Preparation method of high-purity smelting niobium block for high-temperature alloy additive
Through the optimization of the aluminum thermal reduction method and multiple smelting process, the problems of complex traditional processes and high impurities are solved, and the efficient preparation of high-purity niobium blocks is achieved, and the performance of high-temperature alloys is improved.
Patent Information
- Application Number
- CN202411209038.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-12-06
AI Technical Summary
The traditional high-purity smelting niobium block preparation process is complex and the impurity content is high, resulting in a degradation of the performance of high-temperature alloys.
The aluminum thermal reduction method is used instead of carbonization reduction method, and it is optimized through multiple smelting processes, including turning the plate during the first smelting, padding into a melted niobium pad during the second smelting, and switching the shear edges during the third smelting, extending impurities Volatility time and increase volatility space to reduce the C and N impurities content in niobium blocks.
Simplify the process flow, shorten the production cycle, significantly reduce the impurity content, improve the purity and quality of high-purity niobium blocks, and improve the performance of niobium-containing high-temperature alloys.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of high-purity metal single substance preparation, and in particular to a method for preparing a high-purity smelted niobium block for a high-temperature alloy additive. Background Art
[0002] Niobium-containing high-temperature alloys are increasingly used in modern economic life because of their ability to significantly improve heat energy conversion efficiency, good strength and corrosion resistance. Among them, the most important application areas of niobium-containing high-temperature alloys are blades in aircraft engines, turbochargers and exhaust valves in automobile engines, and the processing of bolts, blades, chimney gas reheaters and chemical reaction vessels, pipes, valves, bolts and pumps in high-performance turbine generators. The high-purity niobium additive raw material used in niobium-containing high-temperature alloys is usually high-purity smelted niobium blocks. In traditional processes, the preparation process of high-purity smelted niobium blocks is as follows: Figure 1 As shown, first, NbC is produced by two carburization reduction reactions, then NbC and niobium pentoxide are mixed in a certain proportion, and niobium powder is obtained after high-temperature vacuum reduction reaction, hydrogenation and dehydrogenation. Then, the niobium powder is formed and sintered, and then smelted twice in a vertical electron beam furnace to obtain a high-purity niobium ingot. Then, the high-purity niobium ingot is rolled into a plate, and finally the plate is sheared into blocks to obtain a high-purity niobium block. As can be seen from the above, the defects of the traditional process are: First, from the initial preparation of materials to the final niobium block, since NbC needs to be obtained by carburization reduction reaction in the early stage, NbC and niobium pentoxide are subjected to high-temperature vacuum reduction reaction, hydrogenation and dehydrogenation to obtain niobium powder in the middle stage, and high-purity niobium ingots are obtained after two vertical electron beam melting, and niobium plates are obtained again after rolling and shearing. The process flow is complicated and the production cycle is long; second, due to the use of carburization reduction method in the early stage, more C and N impurities are left in the intermediate product niobium powder, and the subsequent process cannot completely remove C and N. Therefore, the content of C and N impurities in the final high-purity niobium block is relatively high. Since C and N are interstitial elements, they will precipitate on the alloy grain boundaries when added to the alloy, reducing the grain boundary strength, making the alloy exhibit hot brittleness, and reducing the high-temperature strength, thereby reducing the alloy performance. Summary of the invention
[0003] In view of this, it is necessary to provide a method for preparing a high-purity smelting niobium block for a high-temperature alloy additive, so as to simplify the process flow, improve production efficiency, reduce the content of C and N impurities in the high-purity smelting niobium block, improve the purity and quality of the high-purity smelting niobium block, and improve the performance of the niobium-containing high-temperature alloy using the same.
