initiator was 50 rpm.

[0151] The condition for vacuum degassing is that the vacuum degree is less than -90Kpa.

[0152] Example 4

[0153] A UV structural adhesive was prepared, and the raw materials for preparation were:

[0154] Polyurethane modified acrylic resin: 48 parts,

[0155] Diluted monomer: 25 parts,

[0156] Silicone modified acrylate: 5 parts,

[0157] Modified synthetic mica powder: 20 parts,

[0158] Coupling agent: 1 part,

[0159] Adhesion promoter: 1.5 parts,

[0160] Thixotropic agent: 2 parts,

[0161] Initiator: 4 parts.

[0162] In the preparation of raw materials:

[0163] The polyurethane modified acrylic resin is Laromer UA9065.

[0164] The diluent monomer is hydroxyethyl methacrylate.

[0165] The preparation method of silicone-modified acrylate is as follows: weigh 1 mol of terminal methyl dimethoxy silicone oil (viscosity 1000-2000 cps) in a three-necked flask, gradually add 2.2 mol of γ-methacryloxypropyltrimethoxysilane, and after the addition is completed, heat to 40° C., react for 2 hours, then add 0.2% of dibutyltin dilaurate, and react for another hour. After the reaction is completed, cool to room temperature, wash with petroleum ether, and dry to obtain the final product KH-SJ.

[0166] The preparation method of modified mica powder is:

[0167] 1. Prepare 50g solution of deionized water and anhydrous ethanol in a ratio of 1:1 and place it in a 200mL beaker. Then weigh 16.67g of γ-methacryloxypropyltrimethoxysilane and place it in it. Use glacial acetic acid to adjust the pH of the solution to 4-5. Place it in a 60℃ water bath with stirring and heating to promote the pre-hydrolysis of the modifier for standby use.

[0168] 2. Weigh 1 kg of synthetic mica powder and place it in a high-speed mixer. Pre-disperse and mix for 5 minutes. Weigh the silane modifier that has been pre-hydrolyzed in step 1 above and add it three times. Mix at high speed for 20 minutes. Dry the material and test it for later use. The amount of silane modifier is 1.5%.

[0169] The coupling agent is vinyl tris(methoxyethoxy)silane.

[0170] The adhesion promoter is Lencolo 4051.

[0171] The thixotropic agent is silica.

[0172] The initiator is 1 part of 184 initiator + 3 parts of BP initiator.

[0173] The preparation method of the UV structural adhesive in this embodiment is as follows: after mixing polyurethane modified acrylic resin, diluent monomer, organosilicon modified acrylate and modified mica powder, stirring and dispersing, adding coupling agent, adhesion promoter and thixotropic agent, dispersing evenly, and finally adding initiator, stirring evenly and vacuum degassing.

[0174] Polyurethane modified acrylic resin, diluent monomer, organosilicon modified acrylate and modified mica powder were mixed in a planetary mill with a stirring speed of 10 rpm and a dispersing speed of 300 rpm.

[0175] After adding coupling agent, adhesion promoter and thixotropic agent, the stirring speed was 50 rpm and the dispersion speed was 300 rpm.

[0176] The stirring speed when adding the initiator was 50 rpm.

[0177] The condition for vacuum degassing is that the vacuum degree is less than -90Kpa.

[0178] Example 5

[0179] A UV structural adhesive was prepared, and the raw materials for preparation were:

[0180] Polyurethane modified acrylic resin: 48 parts,

[0181] Diluted monomer: 25 parts,

[0182] Silicone modified acrylate: 7 parts,

[0183] Modified synthetic mica powder: 20 parts,

[0184] Coupling agent: 1.5 parts,

[0185] Adhesion promoter: 1 part,

[0186] Thixotropic agent: 4 parts,

[0187] Initiator: 5 parts.

[0188] In the preparation of raw materials:

[0189] The polyurethane modified acrylic resin is EBECRYL246.

[0190] The diluent monomer is isobornyl acrylate.

[0191] The preparation method of silicone-modified acrylate is as follows: weigh 1 mol of terminal methyl dimethoxy silicone oil (viscosity 1000-2000 cps) in a three-necked flask, gradually add 2.2 mol of γ-methacryloxypropyltrimethoxysilane, and after the addition is completed, heat to 40° C., react for 2 hours, then add 0.2% of dibutyltin dilaurate, and react for another hour. After the reaction is completed, cool to room temperature, wash with petroleum ether, and dry to obtain the final product KH-SJ.

