Sodium ion solid electrolyte, preparation method thereof and all-solid-state sodium ion battery
By covering the metal interface protective layer on the base surface of the sodium ion solid electrolyte, the problem of poor stability between the solid electrolyte and sodium metal is solved, the safety and stability of the battery are improved, and the cycle life of the battery is extended.
Patent Information
- Application Number
- CN202411246954.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-06
- Publication Date
- 2024-12-03
AI Technical Summary
The interface stability between the solid electrolyte and sodium metal in existing sodium ion solid-state batteries is poor, which can easily lead to battery short circuits and safety hazards. Traditional methods cannot fundamentally improve interface stability and are costly.
The substrate surface of the sodium ion solid electrolyte is covered with metal interface protective layers, such as Sn, Zn, In, Sb, Bi, Ge, and the metal thin layer is formed through magnetron sputtering technology to promote the alloying of sodium metals, enhance interface stability and Security.
It effectively reduces the growth of sodium dendrites and the risk of electrolyte interface damage, improves the cycle stability and safety performance of the battery, and extends the service life of the battery.
Smart Images

Figure CN119069774A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of sodium ion batteries, and in particular to a sodium ion solid electrolyte and a preparation method thereof, and an all-solid-state sodium ion battery. Background Art
[0002] Sodium metal has a high theoretical specific capacity (1166 mAh g -1 ) and lower electrochemical potential (-2.714V), making it an ideal negative electrode candidate for rechargeable sodium-ion batteries. However, traditional sodium metal batteries are composed of organic liquid electrolytes, which pose a potential risk of fire or even explosion. Solid-state sodium-ion batteries based on solid electrolytes are compatible with sodium metal negative electrodes and have high voltage, high capacity and high energy density, as well as excellent safety and mechanical properties. However, the poor stability and interface compatibility of sodium-ion solid electrolytes greatly hinder their practical application. On the one hand, some solid electrolytes may undergo irreversible chemical reactions with sodium metal, and the generated byproducts greatly affect the normal operation of the battery; on the other hand, the solid electrolyte itself may be penetrated by sodium dendrites, causing damage and short circuits; for example, PEO-NaTFSI, PEO-NaFSI, PVDF-NaTFSI, PVDF-NaFSI, etc.
[0003] In order to improve the stability and interfacial compatibility of the interface between the solid electrolyte and the sodium metal anode, the main methods currently include adding fillers to the solid electrolyte to form a composite electrolyte or modifying the surface of the solid electrolyte. Among them, the composite electrolyte is mainly used in polymer electrolytes, and the added fillers include inorganic materials such as SiO2 and Al2O3, or functional materials with ordered microporous structures such as MOF and COF. The surface modification of the solid electrolyte usually forms an in-situ or non-in-situ protective layer on the interface between the electrolyte and the sodium metal.
[0004] In solid-state sodium-ion batteries, the surface of the sodium negative electrode is usually prone to generate sharp dendrites during the cycle process, piercing the electrolyte layer, causing damage to the electrolyte interface, and in severe cases causing the battery to short-circuit and fail. Traditional methods, whether adding fillers to form a composite electrolyte or surface modification, mainly inhibit electrolyte interface damage by blocking dendrite growth. Such strategies do not fundamentally change the dendrite growth dynamics, but can only delay battery failure, and cannot fundamentally improve the stability of the sodium metal and electrolyte interface. In addition, some methods require expensive materials or precision equipment, which are costly and complex to operate; some reported interface modification methods may also change the intrinsic electrochemical properties of the electrolyte material, resulting in a reduction in battery energy density.
[0005] Therefore, it is necessary to provide a sodium ion solid electrolyte and a preparation method thereof and an all-solid-state sodium ion battery to improve the interface stability between the solid electrolyte and sodium metal in the solid-state sodium ion battery, thereby improving the safety and stability of the solid-state battery. Summary of the invention
[0006] The present invention aims to solve at least one of the technical problems existing in the above-mentioned prior art. To this end, the present invention proposes a sodium ion solid electrolyte and a preparation method thereof and an all-solid-state sodium ion battery, so as to improve the interface stability between the solid electrolyte and sodium metal in the solid-state sodium ion battery, thereby improving the safety and stability of the solid-state battery.