[0004] A method for preparing a high-purity smelted niobium block for a high-temperature alloy additive comprises the following steps: S1. Prepare materials: Prepare the following raw materials by weight: 100 parts of niobium pentoxide, 35-45 parts of aluminum powder, 1-5 parts of calcium oxide and 2-7 parts of calcium fluoride; S2. Mixing: Put the above raw materials into a mixer and mix them evenly; S3, aluminothermic reduction reaction: The mixed materials are subjected to aluminothermic reduction reaction to obtain niobium aluminum alloy; S4, Crushing: The niobium aluminum alloy obtained in S3 is crushed into small pieces of 20-60 mm to obtain a block of niobium aluminum alloy; S5, first smelting: The blocky niobium aluminum alloy is spread flat in a horizontal electron beam furnace crucible for the first smelting to obtain a first-melting niobium plate; S6, Second Melting: After the primary smelting niobium plate is turned upside down, it is placed in the horizontal electron beam furnace crucible again, and a number of smelting niobium pads are placed under the primary smelting niobium plate to perform a second smelting to obtain a secondary smelting niobium plate; S7, the third smelting: The secondary smelting niobium plate is cross-cut into four equal parts and laid flat in a horizontal electron beam furnace crucible, and the cut edges are transferred to the periphery, and a number of high-purity smelting niobium pads are placed underneath, and then smelting is performed to obtain the tertiary smelting niobium plate; S8, cut into blocks: The tertiary smelting niobium plates are cut into blocks to obtain high-purity smelted niobium blocks.
[0005] Preferably, during the first smelting in step S5 and the second smelting in step S6, the vacuum degree of the furnace chamber is less than or equal to 0.05 Pa, and the smelting power is 350-450 kW.
[0006] Preferably, during the third smelting in step S7, the vacuum degree of the furnace chamber is less than or equal to 0.03 Pa, and the smelting power is 400-450 kW.
[0007] Preferably, in step S1, the purity of the niobium pentoxide is greater than or equal to 99.50%, the purity of the metal aluminum powder is greater than or equal to 99%, the purity of the calcium oxide is greater than or equal to 90%, and the purity of the calcium fluoride is greater than or equal to 99%.
[0008] Preferably, in step S1, the raw materials are, by mass, 100 parts of niobium pentoxide, 38-42 parts of metallic aluminum powder, 2-3 parts of calcium oxide, and 3-5 parts of calcium fluoride.
[0009] Preferably, in step S1, the raw materials are, by mass fraction, 100 parts of niobium pentoxide, 40 parts of metallic aluminum powder, 2 parts of calcium oxide, and 4 parts of calcium fluoride.
[0010] Preferably, the aluminothermic reduction reaction in step S3 specifically comprises the following steps: S30, pouring the mixed materials into the crucible three times and compacting them respectively; S31, evacuate the reaction chamber to below 20Pa, and then introduce argon gas into the reaction chamber until the pressure in the reaction chamber rises to 0.07-0.065Mpa; S32, igniting to cause the material to undergo aluminothermic reduction reaction, and obtaining a reaction product after the reaction is completed; S33, the reaction product is slowly cooled in the furnace, and then taken out of the furnace and naturally cooled to room temperature; S34, separating the reaction product into slag and gold to obtain niobium aluminum alloy.
[0011] Preferably, the purity of the smelted niobium pad in step S6 is higher than the purity of the first smelted niobium plate; The purity of the high-purity smelted niobium pad in step S7 is higher than the purity of the secondary smelted niobium plate.
[0012] Preferably, in step S2, the mixing time is 3 hours.
[0013] Preferably, in step S32, during the ignition, the ignition wire used includes a conductor made of bare aluminum wire and a spiral wire made of φ0.6-0.8mm nickel-chromium wire.
[0014] The above-mentioned method for preparing high-purity niobium blocks for high-temperature alloy additives is Figure 1Compared with the conventional process in the prior art shown in the figure, on the one hand, the process flow is greatly simplified, the production cycle is greatly shortened, and the production efficiency is improved; on the other hand, the present invention reduces the content of C and N impurities in the final product and improves the uniformity of impurity distribution through the following points: first, the carbonization reduction method is abandoned and the aluminum thermal reduction method is adopted to reduce the content of C and N impurities in the intermediate product; second, in the second smelting process, the niobium plate for primary smelting is flipped up and down before smelting. By flipping the plate, the part close to the water-cooled surface at the bottom of the crucible in the first smelting is quickly solidified, and the part where the impurities are not fully volatilized is flipped to the top, so that the melted surface does not directly contact the crucible, so that the molten niobium liquid maintains a certain degree of superheat, so that the impurities are fully utilized, thereby reducing the content of impurities in the product and improving the impurity distribution. The uniformity of the distribution of impurities is improved, thereby improving the quality and performance of the final product; in the third and fourth smelting processes, the secondary smelting niobium plate is sheared, and the sheared edges are exchanged inside and outside, so that the parts of the secondary smelting niobium plate that were originally rapidly solidified due to the water-cooled surfaces set around the crucible and the impurities were not fully volatilized are exchanged to the center of the crucible for smelting, so that the impurities are volatilized more thoroughly, the uniformity of the impurity distribution is improved, and the quality and performance of the final product are improved; fourthly, in the second smelting process, a smelting niobium block is padded at the bottom, and in the third smelting process, a high-purity smelting niobium block is padded at the bottom, so as to increase the distance between the material to be smelted and the bottom of the crucible, and make the bottom of the material no longer directly contact the water-cooled surface of the crucible, thereby extending the time for the molten niobium material to drip into the crucible, ensuring the full volatilization of impurities, and improving the quality and performance of the final product. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 This is a process flow chart for preparing high-purity niobium blocks using the carbide reduction method in the traditional process.
