Preparation method of multi-stage composite fiber based on hollow microsphere soft gel

By combining hollow microbeads with polyvinyl alcohol, core-shell structure composite fibers are prepared using spinning technology, which solves the problem of hollow microspheres being prone to cracking and falling off on the fiber membrane, and achieves the flexibility, high temperature resistance and thermal insulation properties of the fibers Improvement.

CN119061526AActive Publication Date: 2024-12-03ZHEJIANG SCI-TECH UNIV

Patent Information

Application Number
CN202411226419.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-03
Publication Date
2024-12-03
Estimated Expiration
2044-09-03

AI Technical Summary

Technical Problem

Existing hollow microspheres are prone to cracking and falling off on the fiber membrane, affecting thermal insulation, thermal stability and high temperature resistance.

Method used

Hollow microbead soft gel is combined with polyvinyl alcohol to prepare core-shell structure composite fibers through spinning technology to form a dense protective layer to prevent hollow microbeads from leaking and improve flexibility.

Benefits of technology

It achieves excellent flexibility, high temperature resistance, strong heat insulation and impact resistance, and is easy to control and stable, avoids the problem of hollow microbeads falling off, and improves the mechanical strength and thermal insulation performance of the fiber.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119061526A_ABST
    Figure CN119061526A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of multistage composite fibers based on hollow microsphere soft gel, which comprises the following steps: adding a proper amount of hollow microspheres into a certain amount of polyvinyl alcohol aqueous solution, and stirring at different rotating speeds to obtain a flowable gel-state soft substance; under the conditions of different drafting speeds and temperatures, the obtained gel-state soft substance is subjected to wire drawing and stretching, and polyvinyl alcohol / hollow microsphere composite fibers with different diameters are obtained; and dipping the composite fiber into another polymer solution for a period of time, taking out and drying to obtain the multi-stage composite fiber of the polyvinyl alcohol / hollow microsphere and polymer with the core-shell structure. The multi-stage composite fiber not only has excellent flexibility and tensile strength, but also has excellent performances such as portability, softness, wearable performance and impact resistance, can well meet the requirements of practical application, and has huge application potential in the fields of heat insulation, fire fighting, impact resistance and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of synthesis and preparation of organic-inorganic hybrid materials, and relates to a method for preparing multi-level composite fibers based on hollow microsphere soft gel. Background Art

[0002] Core-shell structure composite fiber is a functional composite fiber with excellent performance of both core layer and shell layer, which usually has better performance than core layer and shell layer, such as controllable mechanical strength and good thermal conductivity. Its special structure greatly improves the use value of fiber and broadens the application field of fiber. The core-shell structure fiber prepared by controlling temperature, humidity, drawing speed, etc. can give full play to the characteristics of small fiber diameter, large specific surface area and high porosity.

[0003] Chinese patent CN202010096276.X discloses a super-hydrophobic nanofiber membrane and preparation method for oily wastewater treatment, and Chinese patent CN201911043209.5 discloses a preparation method for a silica microsphere / glass fiber cloth composite thermal insulation membrane material. These patents all incorporate hollow microspheres with low thermal conductivity as fillers into the system, and use the high internal porosity and low air content of the fillers to have a great barrier effect on conduction and convection, and can achieve good thermal insulation when blended or coated. However, hollow microspheres attached to the fiber membrane are prone to cracking and falling off, affecting the thermal insulation, thermal stability, and high temperature resistance of the fiber membrane. Summary of the invention

[0004] The present invention provides a method for preparing multi-level composite fibers based on hollow microsphere soft gel, wherein the soft gel material can be quickly prepared into single fibers with a large aspect ratio by simple drawing, and the prepared fibers have the characteristics of excellent flexibility, high temperature resistance, heat insulation and strong impact resistance.

[0005] The present invention provides a method for preparing a multi-level composite fiber based on hollow microsphere soft gel, comprising the following steps:

[0006] The first step: the hollow microspheres are mixed with deionized water to obtain a uniform dispersion, and then the dispersion is added to the PVA aqueous solution and mixed, and stirred to prepare a gel-like soft material with a fluid state.

[0007] Step 2: Spinning the gel soft substance, drying and solidifying it to prepare a morphologically stable polyvinyl alcohol / hollow microbead composite fiber.

[0008] Step 3: immersing the polyvinyl alcohol / hollow microbead composite fiber in a polymer solution, taking it out and drying it, thereby obtaining a core-shell structure multi-level composite fiber with a core layer of polyvinyl alcohol / hollow microbead and a shell layer of polymer.

[0009] As the preferred technical solution:

[0010] In the first step, the stirring time for preparing the gel-like soft substance can be 0-24 hours.

