Method for improving corrosion resistance of magnesium alloy
By generating composite protective films such as MgCO3 and CaCO3 on the surface of magnesium alloy, the problem of poor corrosion resistance of magnesium alloy is solved, and efficient corrosion resistance improvement and environmentally friendly and low-energy consumption are achieved, which extends corrosion resistance time and reduces industrial risk.
Patent Information
- Application Number
- CN202410985895.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-07-23
AI Technical Summary
The corrosion resistance of magnesium alloys is poor, resulting in extremely fast corrosion rate, which limits its use in industrial applications. The existing surface treatment technology has problems such as environmental pollution, complex processes and limited film performance, making it difficult to produce in large-scale production. Meet environmental protection and low energy consumption requirements.
By thermal oxidation treatment under a mixed atmosphere on the surface of the magnesium alloy, a composite protective film with the outer layer film MgCO3 and CaCO3 and the inner layer film CaO, MgO and Al2O3 is generated to improve the corrosion resistance of the magnesium alloy.
It significantly improves the corrosion resistance of magnesium alloys, increases the electrochemical impedance by 10 times, reduces the corrosion current density by 10 times, and extends the corrosion resistance from 24 hours to 144 hours, and has less energy consumption in process and low equipment costs, which meets the requirements of green and environmental protection.
Smart Images

Figure CN119061351A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of magnesium alloy anti-corrosion, and in particular to a method for improving the corrosion resistance of magnesium alloy. Background Art
[0002] Magnesium (Mg) and its alloys have been widely used in the fields of automotive engineering, aerospace, transportation, electronics, biomedicine, etc. due to their high specific strength, good machinability, strong shock absorption performance, good electrical and thermal conductivity, etc. In recent years, the rapid development of economic, environmentally friendly and mobile society brought about by lightweight structures has made lightweight materials occupy a pivotal position. Magnesium (Mg) is one of the first choices for lightweight materials and is known as the "21st century green engineering material". However, due to the low equilibrium potential of magnesium, the magnesium matrix acts as the anode of most secondary phases, which is prone to galvanic corrosion; and the Mg surface protective film is loose and porous, easy to fall off, and cannot provide good protection for the magnesium matrix, resulting in poor corrosion resistance of magnesium alloys. The extremely fast corrosion rate seriously limits the use of magnesium and its alloys, which is the primary factor hindering its development.
[0003] At present, the research and development work to solve the corrosion problem of magnesium alloys is mainly focused on the following two aspects: 1) changing the composition of magnesium alloys, reducing harmful impurities, applying certain processing methods, and changing the organization and phase composition of magnesium alloys through alloying, thermal oxidation treatment, mechanical deformation and other processing methods; 2) surface treatment methods by isolating the metal from the atmosphere for corrosion prevention. Among them, the surface treatment technologies of magnesium alloys include chemical conversion film, anodizing, micro-arc oxidation, vapor deposition and laser surface treatment. The hexavalent chromium contained in the chromate solution in the chemical conversion film method is carcinogenic, which is very harmful to the human body and the environment, and the recycling cost is high; the thickness, chemical composition and microstructure of the coating in the anodizing method are greatly affected by the current and are difficult to control; the micro-arc oxidation area in the micro-arc oxidation method is easily affected by the surface roughness, and breakdown is very likely to occur at the groove position; vapor deposition and laser surface treatment are not suitable for processing large-scale surfaces due to high requirements for the preliminary treatment of the workpiece and high energy consumption. In addition, the protective film formed on the Mg matrix generally also has MgO, and the PBR of MgO is less than 1, which cannot isolate Cl - CaCO3 and MgCO3 have the ability to resist corrosion in Cl - The excellent properties of long-term existence in the environment and PBR≈2 have not received much attention. In short, most of the surface treatment technologies currently widely used have disadvantages such as environmental pollution, complex processes and limited film performance, which restricts their development.