[0007] A first aspect of the present invention provides a sodium ion solid electrolyte.
[0008] Specifically, it includes a substrate and an interface protection layer;
[0009] The interface protection layer covers the surface of the substrate;
[0010] The substrate is a polymer electrolyte;
[0011] The interface protection layer is metal;
[0012] The metal includes at least one of Sn, Zn, In, Sb, Bi and Ge.
[0013] Preferably, the polymer electrolyte comprises a polymer and a sodium salt;
[0014] The polymer includes at least one of polyethylene oxide, polyvinylidene fluoride, polyvinyl alcohol, polyacrylonitrile, polyethyl acrylate, and polyethylene glycol;
[0015] The sodium salt includes at least one of sodium bis(trifluoromethanesulfonyl)imide, sodium bis(fluorosulfonyl)imide, sodium hexafluorophosphate, sodium fluoroborate and sodium nitrate.
[0016] More preferably, the polymer is polyethylene oxide.
[0017] More preferably, the sodium salt is sodium bis(trifluoromethanesulfonyl)imide.
[0018] Preferably, the metal includes at least one of Sn, Zn and In.
[0019] This application forms a thin metal layer on the surface of the substrate of the sodium ion solid electrolyte as an interface protection layer (including Sn, Zn, In, Sb, Bi, Ge), and alloys with the negative electrode sodium metal after contact. The alloyed metal layer can enhance the surface wettability of the sodium metal and the stability of its interface with the electrolyte, which is conducive to the uniform deposition of sodium, thereby reducing the interface impedance and inhibiting the formation of sodium dendrites. Metals with better alloying performance with metallic sodium show better performance in this process. This interface protection layer strategy can effectively reduce the damage to the solid electrolyte interface and reduce the risk of the electrolyte being penetrated by dendrites, thereby greatly improving the cycle stability and safety performance of the battery.
[0020] Preferably, the thickness of the interface protection layer is 50 to 2000 nm.
[0021] More preferably, the thickness of the interface protection layer is 50 to 1000 nm.
[0022] Preferably, the polymer electrolyte includes at least one of a polyethylene oxide-sodium bis(trifluoromethanesulfonyl)imide electrolyte sheet, a polyethylene oxide-sodium bis(trifluoromethanesulfonyl)imide electrolyte sheet, a polyethylene glycol-sodium bis(trifluoromethanesulfonyl)imide electrolyte sheet, and a polyethylene glycol-sodium hexafluorophosphate electrolyte sheet.
[0023] Preferably, the polyethylene oxide-sodium bis(trifluoromethanesulfonylimide) electrolyte sheet has a thickness of 50 to 500 μm.
[0024] More preferably, the polyethylene oxide-sodium bis(trifluoromethanesulfonylimide) electrolyte sheet has a thickness of 80 to 200 μm.
[0025] Preferably, the preparation method of the polyethylene oxide-sodium bis(trifluoromethanesulfonyl)imide electrolyte sheet comprises the following steps:
[0026] Polyethylene oxide and sodium bis(trifluoromethanesulfonyl)imide are dispersed in a solvent and stirred to obtain a mixed solution; the mixed solution is coated on a carrier and dried to obtain a polyethylene oxide-sodium bis(trifluoromethanesulfonyl)imide electrolyte sheet.
[0027] Preferably, the molar ratio of the EO unit in the polyethylene oxide to the sodium ion in the sodium bis(trifluoromethanesulfonyl)imide is 5 to 30:1.
[0028] Further preferably, the molar ratio of the EO unit in the polyethylene oxide to the sodium ion in the sodium bis(trifluoromethanesulfonyl)imide is 15 to 25: 1. This ratio can make the sodium ions well dissolved and transported in the electrolyte, thereby improving the ionic conductivity of the electrolyte.