[0016] Figure 2 The present invention is a flow chart of the method for preparing the high purity niobium block used as a high temperature alloy additive.
[0017] Figure 3 It is a schematic diagram of inserting a high-purity smelted niobium block underneath the secondary smelted niobium plate after cross-average shearing in a specific embodiment of the present invention. DETAILED DESCRIPTION
[0018] The technical solutions and technical effects of the embodiments of the present invention are further described in detail below in conjunction with the accompanying drawings of the present invention.
[0019] Please see Figure 1 As shown, a specific embodiment of the present invention provides a method for preparing a high-purity niobium block for a high-temperature alloy additive, comprising the following steps: S1. Prepare materials: Prepare the following raw materials by weight: 100 parts of niobium pentoxide, 35-45 parts of aluminum powder, 1-5 parts of calcium oxide and 2-7 parts of calcium fluoride; S2. Mixing: Put the above raw materials into a mixer and mix them evenly; for example, the mixer can be a V-type mixer with a rotation speed of 100 rpm; S3, aluminothermic reduction reaction: The mixed materials are subjected to aluminothermic reduction reaction to obtain niobium aluminum alloy; In the early stage of the rough refining process, the present invention adopts the aluminothermic reduction method to obtain the intermediate product niobium aluminum alloy, so as to prepare for the later refining; compared with the technology of adopting the carbide reduction method in the early stage in the prior art, the risk of carbon entering the final product as an impurity is eliminated, the purity and quality of the high-purity smelted niobium are improved, and the performance of the niobium-containing high-temperature alloy using the same is indirectly improved; S4, Crushing: The niobium aluminum alloy obtained in S3 is crushed into small pieces of 20-60 mm to obtain a block of niobium aluminum alloy; For example, a jaw crusher can be used to crush the niobium aluminum alloy; crushing the niobium aluminum alloy into small pieces of 20-60 mm can facilitate the rapid and sufficient melting of the niobium aluminum alloy in the subsequent smelting process, and can also prevent the niobium aluminum alloy from being crushed into powder, which will splash when being scanned by the electron beam during the smelting process, resulting in waste and reduced yield; S5, first smelting: The blocky niobium aluminum alloy is spread flat in a horizontal electron beam furnace crucible for the first smelting to obtain a first-melting niobium plate; the present invention adopts a horizontal electron beam furnace for smelting. Compared with the technology of using a vertical electron beam furnace to melt niobium ingots in the traditional process, the horizontal electron beam furnace can directly melt into niobium plates without the need for subsequent rolling processes, thereby simplifying the process flow and improving production efficiency; the first-melting niobium plate is low-purity smelting niobium; S6, Second Melting: The first-melted niobium plate is flipped upside down and placed in the horizontal electron beam furnace crucible again, and three niobium smelting pads are placed under the first-melted niobium plate for a second smelting to obtain a second-melted niobium plate; Three niobium smelting pads are placed at both ends and the center of the length direction of the first smelting niobium plate to stably support the first smelting niobium plate and to allow as much suspended space as possible under the first smelting plate, so that the molten niobium liquid can drip more smoothly during smelting and impurities can be volatilized more fully; In the horizontal electron beam melting equipment, the crucible is made of copper. During the melting process, the temperature in the furnace can reach 2800-2900 degrees Celsius. The high temperature melts the niobium aluminum alloy into a liquid state, and the aluminum with a higher saturated vapor pressure evaporates into the furnace after the niobium aluminum alloy melts. However, in order to allow the molten material to cool and solidify quickly, the bottom and edges of the crucible where the material is placed are all set with a water cooling device. Therefore, the temperature at the position where the niobium aluminum alloy contacts the crucible can only be lower than the melting point of the crucible copper material, 1083 degrees Celsius. Therefore, during the first smelting, the block niobium aluminum alloy is directly placed in the crucible in the horizontal