[0011] In the first step, the hollow microspheres refer to hollow glass microspheres, and the particle size of the hollow microspheres is 2-60 μm. Microspheres of different particle sizes can be mixed and used.

[0012] In the first step, the flow state means that the soft gel can slowly deform under the action of gravity and external force, the automatic deformation rate under gravity is 0.001-0.5 m / s, it can deform immediately under external force, and the deformation caused by the external force can slowly disappear after the external force is removed.

[0013] In the first step, the microstructure of the gel-like soft material is as follows: the PVA on the surface of the hollow microbeads encounters the boric acid diffused from the hollow microbeads themselves and produces local flocculation in the area around the surface of the hollow microbeads, while the PVA far away from the hollow microbeads can still slide freely and play a lubricating role on the hollow microbead / flocculated PVA complex. This microstructure in which part of the PVA is locally flocculated and the other part can slide relatively makes the soft gel have both solid properties and a certain fluidity.

[0014] In the first step, the mass ratio of glass microspheres to deionized water is 1:0.1-5. The PVA accounts for 1%-20% of the total mass of the gel soft substance; the hollow microsphere dispersion accounts for 1%-10% of the total mass of the gel soft substance.

[0015] In the first step, the PVA is one of those with alcoholysis degree of 88% or 99% or a mixture of two or more thereof.

[0016] In the second step, the spinning refers to stretching spinning under the conditions of 20-55° C. and 20%-70% relative humidity, and the stretching speed is 0.1-5 m / s.

[0017] In the second step, the curing temperature is 30 to 100° C. and the highest temperature is maintained for 12 to 48 hours to remove the solvent and obtain a stable fiber morphology.

[0018] In the third step, the polymer in the polymer solution is one or more of polyurethane, polyimide, polyamide, polyvinyl pyrrolidone, polyaryl sulfone, polyacrylonitrile, polysiloxane, polyvinyl formal, and melamine formaldehyde resin.

[0019] The core layer and the shell layer of the multi-level composite fiber prepared by the present invention are tightly connected, but there is a clear interface between the shell layer and the core layer. The shell layer of the core-shell structure multi-level composite fiber is a continuous unbroken layer, which can effectively prevent the leakage of the hollow microspheres in the core layer; the PVA in the core layer can prevent the free movement of the hollow microspheres and has a damping effect.

[0020] The present invention adopts spinning technology to prepare multi-level composite fibers of polyvinyl alcohol / hollow microspheres @ polymer with a core-shell structure. The obtained single fiber inherits the high temperature resistance of silicon dioxide and has good flexibility after coating. Compared with directly blending hollow microspheres in the fiber membrane, it is easier to control and not easy to fall off. By adjusting the spinning parameters and the curing process, a multi-level composite fiber of polyvinyl alcohol / hollow microspheres @ polymer with a core-shell structure is obtained. Since the surface of the single fiber is evenly coated with the polymer solution, a dense protective layer is formed, which improves the flexibility of the single fiber. In addition, hollow microspheres have the advantages of light weight, high strength, good fluidity, heat insulation, corrosion resistance, etc., and play an increasingly important role in the development of heat insulation, wear resistance, and other composite materials, and their application in new energy industries and biomaterials has been rapidly developed.

[0021] The present invention adopts hollow microspheres to replace hollow silicon dioxide microspheres. Since the hollow microspheres themselves contain boric acid, after the hollow microspheres are dispersed in a polyvinyl alcohol solution, the polyvinyl alcohol and the surface of the hollow microspheres are cross-linked, and the mixture of the two presents a transparent substance that can flow and is in a soft gel state. The soft gel state substance has excellent biocompatibility, and can prepare continuous fibers with a large aspect ratio under external force stretching. Hollow microspheres are easy to obtain and simple to operate. Introducing hollow microspheres into polyvinyl alcohol fibers is beneficial to reducing their thermal conductivity and enhancing low-speed impact resistance. The core-shell composite fiber prepared with the hollow microspheres as the core has good mechanical strength, and effectively prevents leakage of the internal hollow microspheres, and can be used as a lightweight heat insulation, phase change, and low-speed impact resistance material. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is a SEM cross-sectional view of the multi-stage composite fiber of polyvinyl alcohol / hollow microspheres@polymer with a core-shell structure in Example 1.

[0023] Figure 2 This is a comparison diagram of the stretching of the polyvinyl alcohol / hollow microsphere fiber with a core-shell structure and the polyvinyl alcohol / hollow microsphere@polymer multi-stage composite fiber in Example 1. DETAILED DESCRIPTION

[0024] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.