[0029] Preferably, the solvent comprises acetonitrile.
[0030] Preferably, the coating method includes at least one of blade coating and casting.
[0031] Preferably, the carrier includes any one of a silicone oil paper sheet, a silicone sheet, and a polytetrafluoroethylene plate.
[0032] Preferably, the stirring temperature is 30 to 120° C. and the stirring time is 4 to 48 hours.
[0033] Further preferably, the stirring temperature is 60-90° C. and the stirring time is 24-36 hours. Under such stirring conditions, polyethylene oxide and sodium bis(trifluoromethanesulfonyl)imide can be fully mixed to form a uniform mixed solution, so that the polymer and the sodium salt are evenly distributed, thereby improving the uniformity and consistency of the electrolyte; it can also improve the ion conductivity of the electrolyte, reduce the internal resistance, thereby improving the battery performance, while taking into account the production efficiency.
[0034] Preferably, the drying temperature is 30 to 120° C. and the drying time is 8 to 48 hours.
[0035] More preferably, the drying temperature is 80-100° C. and the drying time is 24-36 hours. Such drying conditions can reduce the formation of bubbles and pores in the electrolyte, improve the density and stability of the electrolyte, and take into account production efficiency.
[0036] A second aspect of the present invention provides a method for preparing a sodium ion solid electrolyte.
[0037] Specifically, the following steps are included:
[0038] The metal is sputtered onto the surface of the substrate by magnetron sputtering technology to form an interface protection layer to prepare a sodium ion solid electrolyte.
[0039] Preferably, the sputtering power is 3-20 W, the time is 10-1200 s, and the pressure is 0.2-20 Pa.
[0040] Further preferably, the sputtering power is 5-15 W, the time is 50-600 s, and the pressure is 0.2-8 Pa.
[0041] Preferably, the sputtering gas includes argon.
[0042] This preparation method uses magnetron sputtering technology to evenly sputter metal atoms onto the surface of a solid polymer electrolyte. During the preparation process, the composition, power, time, and pressure of the sputtering gas are controlled to precisely control the properties and thickness of the sputtered metal thin layer, thereby achieving precise regulation of the solid electrolyte. Moreover, this preparation method is applicable to different types of polymer electrolytes and inorganic electrolytes, and has extremely strong universality. In actual production, the most suitable electrolyte material can be selected according to specific application requirements, and the corresponding solid electrolyte can be prepared. In short, this preparation method realizes the flexible preparation of different types of electrolytes, and has the advantages of high purity, high control accuracy, good film uniformity, and high preparation efficiency.
[0043] A third aspect of the present invention provides an all-solid-state sodium ion battery.
[0044] Specifically, the all-solid-state sodium ion battery includes the sodium ion solid electrolyte provided in the first aspect.
[0045] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0046] The present invention covers a suitable metal source such as Sn, Zn, In, Sb, Bi and Ge on the surface of the substrate as an interface protection layer, and forms a stable metal thin layer interface through alloying of sodium and the metal source, which can effectively prevent the growth of sodium dendrites, reduce the damage of the sodium ion solid electrolyte during the battery cycle, improve the interface wettability, and reduce the interface charge conduction impedance, thereby improving the interface stability between the sodium metal negative electrode and the solid electrolyte, and further obtaining a stable long-cycle all-solid-state sodium ion battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0047] Figure 1 The photos are of the PEO substrate without metal sputtering and the sodium ion solid electrolyte after sputtering different metals;
[0048] Figure 2 This is a SEM image of the surface morphology of PEO-Sn after deposition of metallic sodium provided in Example 1;
[0049] Figure 3 The surface morphology SEM image of PEO-NaTFSI after sodium deposition provided in Comparative Example 1;
[0050] Figure 4 XRD characterization test result diagram of the sodium ion solid electrolyte provided in Example 1, Example 2, Example 3, Example 4, and Comparative Example 1;
[0051] Figure 5 A FIB-SEM characterization test result diagram of the sodium ion solid electrolyte provided in Example 1;
[0052] Figure 6The AC impedance spectra of sodium-sodium symmetric batteries made of sodium ion solid electrolytes corresponding to Example 1, Example 5, Example 6, Comparative Example 1, Comparative Example 2, and Comparative Example 3;
[0053] Figure 7 The AC impedance spectra of the sodium-sodium symmetric batteries made of the sodium ion solid electrolyte corresponding to Example 1, Example 2, Example 3, Example 4, and Comparative Example 1;
[0054] Figure 8 This is a comparison chart of the cyclic charge and discharge performance results of the sodium-sodium symmetric battery made of the corresponding sodium ion solid electrolyte of Example 1 and Comparative Example 1;
[0055] Fig. 9 This is a comparison chart of the long cycle voltage distribution test results of the sodium-sodium symmetric battery made with the corresponding sodium ion solid electrolyte in Example 1 and Comparative Example 1. DETAILED DESCRIPTION
[0056] In order to make the technical scheme of the present invention more clearly understood by those skilled in the art, the following embodiments are listed for illustration. It should be pointed out that the following embodiments do not limit the protection scope of the present invention.