[0004] Therefore, the above technical solutions have the following shortcomings in actual use: the existing methods for improving the corrosion resistance of magnesium alloys cannot meet the requirements of environmental protection and low energy consumption while meeting the requirements of large-scale production. Therefore, a method for improving the corrosion resistance of magnesium alloys that is green, environmentally friendly, has low energy consumption, contains carbonate in the protective film, and meets the requirements of large-scale production is urgently needed. Summary of the invention
[0005] The purpose of the present invention is to provide a method for improving the corrosion resistance of magnesium alloys by thermal oxidation treatment under a mixed atmosphere, so as to solve the problem that the corrosion resistance of magnesium alloys is poor and the extremely fast corrosion rate seriously limits the use of magnesium and its alloys mentioned in the above background technology. The present invention provides a method for improving the corrosion resistance of magnesium alloys that is simple to operate, low in cost, does not involve strong acids and alkalis, and is green and environmentally friendly; through this method, the corrosion resistance of magnesium and magnesium alloys can be effectively improved, the process risks and economic decline caused by the corrosion of magnesium and magnesium alloys are reduced, and the foundation for expanding the scope of use of magnesium and magnesium alloys is laid.
[0006] In order to achieve the above object, the present invention adopts the following technical solutions:
[0007] A method for improving the corrosion resistance of a magnesium alloy comprises the following steps:
[0008] Step 1: Mix carbon dioxide and oxygen with a mass fraction of 99.999% in proportion to obtain a mixed atmosphere;
[0009] Step 2: The magnesium alloy is ground and polished, and ultrasonically cleaned with ethanol, and then thermally oxidized in a heating device into which a mixed atmosphere is introduced, and the heat is kept to form a composite protective film on the surface of the magnesium alloy with an outer layer of MgCO3 and CaCO3 and an inner layer of CaO, MgO and Al2O3.
[0010] Preferably, the ratio of carbon dioxide to oxygen in step 1 is (1-3):1.
[0011] Preferably, the mixed atmosphere formed by carbon dioxide and oxygen in step 1 is introduced into the heating device at a flow rate of 150 ml / min-250 ml / min.
[0012] Preferably, the magnesium alloy is ground into 3000-7000 mesh in step 2.
[0013] Preferably, the ultrasonic cleaning with ethanol in step 2 is performed for 1 min to 5 min.
[0014] Preferably, the thermal oxidation treatment temperature in step 2 is 350°C-450°C.
[0015] Preferably, the insulation time described in step 2 is 900min-1440min.
[0016] Preferably, the outer layer of the composite protective film described in step 2 is located at the interface between the oxide film on the surface of the magnesium alloy and the mixed atmosphere; the inner layer of the composite protective film is the interface between the magnesium alloy substrate and the oxide film on the surface of the magnesium alloy.
[0017] Preferably, in step 2, the outer layer of the composite protective film has a thickness of 95-125 nm, and the inner layer has a thickness of 30-40 nm.
[0018] The beneficial effects of the present invention are:
[0019] The present invention provides a method for improving the corrosion resistance of magnesium alloys by thermal oxidation treatment under a mixed atmosphere. The method comprises the following steps: thermally oxidizing magnesium and magnesium alloys in a mixed atmosphere of carbon dioxide and oxygen to generate a composite film with an outer film thickness of 95-125nm and an inner film thickness of 30-40nm on the surface of magnesium and magnesium alloys. The composite film is flat and dense, has good adhesion, and significantly improves the corrosion resistance of magnesium and magnesium alloys. The electrochemical impedance is increased by 10 times, the corrosion current density is reduced by 10 times, and the salt spray test shows that the corrosion resistance days are increased from 24h to 144h. In addition, the method has low energy consumption, low equipment cost, simple operation process, and no strong acid and alkali in the production process, which meets the requirements of green environmental protection. The use of the method will significantly improve the utilization rate, utilization rate and market share of metal magnesium and magnesium alloys, reduce the industrial risks and economic losses caused by the high corrosion of magnesium and magnesium alloys, and lay the foundation for the promotion and development of modern industry. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 The surface scanning electron microscopic morphology of the AM60+2.0Ca magnesium alloy without thermal oxidation treatment in Example 1 after being corroded in 5wt.% NaCl salt spray for 24h, 48h and 72h and the AM60+2.0Ca magnesium alloy after being corroded in 5wt.% NaCl salt spray for 24h, 72h and 144h;