electron beam furnace. During the smelting process, the molten material drips directly onto the water-cooled surface of the crucible, and the temperature drops sharply and solidifies quickly, causing the impurities in the molten niobium to be unable to be completely volatilized due to too short a volatilization time, and impurity defects will be formed in the final formed single-melting niobium plate; especially for the part of the single-melting niobium plate close to the bottom of the crucible, since the temperature can only reach 1083 degrees Celsius, the material cannot be fully melted; and the material slightly above the bottom will also cool and solidify faster, and the impurity content will be higher than those parts relatively far from the bottom of the crucible, resulting in uneven distribution of the remaining impurities in the single-melting niobium plate; Therefore, during the second smelting, three smelting niobium pads are placed under the first smelting niobium plate, and the first smelting niobium plate is turned up and down. On the one hand, during the smelting process, since there is a smelting niobium block between the material and the crucible, the distance between the material and the bottom of the crucible becomes larger. After the material is melted, the time for dripping into the crucible becomes longer, and the impurities have more sufficient volatilization time, thereby reducing the content of impurities in the product and improving the quality and performance of the product; on the other hand, the material at the bottom can be more fully melted because it is no longer in direct contact with the water-cooled surface of the crucible, and after melting, the impurities can also be volatilized more thoroughly; on the other hand, the first smelting niobium plate is turned over, so that the part with more impurities left at the bottom of the first smelting niobium plate obtained after the first smelting is turned up, and during the second smelting process, the impurities in these parts can be more fully volatilized because the distance from the bottom of the crucible becomes larger, which helps to improve the uniformity of impurity distribution in the final product; S7, the third smelting: The secondary smelting niobium plate is cross-cut into four equal parts and laid flat in a horizontal electron beam furnace crucible. The cut edges are transferred to the periphery and six high-purity smelting niobium pads are placed underneath. After that, smelting is performed to obtain the tertiary smelting niobium plate. The placement positions of the six high-purity smelting niobium pads are as follows: Figure 3As shown, firstly, they are placed along the length direction of the rectangle formed after the shearing secondary melting niobium plate is replaced and reset, and then along the length midline of each sheared niobium plate. The four blocks at both ends are placed under each niobium plate, and the two blocks in the center are placed on the seams between two adjacent blocks. The six high-purity niobium pads are used to stably support the reset niobium plate after shearing and replacement, and at the same time, there is as much suspended space as possible under the niobium plate, so that the molten niobium liquid can drip more smoothly during smelting, and the impurities can be volatilized more fully. During the third smelting process, the secondary smelting niobium plate is cross-cut into four equal parts, and the cut edges are transferred to the periphery. The benefit of this arrangement is that since the crucible is also surrounded by water-cooled surfaces, the impurity content at the four sides is relatively high during the smelting process. By cutting the secondary smelting niobium plate into four equal parts and transferring the cut edges to the periphery, the four sides with a high impurity level distribution are placed in the center for smelting, and the high-purity smelting niobium pads are placed below to make the impurities evaporate more thoroughly, and the final tertiary smelting niobium plate has less impurities and a more even distribution of the remaining impurities. S8, cut into blocks: The tertiary smelting niobium plates are cut into blocks to obtain high-purity smelted niobium blocks.
[0020] Furthermore, during the first smelting in step S5 and the second smelting in step S6, the vacuum degree of the furnace chamber is less than or equal to 0.05 Pa, and the smelting power is 350-450 kW.
[0021] Furthermore, during the third smelting in step S7, the vacuum degree of the furnace chamber is less than or equal to 0.03 Pa, and the smelting power is 400-450 kW.