[0057] Unless otherwise specified, the raw materials, reagents or devices used in the following examples can be obtained from conventional commercial sources or by existing known methods.
[0058] Example 1
[0059] Sodium ion solid electrolyte and preparation method thereof.
[0060] The preparation method is as follows:
[0061] (1) Polyethylene oxide (PEO) and sodium bis(trifluoromethanesulfonyl)imide (NaTFSI)
[0062] (Macklin, >98%) was added to ultra-dry acetonitrile, the molar ratio of EO unit to sodium ion was set to 20:1, and the concentration of PEO in acetonitrile was 0.1 g / mL; it was stirred at 80°C for 24 hours until a uniform mixed solution was formed, and then the mixed solution was poured onto silicone oil paper, coated with a scraper, and heated and dried at 80°C for 24 hours; finally, it was cooled and cut into discs of appropriate size, and the thickness was measured to be 140 μm, thus obtaining a PEO-NaTFSI electrolyte sheet.
[0063] (2) The PEO-NaTFSI electrolyte sheet was subjected to magnetron sputtering. Using magnetron sputtering technology, in an argon environment, Sn metal source was used as a target to sputter Sn onto the surface of the PEO-NaTFSI electrolyte sheet to obtain a sodium ion solid electrolyte PEO-Sn; the sputtering power was 15 W; the sputtering time was 600 s; and the sputtering vacuum pressure was 5 Pa.
[0064] Example 2
[0065] Sodium ion solid electrolyte and preparation method thereof.
[0066] The difference from Example 1 is that the sputtering time is 50 s.
[0067] Example 3
[0068] Sodium ion solid electrolyte and preparation method thereof.
[0069] The difference from Example 1 is that the sputtering time is 150 s.
[0070] Example 4
[0071] Sodium ion solid electrolyte and preparation method thereof.
[0072] The difference from Example 1 is that the sputtering time is 300 s.
[0073] Example 5
[0074] Sodium ion solid electrolyte and preparation method thereof.
[0075] The difference from Example 3 is that the metal is Zn.
[0076] Example 6
[0077] Sodium ion solid electrolyte and preparation method thereof.
[0078] The difference from Example 3 is that the metal is In.
[0079] Comparative Example 1
[0080] Sodium ion solid electrolyte and preparation method thereof.
[0081] The difference from Example 1 is that no metal is sputtered.
[0082] Comparative Example 2
[0083] Sodium ion solid electrolyte and preparation method thereof.
[0084] The difference from Example 1 is that the metal is Au.
[0085] Comparative Example 3
[0086] Sodium ion solid electrolyte and preparation method thereof.
[0087] The difference from Example 1 is that the metal is Cu.