[0021] Figure 2 The cross-sectional scanning electron microscopic morphology of the AM60+2.0Ca magnesium alloy without thermal oxidation treatment in Example 1 after being corroded in 5wt.% NaCl salt spray for 24h, 48h and 72h and the AM60+2.0Ca magnesium alloy after being corroded in 5wt.% NaCl salt spray for 24h, 72h and 144h;
[0022] Figure 3The weight loss graphs of the AM60+2.0Ca magnesium alloy without thermal oxidation treatment in Example 1 after being corroded in 5wt.% NaCl salt spray for 24h, 48h and 72h and the AM60+2.0Ca magnesium alloy after being corroded in 5wt.% NaCl salt spray for 24h, 72h and 144h;
[0023] Figure 4 Nyquist plots of the AM60+2.0Ca magnesium alloys that have not been subjected to thermal oxidation treatment and have been subjected to thermal oxidation treatment in Example 1;
[0024] Figure 5 The polarization curves of the AM60+2.0Ca magnesium alloys without thermal oxidation treatment and after thermal oxidation treatment in Example 1;
[0025] Figure 6 Schematic diagram of TEM test results of the composite protective film on the surface of magnesium alloy after thermal oxidation treatment. DETAILED DESCRIPTION
[0026] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.
[0027] An embodiment of the present invention provides a method for improving the corrosion resistance of a magnesium alloy, which comprises the following steps:
[0028] (1) Mix carbon dioxide and oxygen with a mass fraction of 99.999% in a uniform proportion;
[0029] (2) The magnesium alloy is ground and polished, ultrasonically cleaned with ethanol, and then thermally oxidized in a tubular furnace into which a mixed atmosphere is introduced. The temperature is kept for a certain period of time to form an outer film of MgCO3 and CaCO3 and an inner film of a composite film of CaO, MgO and Al2O3 on the surface of the magnesium alloy, thereby improving the corrosion resistance of magnesium and magnesium alloys.
[0030] As another preferred embodiment of the present invention, the mixed atmosphere is a mixed gas of CO2:O2=1:1-1:3. If the CO2 content is too high, it will act as a protective gas and fail to form a protective film. If the O2 content is too high, the generated protective film will break and the base metal will be directly oxidized.
[0031] As another preferred embodiment of the present invention, the magnesium alloy needs to be polished to 3000-7000 meshes. If the mesh is less than 3000, the metal surface will be scratched obviously, and corrosion will occur preferentially at the scratches.
[0032] As another preferred embodiment of the present invention, the ultrasonic cleaning with ethanol has a cleaning time of 1 min-5 min.
[0033] As another preferred embodiment of the present invention, the thermal oxidation treatment temperature is 400° C.-450° C. If the thermal oxidation treatment temperature is too high, the alloy will be preferentially oxidized, and if it is too low, the thickness of the outer layer MgCO3 and CaCO3 film formed will be insufficient.
[0034] As another preferred embodiment of the present invention, the thermal oxidation treatment holding time is 600min-1200min. Too short a holding time will result in insufficient thickness of the outer layer MgCO3 and CaCO3 film formed, while too long a holding time will result in a waste of energy.
[0035] As another preferred embodiment of the present invention, the flow rate of CO2 and O2 forming a mixed atmosphere during the thermal oxidation treatment is 150ml / min-250ml / min.
[0036] Embodiment 1:
[0037] An embodiment of the present invention provides a method for improving the corrosion resistance of a magnesium alloy by thermal oxidation treatment in a mixed atmosphere, which comprises the following steps:
[0038] (1) mixing carbon dioxide with a mass fraction of 99.999% and oxygen in a uniform proportion to form a mixed atmosphere with a carbon dioxide to oxygen mixing ratio of 1:3;
[0039] (2) AM60+2.0Ca magnesium alloy was ground to 5000 mesh. Then it was polished with diamond polishing paste, and the polished sample was placed in ethanol for ultrasonic cleaning for 3 minutes, and the sample was taken out and dried with cold air;
[0040] (3) The sample after being dried by cold air was placed in a tube furnace into which a mixed atmosphere was introduced for thermal oxidation treatment. The thermal oxidation treatment temperature was 440°C, the thermal oxidation treatment holding time was 900 min, and the flow rate of the mixed atmosphere formed by CO2 and O2 during the thermal oxidation treatment was 200 ml / min;
[0041] (4) After cooling to room temperature in the furnace, a corrosion-resistant magnesium product is obtained, wherein the outer layer is a composite film of MgCO3 and CaCO3, and the inner layer is a composite film of CaO, MgO and Al2O3.