[0192] The preparation method of modified mica powder is:

[0193] 1. Prepare 50g solution of deionized water and anhydrous ethanol in a ratio of 1:1 and place it in a 200mL beaker. Then weigh 16.67g of γ-methacryloxypropyltrimethoxysilane and place it in it. Use glacial acetic acid to adjust the pH of the solution to 4-5. Place it in a 60℃ water bath with stirring and heating to promote the pre-hydrolysis of the modifier for standby use.

[0194] 2. Weigh 1 kg of synthetic mica powder and place it in a high-speed mixer. Pre-disperse and mix for 5 minutes. Weigh the silane modifier that has been pre-hydrolyzed in step 1 above and add it three times. Mix at high speed for 20 minutes. Dry the material and test it for later use. The amount of silane modifier is 1.5%.

[0195] The coupling agent is vinyltriethoxysilane.

[0196] The adhesion promoter is Lencolo 4051.

[0197] The thixotropic agent is silica.

[0198] The initiator was Lencolo 5032 initiator.

[0199] The preparation method of the UV structural adhesive in this embodiment is as follows: after mixing polyurethane modified acrylic resin, diluent monomer, organosilicon modified acrylate and modified mica powder, stirring and dispersing, adding coupling agent, adhesion promoter and thixotropic agent, dispersing evenly, and finally adding initiator, stirring evenly and vacuum degassing.

[0200] Polyurethane modified acrylic resin, diluent monomer, organosilicon modified acrylate and modified mica powder were mixed in a planetary mill with a stirring speed of 10 rpm and a dispersing speed of 300 rpm.

[0201] After adding coupling agent, adhesion promoter and thixotropic agent, the stirring speed was 50 rpm and the dispersion speed was 300 rpm.

[0202] The stirring speed when adding the initiator was 50 rpm.

[0203] The condition for vacuum degassing is that the vacuum degree is less than -90Kpa.

[0204] Comparative Example 1

[0205] A UV structural adhesive was prepared, and the raw materials for preparation were:

[0206] Polyurethane modified acrylic resin: 48 parts,

[0207] Diluted monomer: 20 parts,

[0208] Coupling agent: 1 part,

[0209] Adhesion promoter: 1 part,

[0210] Thixotropic agent: 4 parts,

[0211] Initiator: 4 parts.

[0212] In the preparation of raw materials:

[0213] The polyurethane modified acrylic resin is L-6120.

[0214] The diluent monomer is dimethyl acrylamide.

[0215] The coupling agent is vinyltrimethoxysilane.

[0216] The adhesion promoter is EM39.

[0217] The thixotropic agent is silica.

[0218] The initiator is 184 initiator.

[0219] The preparation method of the UV structural adhesive in this embodiment is: after mixing the polyurethane modified acrylic resin and the diluent monomer, stirring and dispersing, adding the coupling agent, the adhesion promoter and the thixotropic agent, dispersing them evenly, and finally adding the initiator, stirring evenly and vacuum degassing.

[0220] Polyurethane modified acrylic resin, diluent monomer, organosilicon modified acrylate and modified mica powder were mixed in a planetary mill with a stirring speed of 10 rpm and a dispersing speed of 300 rpm.

[0221] After adding coupling agent, adhesion promoter and thixotropic agent, the stirring speed was 50 rpm and the dispersion speed was 300 rpm.

[0222] The stirring speed when adding the initiator was 50 rpm.

[0223] The condition for vacuum degassing is that the vacuum degree is less than -90Kpa.

[0224] Comparative Example 2

[0225] A UV structural adhesive was prepared, and the raw materials for preparation were:

[0226] Polyurethane modified acrylic resin: 50 parts,

[0227] Diluted monomer: 25 parts,

[0228] Coupling agent: 1 part,

[0229] Adhesion promoter: 1.5 parts,

[0230] Thixotropic agent: 5 parts,

[0231] Initiator: 4 parts.

[0232] In the preparation of raw materials:

[0233] The polyurethane modified acrylic resin is L-6122C.

[0234] The diluent monomer is hydroxyethyl methacrylate.

[0235] The coupling agent is vinyltrimethoxysilane.

[0236] The adhesion promoter is EM39.

[0237] The thixotropic agent is silica.

[0238] The initiator is 1173 initiator.

[0239] The preparation method of the UV structural adhesive in this embodiment is: after mixing the polyurethane modified acrylic resin and the diluent monomer, stirring and dispersing, adding the coupling agent, the adhesion promoter and the thixotropic agent, dispersing them evenly, and finally adding the initiator, stirring evenly and vacuum degassing.

[0240] Polyurethane modified acrylic resin, diluent monomer, organosilicon modified acrylate and modified mica powder were mixed in a planetary mill with a stirring speed of 10 rpm and a dispersing speed of 300 rpm.