[0022] Since the volatilization rate of impurities is proportional to their saturated vapor pressure, the volatilization amount of impurities increases with the increase of furnace chamber melting temperature and increases with the decrease of furnace chamber pressure. Therefore, during the third melting, the melting power is increased, and the melting temperature is increased to increase the volatilization rate of impurities, thereby improving the quality of the product; and the volatilization rate of impurities is further increased by increasing the furnace chamber vacuum and reducing the furnace chamber pressure, thereby improving the quality of the product. Furthermore, in step S1, the purity of the niobium pentoxide is greater than or equal to 99.50%, the purity of the metal aluminum powder is greater than or equal to 99%, the purity of the calcium oxide is greater than or equal to 90%, and the purity of the calcium fluoride is greater than or equal to 99%.
[0023] Furthermore, in step S1, the raw materials are, by mass, 100 parts of niobium pentoxide, 38-42 parts of metallic aluminum powder, 2-3 parts of calcium oxide, and 3-5 parts of calcium fluoride.
[0024] Furthermore, in step S1, the raw materials are, by mass fraction, 100 parts of niobium pentoxide, 40 parts of metallic aluminum powder, 2 parts of calcium oxide, and 4 parts of calcium fluoride.
[0025] Furthermore, the aluminothermic reduction reaction in step S3 specifically comprises the following steps: S30, pouring the mixed materials into the crucible three times and compacting them respectively; S31, evacuate the reaction chamber to below 20Pa, and then introduce argon gas into the reaction chamber until the pressure in the reaction chamber rises to 0.07-0.065Mpa; S32, igniting to cause the material to undergo aluminothermic reduction reaction, and obtaining a reaction product after the reaction is completed; S33, the reaction product is slowly cooled in the furnace, and then taken out of the furnace and naturally cooled to room temperature; S34, separating the reaction product into slag and gold to obtain niobium aluminum alloy.
[0026] Furthermore, the purity of the smelted niobium pad in step S6 is higher than the purity of the first smelted niobium plate; for example, it can be obtained by shearing the second smelted niobium plate obtained after the second smelting; The purity of the high-purity smelted niobium pad in step S7 is higher than that of the secondary smelted niobium plate; for example, it can be obtained by shearing the tertiary smelted niobium plate obtained after the third smelting.
[0027] Furthermore, in step S2, the mixing time is 3 hours.
[0028] Furthermore, in step S32, during the ignition, the ignition wire used includes a conductor made of bare aluminum wire and a spiral wire made of φ0.6-0.8mm nickel-chromium wire.
[0029] The beneficial effects of the present invention will be further described in detail below in conjunction with specific embodiments.
[0030] Examples 1-24 The high-purity niobium blocks for high-temperature alloy additives provided in Examples 1-12 are prepared by the preparation method provided in the specific embodiment of the present invention, wherein, in the second smelting, the first-melting niobium plate is turned upside down, and in the third smelting, the second-melting niobium plate is sheared and the shearing edge is adjusted to the periphery, and other process parameters are detailed in Table 1; the high-purity niobium blocks for high-temperature alloy additives provided in Examples 13-18 are prepared by the preparation method provided in the specific embodiment of the present invention, wherein, in the second smelting, the first-melting niobium plate is not turned upside down, and other process parameters are the same as those of Examples 1-6, and are detailed in Table 2; the high-purity niobium blocks for high-temperature alloy additives provided in Examples 19-24 are prepared by the preparation method provided in the specific embodiment of the present invention, wherein, in the third smelting, the second-melting niobium plate is sheared and the shearing edge is not adjusted to the periphery, and other process parameters are the same as those of Examples 7-12, and are detailed in Table 2; Comparative Examples 1-3 The smelting niobium is prepared by the carbide reduction method according to the traditional process; Table 1
[0031] Table 2
[0032] For the high purity niobium blocks for high temperature alloy additives prepared in Examples 1-24 of the present invention, the impurities C and N at the edge of the upper surface, the center of the upper surface and the center of the lower surface were measured, and the results are shown in Tables 3-4; for the smelted niobium prepared in Comparative Examples 1-3, the impurities C and N at the center of the upper surface were measured, and the results are shown in Table 5; Table 3
[0033] Table 4
[0034] Table 5