[0042] Embodiment 2:
[0043] An embodiment of the present invention provides a method for improving the corrosion resistance of a magnesium alloy by thermal oxidation treatment in a mixed atmosphere, which comprises the following steps:
[0044] (2) The AZ80+1.5Ca magnesium alloy was ground to 5000 mesh and then polished with diamond polishing paste. The polished sample was placed in ethanol for ultrasonic cleaning for 3 min, and the sample was taken out and dried with cold air;
[0045] (1), (3) and (4) are the same as in Example 1.
[0046] Embodiment 3:
[0047] An embodiment of the present invention provides a method for improving the corrosion resistance of a magnesium alloy by thermal oxidation treatment in a mixed atmosphere, which comprises the following steps:
[0048] (1) mixing carbon dioxide with a mass fraction of 99.999% and oxygen in a uniform proportion to form a mixed atmosphere with a carbon dioxide to oxygen mixing ratio of 1:1.5;
[0049] (2)-(4) Same as Example 1
[0050] Embodiment 4:
[0051] An embodiment of the present invention provides a method for improving the corrosion resistance of a magnesium alloy by thermal oxidation treatment in a mixed atmosphere, which comprises the following steps:
[0052] (2) AM60+2.0Ca magnesium alloy was ground to 7000 mesh and then polished with diamond polishing paste. The polished sample was placed in ethanol for ultrasonic cleaning for 3 min and the sample was taken out and dried with cold air;
[0053] (1), (3) and (4) are the same as in Example 1.
[0054] Embodiment 5:
[0055] An embodiment of the present invention provides a method for improving the corrosion resistance of a magnesium alloy by thermal oxidation treatment in a mixed atmosphere, which comprises the following steps:
[0056] (3) The sample after being dried by cold air is placed in a tube furnace into which a mixed atmosphere is introduced for thermal oxidation treatment. The thermal oxidation treatment temperature is 400° C., the thermal oxidation treatment holding time is 900 min, and the flow rate of the mixed atmosphere formed by carbon dioxide and oxygen during the thermal oxidation treatment is 200 ml / min;
[0057] (1), (2) and (4) are the same as in Example 1.
[0058] Embodiment 6:
[0059] An embodiment of the present invention provides a method for improving the corrosion resistance of a magnesium alloy by thermal oxidation treatment in a mixed atmosphere, which comprises the following steps:
[0060] (3) The sample after being dried by cold air was placed in a tube furnace into which a mixed atmosphere was introduced for thermal oxidation treatment. The thermal oxidation treatment temperature was 440°C, the thermal oxidation treatment holding time was 1440 min, and the flow rate of the mixed atmosphere formed by carbon dioxide and oxygen during the thermal oxidation treatment was 200 ml / min;
[0061] (1), (2) and (4) are the same as in Example 1.
[0062] Embodiment 7:
[0063] An embodiment of the present invention provides a method for improving the corrosion resistance of a magnesium alloy by thermal oxidation treatment in a mixed atmosphere, which comprises the following steps:
[0064] (1) mixing carbon dioxide with a mass fraction of 99.999% and oxygen in a uniform proportion to form a mixed atmosphere with a carbon dioxide to oxygen mixing ratio of 1:1.5;
[0065] (2)-(4) Same as Example 2
[0066] Embodiment 8:
[0067] An embodiment of the present invention provides a method for improving the corrosion resistance of a magnesium alloy by thermal oxidation treatment in a mixed atmosphere, which comprises the following steps:
[0068] (2) Grind the AZ80+1.5Ca magnesium alloy to 7000 mesh. Then polish it with diamond polishing paste, place the polished sample in ethanol for ultrasonic cleaning for 3 minutes, take out the sample and blow dry it with cold air;
[0069] (1), (3) and (4) are the same as those in Example 2.