[0241] After adding coupling agent, adhesion promoter and thixotropic agent, the stirring speed was 50 rpm and the dispersion speed was 300 rpm.

[0242] The stirring speed when adding the initiator was 50 rpm.

[0243] The condition for vacuum degassing is that the vacuum degree is less than -90Kpa.

[0244] Performance Testing

[0245] The properties of the UV structural adhesives prepared in Examples 1 to 5 and Comparative Examples 1 and 2 were tested, and the results are shown in Table 2.

[0246] Table 2

[0247]

[0248] In Table 2, the viscosity test standard is ASTM D4287, the shear rate is 5- S (refers to the viscosity under the condition of shear rate of 5 / S. Because the shear rate is different, the viscosity obtained is different).

[0249] The thixotropic index test standard is GB / T 2794-2022, 0.5 / 5 - S (Regarding the definition of thixotropic index, the national standard usually refers to the viscosity at 0.5rpm divided by the viscosity at 5rpm).

[0250] Adhesion was tested by the 100-grid method.

[0251] The standard for peel strength test is GB / T 2792-2014.

[0252] The standard for water vapor transmission rate test is GB 1037-2021.

[0253] From the test results in Table 2, it can be seen that the introduction of modified mica powder and silicone-modified acrylate can effectively improve the water vapor isolation, adhesion to glass and moisture and heat resistance of the UV glue itself.

[0254] The present invention has been described in detail above in conjunction with the embodiments, but the present invention is not limited to the above embodiments, and various changes can be made within the knowledge scope of ordinary technicians in the relevant technical field without departing from the purpose of the present invention.

Claims

1. A UV structural adhesive, characterized in that: The preparation raw materials include polyurethane modified acrylic resin, diluent monomer, organosilicon modified acrylate, modified mica powder, coupling agent, adhesion promoter, thixotropic agent and initiator.

2. The UV structural adhesive according to claim 1, characterized in that: In parts by weight, the raw materials for preparation include: polyurethane modified acrylic resin: 45 parts to 55 parts, Diluent: 20 to 30 parts, Silicone modified acrylate: 2 to 7 parts, Modified mica powder: 10 to 25 parts, Coupling agent: 0.5 to 2 parts, Adhesion promoter: 0.5 to 2 parts, Thixotropic agent: 1 to 5 parts, Initiator: 2 to 6 parts.

3. The UV structural adhesive according to claim 1 or 2, characterized in that: The polyurethane modified acrylic resin includes at least one of L-8402, L-8403, L-8405C, L-8412A, L-8414, L-8442, BASF Laromer UA 9065, allnex EBECRYL246 and allnex EBECRYL8894.

4. The UV structural adhesive according to claim 1 or 2, characterized in that: The preparation method of the organosilicon-modified acrylate comprises: dropping gamma-methacryloxypropyltrimethoxysilane into terminal methyl dimethoxy silicone oil, heating the reaction, and then dropping dibutyltin dilaurate for reaction.

5. The UV structural adhesive according to claim 1 or 2, characterized in that: The preparation method of the modified mica powder comprises: (1) dissolving a silane modifier in an alcohol solution, adjusting the pH, and then heating to obtain a pre-hydrolyzed silane modifier; (2) After the mica powder is dispersed, the pre-hydrolyzed silane modifier is added, mixed at high speed, and then dried.

6. The UV structural adhesive according to claim 1 or 2, characterized in that: The diluent monomer includes at least one of dimethyl acrylamide, hydroxyethyl methacrylate, hydroxypropyl methacrylate, isobornyl acrylate, lauryl acrylate and cyclohexyl methacrylate.

7. The UV structural adhesive according to claim 1 or 2, characterized in that: The coupling agent includes at least one of vinyl trimethoxy silane, vinyl tri (methoxyethoxy) silane, vinyl triethoxy silane and aminopropyl triethoxy silane.

8. The UV structural adhesive according to claim 1 or 2, characterized in that: The initiator includes at least one of 184, BP, Omnirad500, TR-NPI-20400, 819, ITX and Lencolo 5032.

9. A method for preparing the UV structural adhesive according to any one of claims 1 to 8, characterized in that: The method comprises the following steps: mixing the polyurethane modified acrylic resin, diluent monomer, organosilicon modified acrylate and modified mica powder, stirring and dispersing them, adding the coupling agent, adhesion promoter and thixotropic agent, dispersing them uniformly, and finally adding the initiator, stirring and degassing them uniformly.

10. An OLED display device, characterized in that: The OLED display device comprises the UV structural adhesive according to any one of claims 1 to 8.

Citation Information

Cited By

  • High-pressure oxide skin cleaning system