[0088] Performance testing:
[0089] 1. The sodium-sodium symmetric battery assembled with the sodium ion solid electrolyte provided in Example 1 and Comparative Example 1 was subjected to metal sodium deposition, and then the battery was disassembled to perform SEM characterization on each sodium ion solid electrolyte. The test results are as follows: Figure 2 , Figure 3 As shown, Figure 2 The surface morphology of the PEO-Sn after the deposition of metallic sodium provided in Example 1, Figure 3 This is the surface morphology of PEO-NaTFSI after sodium deposition provided in Comparative Example 1.
[0090] from Figure 2 It can be seen that spherical and moss-like metallic sodium deposits appear on the surface of the modified PEO-Sn in Example 1; Figure 3 It can be seen that dendritic metallic sodium dendrites appear on the surface of PEO-NaTFSI without surface metal modification in Comparative Example 1; these morphological features indicate that under the modification of the Sn layer, Na nucleates and grows in a spherical or moss-like form, thereby preventing the formation of Na dendrites.
[0091] 2. XRD characterization test was performed on the sodium ion solid electrolytes provided in Example 1, Example 2, Example 3, Example 4 and Comparative Example 1, and FIB-SEM characterization test was performed on Example 1. The test results are as follows: Figure 4 and Figure 5 shown.
[0092] from Figure 4 It can be seen that as the sputtering time increases, the diffraction peak signal corresponding to Sn increases, indicating that the Sn metal content on the surface of PEO-NaTFSI continues to increase. Figure 5 It can be seen that after focused ion beam cutting, the thickness of the Sn layer can be observed to be in the range of 0 to 800 nm, of which the thickness after 600s of magnetron sputtering is about 600 to 800nm. At the same time, after testing, it was found that the thickness after 300s of magnetron sputtering is about 300 to 400nm, the thickness after 150s of magnetron sputtering is about 150 to 200nm, and the thickness after 50s of magnetron sputtering is about 50 to 100nm. It can be seen that by adjusting the sputtering time, the thickness of the interface protection layer on the surface of the solid electrolyte substrate can be accurately controlled.
[0093] 3. The sodium ion solid electrolytes provided in Example 1, Example 5, Example 6, Comparative Example 1, Comparative Example 2, and Comparative Example 3 were used to prepare corresponding sodium-sodium symmetric batteries. A bias voltage of 10 mV was applied in the frequency range of 1 Hz to 7 MHz, and an electrochemical impedance test was performed to obtain the following results: Figure 6 Impedance data graph shown.
[0094] Figure 6 In the embodiment 1 (PEO-Sn), the embodiment 5 (PEO-Zn), the embodiment 6 (PEO-In), the comparative example 2 (PEO-Au), and the comparative example 3 (PEO-Cu) are Na symmetric batteries assembled with sodium ion solid electrolytes obtained by sputtering PEO-NaTFSI under different metal sources for the same time of 150s; the comparative example 1 (PEO) is a Na symmetric battery directly assembled with PEO-NaTFSI solid electrolyte without metal sputtering, corresponding to the comparative example 1. Figure 6 It can be seen that among these metal layers, metal Sn, Zn, and In all have a certain optimization effect on the sodium metal interface resistance, among which the Sn layer has the best resistance optimization effect on the Na symmetric battery, while Au and Cu as comparative examples not only fail to reduce the interface impedance, but also affect the original performance of the battery. Among them, the impedance of sputtered Cu is much greater than that of unsputtered PEO, and the sputtered Au PEO is directly penetrated by sputtering and causes a short circuit. In particular, the difference in resistance of these Na symmetric batteries is equivalent to the difference in interface resistance between the solid electrolyte and the sodium metal negative electrode, because the resistance of the bulk PEO is constant.
[0095] 4. The sodium ion solid electrolytes provided in Example 1, Example 2, Example 3, Example 4, and Comparative Example 1 were used to prepare corresponding sodium-sodium symmetric batteries, and electrochemical impedance tests were performed. For the sodium-sodium symmetric battery prepared from the above sodium ion solid electrolytes, a bias voltage of 10 mV was applied in the frequency range of 1 Hz to 7 MHz, and an EIS test was performed to obtain the following results: Figure 7 The AC impedance spectra of the sodium-sodium symmetric batteries made of solid electrolytes corresponding to Example 1, Example 2, Example 3, Example 4 and Comparative Example 1 are shown.