[0070] Embodiment 9:
[0071] An embodiment of the present invention provides a method for improving the corrosion resistance of a magnesium alloy by thermal oxidation treatment in a mixed atmosphere, which comprises the following steps:
[0072] (3) The sample after being dried by cold air is placed in a tube furnace into which a mixed atmosphere is introduced for thermal oxidation treatment. The thermal oxidation treatment temperature is 400° C., the thermal oxidation treatment holding time is 900 min, and the flow rate of the mixed atmosphere formed by carbon dioxide and oxygen during the thermal oxidation treatment is 200 ml / min;
[0073] (1), (2) and (4) are the same as those in Example 2.
[0074] Embodiment 10:
[0075] An embodiment of the present invention provides a method for improving the corrosion resistance of a magnesium alloy by thermal oxidation treatment in a mixed atmosphere, which comprises the following steps:
[0076] (3) The sample after being dried by cold air was placed in a tube furnace into which a mixed atmosphere was introduced for thermal oxidation treatment. The thermal oxidation treatment temperature was 440°C, the thermal oxidation treatment holding time was 1440 min, and the flow rate of the mixed atmosphere formed by carbon dioxide and oxygen during the thermal oxidation treatment was 200 ml / min;
[0077] (1), (2) and (4) are the same as those in Example 2.
[0078] The experimental analysis of the above embodiments leads to the following conclusions:
[0079] See also Figure 1-3 The scanning electron microscopic morphology and weight loss rate of AM60+2.0Ca without thermal oxidation treatment after corrosion in 3.5wt% NaCl salt spray for 24h, 48h and 72h and AM60+2.0Ca with mixed atmosphere thermal oxidation treatment after corrosion in 3.5wt% NaCl salt spray for 24h, 72h and 144h are shown. For the AM60+2.0Ca alloy without thermal oxidation treatment, serious corrosion has occurred on the surface after 24h. As the corrosion time increases, the corrosion pits on the alloy surface gradually grow, and almost occupy the entire alloy surface at 72h. For the AM60+2.0Ca alloy with thermal oxidation treatment, only slight corrosion occurs on the matrix near the grain boundary after 24h. At 72h, the corrosion gradually expands along the matrix, but until 144h, some of the AM60+2.0Ca alloy surfaces that have been thermally oxidized are still not corroded. The depth of the corrosion pit of the AM60+2.0Ca alloy that has not been thermally oxidized has reached 65μm after 24h of corrosion, and the depth of the corrosion pit reaches 120μm when the corrosion time reaches 72h. The depth of the corrosion pit of the AM60+2.0Ca alloy that has been thermally oxidized is extremely small after 24h of corrosion, and the depth of the corrosion pit only increases to 20μm when the corrosion time is extended to 144h (significantly less than 65μm of the AM60+2.0Ca alloy that has not been thermally oxidized after 24h of corrosion). The corresponding energy spectrum shows that the corrosion pit first appears near the grain boundary, which is related to the occurrence of microgalvanic corrosion. The salt spray test shows that the corrosion resistance days are increased from 24h to 144h. And the weight loss rate of the AM60+2.0Ca alloy that has been thermally oxidized in 144h is one tenth of the weight loss rate of the AM60+2.0Ca alloy that has not been thermally oxidized in 72h. This shows that the composite protective film with the outer film of MgCO3 and CaCO3 and the inner film of CaO, MgO and Al2O3 can slow down the corrosion rate of magnesium alloy.
[0080] See also Figure 4-5 The Nyquist diagram and polarization curve of AM60+2.0Ca alloy without thermal oxidation treatment and after mixed atmosphere thermal oxidation treatment are shown. The Nyquist diagram of AM60+2.0Ca alloy without thermal oxidation treatment shows a capacitive arc in the high frequency region and an inductive arc in the low frequency region (only the charge transfer resistance is 296.9Ωcm 2 ), and the corrosion potential is lower (-1.56V), and the corrosion current is larger (112.8μA cm -2), which indicates that the corrosion process of AM60+2.0Ca alloy is relatively rapid. The Nyquist diagram of AM60+2.0Ca alloy treated by mixed atmosphere thermal oxidation shows two capacitive arcs in high frequency region and one inductive arc in low frequency region, and the radius of the capacitive arc is larger (the charge transfer resistance and surface film resistance are 3634.2Ωcm in total). 2 ), the corrosion potential is higher (-1.48V), and the corrosion current is smaller (14.26μA cm -2 ), indicating that the composite protective film with the outer layer of MgCO3 and CaCO3 and the inner layer of CaO, MgO and Al2O3 can improve the corrosion resistance of magnesium alloy.