[0025] Example 1

[0026] Step 1: Take 2.4g of 10-250μm hollow microbeads and 9.6g of deionized water, and ultrasonically disperse them to obtain a uniform microbead dispersion. In addition, slowly add 3.625g of PVA-1788 to 25.375g of deionized water, keep magnetic stirring in an 80°C water bath for 4h, then stop heating to obtain a 12.5% ​​PVA solution. The obtained PVA solution is mixed with the microbead dispersion and stirred at room temperature for 12h to obtain a fluid gel soft material.

[0027] Step 2: Spin the gel soft substance into composite fiber. Spinning process parameters: spinning temperature 35°C, relative humidity 40%, drawing speed 0.5m / s. Put the prepared fiber into an oven for curing, the curing temperature is 80°C, and the highest temperature is maintained for 12 hours to obtain polyvinyl alcohol / hollow microsphere composite fiber.

[0028] The third step: immersing the polyvinyl alcohol / hollow microsphere composite fiber in an aqueous polyurethane with a solid content of 60% for a period of time, taking it out and drying it in an oven at 80°C to obtain a core-shell structure multi-level composite fiber (polyvinyl alcohol / hollow microsphere@polymer multi-level composite fiber) with a core layer of polyvinyl alcohol / hollow microsphere and a shell layer of aqueous polyurethane. Figure 1 This is a SEM cross-sectional view of the multi-stage composite fiber obtained in Example 1. The fiber was subjected to a tensile test of mechanical properties. Figure 2 The tensile curves of the polyvinyl alcohol / hollow microsphere fiber with core-shell structure and the polyvinyl alcohol / hollow microsphere@waterborne polyurethane multi-stage composite fiber in Example 1. Integrating the two curves, the breaking work of the polyvinyl alcohol / hollow microsphere fiber is 0.212 J / mm 2 The breaking work of the multi-level composite fiber of polyvinyl alcohol / hollow microspheres@waterborne polyurethane is 0.583 J / mm 2 , the latter's fracture work increased to 2.75 times.

[0029] Example 2

[0030] Step 1: Take 2.4g of 10-250μm hollow microbeads and 9.6g of deionized water, and ultrasonically disperse them to obtain a uniform microbead dispersion. In addition, slowly add 3.625g of PVA-1788 to 25.375g of deionized water, keep magnetic stirring in an 80°C water bath for 4h, then stop heating to obtain a 12.5% ​​PVA solution. The obtained PVA solution is mixed with the microbead dispersion and stirred at room temperature for 12h to obtain a fluid gel soft material.

[0031] Step 2: Spin the gel soft substance into composite fiber. Spinning process parameters: spinning temperature 35°C, relative humidity 40%, drawing speed 0.5m / s. Put the prepared fiber into an oven for curing, the curing temperature is 80°C, and the highest temperature is maintained for 12 hours to obtain polyvinyl alcohol / hollow microsphere composite fiber.

[0032] Step 3: Dip the polyvinyl alcohol / hollow microsphere composite fiber in polyimide with a solid content of 15% for a period of time, take it out and dry it in an oven at 80°C to obtain a multi-level composite fiber of polyvinyl alcohol / hollow microspheres@polyimide with a core layer of polyvinyl alcohol / hollow microspheres and a shell layer of polyimide. The multi-level composite fiber is placed in the outer flame of an alcohol lamp, does not melt, and extinguishes itself when away from the flame. The limiting oxygen index of the material reaches 40%, and the material is difficult to burn.

[0033] Step 4: Fix the multi-level composite fiber on the workbench and perform a pendulum impact test on the fiber. Because the hollow microspheres are filled inside a single fiber, a large amount of impact energy is absorbed during the impact process and it is easy to break, and the impact performance is enhanced.

[0034] Example 3

[0035] Step 1: Take 2.4g of 10-250μm hollow microspheres and 9.6g of deionized water, and ultrasonically disperse them to obtain a uniform microsphere dispersion; in addition, slowly add 3.625g of polyvinyl pyrrolidone (PVP) to 25.375g of deionized water, and magnetically stir for 4h to obtain a 12.5% ​​PVP solution. The obtained PVP solution is mixed with the microsphere dispersion and stirred at room temperature for 12h. No fluid gel soft substance is obtained, but a PVP solution containing glass microspheres is obtained.

[0036] Step 2: The material was spun into composite fibers. Spinning process parameters: spinning temperature 35°C, relative humidity 40%, drawing speed 0.5 m / s. The prepared material was put into an oven for curing, the curing temperature was 80°C, and the highest temperature was maintained for 12 hours, but no polyvinyl pyrrolidone / hollow microsphere composite fibers were obtained.