[0096] Figure 7 In the embodiment 2 (PEO-50s), the embodiment 3 (PEO-150s), the embodiment 4 (PEO-300s), and the embodiment 1 (PEO-600s) are Na symmetric batteries assembled with solid electrolytes obtained by sputtering different times of sodium ion solid electrolytes with PEO-NaTFSI as the base under Sn as the metal source; PEO is a Na symmetric battery directly assembled with PEO-NaTFSI solid electrolyte without metal sputtering, corresponding to the corresponding embodiment 1. Figure 7It can be seen that with the increase of sputtering time, the impedance of the Na symmetric battery is gradually decreasing, which indicates that the degree of alloying between Na metal and electrolyte is constantly improving, the interface impedance is gradually decreasing, and the interface compatibility is gradually improving. Among them, the sodium ion solid electrolyte corresponding to Example 1 obtained by sputtering for 600s has the best interface impedance performance. It can be understood that the metal sputtering time plays a key role in the performance of the obtained sodium ion solid electrolyte, and appropriately extending the sputtering time can effectively improve the interface contact performance of the solid electrolyte.
[0097] 5. The sodium ion solid electrolytes provided in Example 1 and Comparative Example 1 were prepared into corresponding sodium-sodium symmetric batteries and sodium ion batteries, and the above batteries were subjected to the following electrochemical performance tests:
[0098] (1) Cyclic charge and discharge test: For the sodium ion battery prepared by the above sodium ion solid electrolyte, the first two cycles were charged and discharged at 0.2C, and the subsequent cycles were charged and discharged at 0.5C. Figure 8 The cycle charge and discharge performance diagram shown.
[0099] Figure 8 In the embodiment, PEO is a sodium ion battery composed of a PEO-NaTFSI electrolyte without sputtering metal corresponding to Comparative Example 1, and PEO-Sn is a sodium ion battery assembled with a solid electrolyte PEO-Sn provided in Example 1. Figure 8 It can be seen that PEO without sputtering metal layer shows extremely poor coulombic efficiency stability. The coulombic efficiency will change abruptly in the initial cycle process, and the capacity begins to decay rapidly after 180 cycles; PEO-Sn shows extremely stable cycle performance, with a coulombic efficiency of nearly 99% in each cycle, and can be stably cycled for more than 400 cycles without obvious capacity decay.
[0100] (2) Long cycle voltage distribution test: for the Na symmetric battery prepared with the above sodium ion solid electrolyte, a single cycle at 0.1 mA / cm 2 The charge and discharge are performed for 30 minutes each, and the voltage distribution in the long cycle test is recorded. The test results are as follows: Fig. 9 shown.
[0101] Fig. 9 In the test, the Na symmetric battery long cycle test assembled with Example 1 and Comparative Example 1 as electrolyte was carried out at 60°C, in order to ensure that the Na deposition morphology on the surface of the multi-electrolyte can be observed while the battery is charged and discharged within the normal voltage range. Fig. 9It can be seen that the sodium symmetric battery prepared by the PEO-NaTFSI electrolyte without sputtering metal corresponding to Comparative Example 1 has extremely unstable voltage during the cycle, and micro short circuits and large voltage fluctuations occur many times. Finally, it is penetrated by dendrites after 116 hours of cycle, and the voltage drops sharply to 0V, and the battery short circuits; while the Na symmetric battery assembled by the corresponding electrolyte of Example 1 with sputtering Sn can still maintain stable cycle after continuous cycle charging for 1200 hours, and the charge and discharge voltage remains basically stable.
[0102] The preferred specific embodiments of the present invention are described in detail above. It should be understood that a person skilled in the art can make many modifications and changes based on the concept of the present invention without creative work. Therefore, any technical solution obtained by any modification, equivalent replacement, improvement, etc. made by a person skilled in the art based on the concept of the present invention through logical analysis, reasoning or limited experiments on the basis of the prior art shall be within the scope of protection determined by the claims.