[0081] Figure 6 The TEM test results of AM60+2.0Ca (CO2:O2 3:1) alloy after thermal oxidation treatment are shown. Figure 6 (a)-(f) show the STEM images of the cross-section protective layer of AM60+2.0Ca alloy after thermal oxidation treatment and the corresponding energy spectra of Mg, Al, Ca, O and C. Figure 6 The cross-sectional STEM images and corresponding energy spectra in (a)-(f) show that the signals of Mg, Ca, O, and C can be detected throughout the surface protective layer, while the signal of C is mainly distributed in the outer layer. The signal of Al can only be measured in the area close to the substrate. Therefore, the MgCO3 and CaCO3 protective films formed by the mixed atmosphere thermal oxidation treatment are the main reasons for improving the corrosion resistance of the AM60+2.0Ca alloy.
[0082] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A method for improving the corrosion resistance of a magnesium alloy, characterized in that: The following steps are involved: Step 1: Mix carbon dioxide and oxygen with a mass fraction of 99.999% in proportion to obtain a mixed atmosphere; Step 2: The magnesium alloy is ground and polished, and ultrasonically cleaned with ethanol, and then thermally oxidized in a heating device into which a mixed atmosphere is introduced, and the heat is kept to form a composite protective film on the surface of the magnesium alloy with an outer layer of MgCO3 and CaCO3 and an inner layer of CaO, MgO and Al2O3.
2. A method for improving the corrosion resistance of magnesium alloy according to claim 1, characterized in that: The ratio of carbon dioxide to oxygen described in step 1 is (1-3):
1.
3. The method for improving the corrosion resistance of magnesium alloy according to claim 1, characterized in that: The mixed atmosphere formed by carbon dioxide and oxygen described in step 1 is introduced into the heating device at a flow rate of 150ml / min-250ml / min.
4. The method for improving the corrosion resistance of magnesium alloy according to claim 1, characterized in that: The magnesium alloy is ground to 3000-7000 mesh as described in step 2.
5. The method for improving the corrosion resistance of magnesium alloy according to claim 1, characterized in that: The duration of ultrasonic cleaning with ethanol in step 2 is 1 min to 5 min.
6. The method for improving the corrosion resistance of magnesium alloy according to claim 1, characterized in that: The thermal oxidation treatment temperature in step 2 is 350°C-450°C.
7. The method for improving the corrosion resistance of magnesium alloy according to claim 1, characterized in that: The holding time described in step 2 is 900min-1440min.
8. The method for improving the corrosion resistance of magnesium alloy according to claim 1, characterized in that: The outer layer of the composite protective film described in step 2 is located at the interface between the oxide film on the surface of the magnesium alloy and the mixed atmosphere; the inner layer of the composite protective film is the interface between the magnesium alloy substrate and the oxide film on the surface of the magnesium alloy.
9. The method for improving the corrosion resistance of magnesium alloy according to claim 1, characterized in that: In step 2, the outer layer of the composite protective film has a thickness of 95-125 nm, and the inner layer has a thickness of 30-40 nm.
Citation Information
Patent Citations
Catalytic oxidizer and process method for preparing corrosion resistant ceramic membranes
CN102864406A
Medical implant comprising biodegradable magnesium-ased alloy and method for its manufacture
CN103260660A
Anti-corrosion method of magnesium and magnesium alloy and application of MgCO3 layer as anti-corrosion layer
CN106381460A
Surface coating capable of improving medical magnesium alloy corrosion resistance and preparation method thereof
CN110512202A
Device and method for performing anti-corrosion treatment on magnesium and magnesium alloy by using supercritical carbon dioxide