[0037] The third step: impregnating it in an aqueous polyurethane with a solid content of 60%. The polyvinyl pyrrolidone / hollow microsphere composite fiber disintegrates due to the direct dissolution of polyvinyl pyrrolidone, and no multi-level composite fiber is obtained. The above-mentioned embodiments only express several implementation methods of the present invention, and the description is relatively specific and detailed, but it cannot be understood as a limitation on the scope of the patent of the present invention. It should be pointed out that for ordinary technicians in this field, several deformations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the present invention shall be based on the attached claims.

Claims

1. A method for preparing multi-level composite fibers based on hollow microsphere soft gel, characterized in that: The steps include: The first step: mixing the hollow microspheres with deionized water to obtain a uniform dispersion, and then adding the dispersion into the PVA aqueous solution, mixing, and stirring to prepare a gel-like soft material with a fluid state; Step 2: spinning the gel soft substance, drying and solidifying it to prepare a morphologically stable polyvinyl alcohol / hollow microbead composite fiber; Step 3: immersing the polyvinyl alcohol / hollow microbead composite fiber in a polymer solution, taking it out and drying it, thereby obtaining a core-shell structure multi-level composite fiber with a core layer of polyvinyl alcohol / hollow microbead and a shell layer of polymer.

2. The method for preparing a multi-stage composite fiber according to claim 1, characterized in that: In the first step, the hollow microspheres refer to borosilicate hollow glass microspheres, the particle size of the spheres ranges from 10 to 250 μm, and the wall thickness is 0.1 to 0.2 times the particle size of the hollow microspheres. Microspheres of different particle sizes can be mixed and used.

3. The method for preparing a multi-stage composite fiber according to claim 1, characterized in that: In the first step, the flow state means that the soft gel can slowly deform under the action of gravity and external force, the automatic deformation rate under gravity is 0.001-0.5 m / s, it can deform immediately under external force, and the deformation caused by the external force can slowly disappear after the external force is removed.

4. The method for preparing a multi-stage composite fiber according to claim 1, characterized in that: In the first step, the mass ratio of the hollow microspheres to deionized water is 1:0.1-5; the PVA accounts for 1%-20% of the total mass of the gel-state soft substance; the hollow microsphere dispersion accounts for 1%-10% of the total mass of the gel-state soft substance; the PVA has an alcoholysis degree of 88% or 99% or a mixture of two or more thereof.

5. The method for preparing a multi-stage composite fiber according to claim 1, characterized in that: In the first step, the microstructure of the gel-like soft material is as follows: the PVA on the surface of the hollow microbeads encounters the boric acid diffused from the hollow microbeads themselves and produces local flocculation in the area around the surface of the hollow microbeads, while the PVA farther away from the hollow microbeads can still slide freely and play a lubricating role on the hollow microbead / flocculated PVA complex. This microstructure in which part of the PVA is locally flocculated and the other part can slide relatively makes the soft gel have both solid properties and fluidity.

6. The method for preparing a multi-stage composite fiber according to claim 1, characterized in that: In the second step, the spinning refers to stretching spinning under the conditions of 20-55° C. and 20%-70% relative humidity, and the stretching speed is 0.1-5 m / s.

7. The method for preparing a multi-stage composite fiber according to claim 1, characterized in that: In the second step, the curing temperature is 30-100° C. and the maximum temperature is maintained for 0-48 hours to remove the solvent and obtain a stable fiber morphology.

8. The method for preparing a multi-stage composite fiber according to claim 1, characterized in that: In the third step, the polymer concentration in the polymer solution is 5wt% to 60wt%, and the polymer is one or more of polyurethane, polyimide, polyamide, polyvinyl pyrrolidone, polyaryl sulfone, polyacrylonitrile, polysiloxane, polyvinyl formal, and melamine formaldehyde resin.

9. A multi-level composite fiber prepared by the method according to any one of claims 1 to 8, characterized in that: The core layer and the shell layer of the multi-stage composite fiber are tightly connected, but there is a clear interface between the shell layer and the core layer.

10. The multi-stage composite fiber according to claim 9, characterized in that: The shell layer of the core-shell structure multi-stage composite fiber is a continuous unbroken layer, which can effectively prevent the leakage of the hollow microbeads in the core layer; the PVA in the core layer can prevent the hollow microbeads from moving freely, and has a damping effect.

Citation Information

Patent Citations

  • Preparation method of hollow carbon microsphere loaded carbon fiber fabric composite material

    CN112281259A

  • Novel zero-convection high-heat-insulation SiBN fiber aerogel and preparation method thereof

    CN118005371A

  • Composite fiber and manufacturing method therefor, composite material and manufacturing method therefor

    JP2017057537A

  • IN118CHN2014A

Cited By

  • PVA / hollow glass microsphere composite phase change thermal insulation material and preparation method thereof

    CN121248993A