Claims
1. A sodium ion solid electrolyte, characterized in that: including a substrate and an interface protection layer; The interface protection layer covers the surface of the substrate; The substrate is a polymer electrolyte; The interface protection layer is metal; The metal includes at least one of Sn, Zn, In, Sb, Bi and Ge.
2. The sodium ion solid electrolyte according to claim 1, characterized in that The polymer electrolyte comprises a polymer and a sodium salt; The polymer includes at least one of polyethylene oxide, polyvinylidene fluoride, polyvinyl alcohol, polyacrylonitrile, polyethyl acrylate, and polyethylene glycol; The sodium salt includes at least one of sodium bis(trifluoromethanesulfonyl)imide, sodium bis(fluorosulfonyl)imide, sodium hexafluorophosphate, sodium fluoroborate and sodium nitrate.
3. The sodium ion solid electrolyte according to claim 1, characterized in that The thickness of the interface protection layer is 50-2000 nm.
4. The sodium ion solid electrolyte according to claim 1, characterized in that The polymer electrolyte includes at least one of a polyethylene oxide-sodium bis(trifluoromethanesulfonyl)imide electrolyte sheet, a polyethylene oxide-sodium bis(fluorosulfonyl)imide electrolyte sheet, a polyethylene glycol-sodium bis(trifluoromethanesulfonyl)imide electrolyte sheet, and a polyethylene glycol-sodium hexafluorophosphate electrolyte sheet.
5. The sodium ion solid electrolyte according to claim 4, characterized in that The thickness of the polyethylene oxide-sodium bis(trifluoromethanesulfonyl)imide electrolyte sheet is 50-500 μm.
6. The sodium ion solid electrolyte according to claim 4, characterized in that The preparation method of the polyethylene oxide-sodium bis(trifluoromethanesulfonyl)imide electrolyte sheet comprises the following steps: Polyethylene oxide and sodium bis(trifluoromethanesulfonyl)imide are dispersed in a solvent and stirred to obtain a mixed solution; the mixed solution is coated on a carrier and dried to obtain a polyethylene oxide-sodium bis(trifluoromethanesulfonyl)imide electrolyte sheet.
7. The sodium ion solid electrolyte according to claim 4, characterized in that The molar ratio of the EO unit in the polyethylene oxide to the sodium ion in the sodium bis(trifluoromethanesulfonyl)imide is 5 to 30:
1.
8. The method for preparing a sodium ion solid electrolyte according to any one of claims 1 to 7, characterized in that: The following steps are involved: The metal is sputtered onto the surface of the substrate by magnetron sputtering technology to form an interface protection layer to prepare a sodium ion solid electrolyte.
9. The preparation method according to claim 8, characterized in that: The sputtering power is 3-20W, the time is 10-1200s, and the pressure is 0.2-20Pa.
10. An all-solid-state sodium ion battery, characterized in that: The all-solid-state sodium ion battery comprises the sodium ion solid electrolyte according to any one of claims 1 to 7.
Citation Information
Patent Citations
Liquid metal interface buffered solid-state battery and preparation method thereof
CN116682927A
Ultra-thin type AGV differential driving device
KR102160513B1
Solid electrolyte for all-solid sodium battery, and all-solid sodium battery
US20200335815A1
Solid-state electrolyte, secondary battery, battery module, battery pack, and electrical device
WO2024152735A1
Cited By
Polymer solid electrolyte and solid sodium battery based on polymer solid electrolyte
CN119601766A
Alloy interface layer for solid sodium-ion battery and preparation method and application of alloy interface layer
CN119786751A
Alloy negative electrode composite sodium solid electrolyte material and preparation method and application thereof
CN121662930A
Sodium-ion solid electrolyte, sodium-ion solid battery and preparation method of sodium-ion solid electrolyte and sodium-ion solid battery
CN121709705A
A sodium ion solid-state electrolyte, a sodium ion solid-state battery and a preparation method thereof
CN121709705B