[0035] It can be seen from the data in Table 3 and Table 5 that the high-purity niobium block prepared by the preparation method provided in the specific embodiment of the present invention has a greatly reduced content of impurities C and N compared with the smelted niobium prepared by the carbide reduction method according to the traditional process; From the data of Examples 1-6 in Table 3 and Examples 13-18 in Table 4, it can be seen that the high-purity niobium block obtained by the preparation method provided by the specific embodiment of the present invention has less content of impurities C and N, and volatilizes more fully during the production process, and the content of C and N at the center of the lower surface is not much different from their contents at the edge and center of the upper surface, and the uniformity of impurity distribution is improved. Accordingly, the quality of the high-purity niobium block is better. On the contrary, in the niobium block obtained by not turning the niobium plate of the first smelting up and down in the second smelting, the content of C and N at the center of the lower surface is significantly different from their contents at the edge and center of the upper surface. Therefore, turning the niobium plate of the first smelting up and down in the second smelting is helpful to make the impurities C and N volatilize more fully, reduce the content of impurities C and N in the final product, and improve the uniformity of impurity distribution, thereby improving the quality of the final product. It can be seen from the data of Examples 7-12 in Table 3 and Examples 14-24 in Table 4 that the high-purity niobium block obtained by the preparation method provided by the specific embodiment of the present invention has less content of impurities C and N, and volatilizes more fully during the preparation process, compared with the niobium block obtained by shearing the secondary smelting niobium plate in the third smelting without adjusting the shearing edge to the periphery, and the high-purity niobium block obtained by the preparation method provided by the specific embodiment of the present invention has less content of impurities C and N, and volatilizes more fully during the preparation process, and the content of C and N at the edge of the upper surface is not much different from that at the center of the upper surface and the center of the lower surface, and the impurity distribution is uniform. The uniformity is improved, and accordingly, the quality of the high-purity niobium block is better; on the contrary, in the third smelting, after the secondary smelting niobium plate is sheared, the shearing edge is not adjusted to the periphery to prepare the niobium block, the content of C and N at the edge of the upper surface is significantly different from their content at the center of the upper surface and the center of the lower surface; therefore, in the third smelting, after the secondary smelting niobium plate is sheared, the shearing edge is adjusted to the periphery, which is helpful to make the impurities C and N volatilize more fully, reduce the content of impurities C and N in the final product, and improve the uniformity of impurity distribution, thereby improving the quality of the final product; In Table 3, according to the comparison of the data of Examples 1 and 7, the data of Examples 2 and 8, the data of Examples 3 and 9, the data of Examples 4 and 10, the data of Examples 5 and 11, and the data of Examples 6 and 12, it can be seen that with the increase of the smelting power in the first smelting, the second smelting and the third smelting, the smelting temperature increases, and since the volatilization amount of impurities increases with the increase of the furnace chamber smelting temperature, the impurity content in the high-purity niobium block finally obtained is getting less and less, and the quality of the high-purity niobium block is getting better and better.
[0036] What is disclosed above is only a preferred embodiment of the present invention, which certainly cannot be used to limit the scope of rights of the present invention. A person skilled in the art can understand that all or part of the processes of the above embodiments and equivalent changes made according to the claims of the present invention still fall within the scope of the invention.
Claims
1. A method for preparing high-purity smelted niobium for high-temperature alloy additives, characterized in that: The following steps are involved: S1. Prepare materials: Prepare the following raw materials by weight: 100 parts of niobium pentoxide, 35-45 parts of aluminum powder, 1-5 parts of calcium oxide and 2-7 parts of calcium fluoride; S2. Mixing: Put the above raw materials into a mixer and mix them evenly; S3, aluminothermic reduction reaction: The mixed raw materials are subjected to aluminothermic reduction reaction to obtain niobium aluminum alloy; S4, Crushing: The niobium aluminum alloy obtained in S3 is crushed into small pieces of 20-60 mm to obtain a block of niobium aluminum alloy; S5, first smelting: The blocky niobium aluminum alloy is spread flat in a horizontal electron beam furnace crucible for the first smelting to obtain a first-melting niobium plate; S6, Second Melting: After the primary smelting niobium plate is turned upside down, it is placed in the horizontal electron beam furnace crucible again, and a number of smelting niobium pads are placed under the primary smelting niobium plate to perform a second smelting to obtain a secondary smelting niobium plate; S7, the third smelting: The secondary smelting niobium plate is cross-cut into four equal parts and laid flat in a horizontal electron beam furnace crucible, and the cut edges are transferred to the periphery, and a number of high-purity smelting niobium pads are placed underneath, and then smelting is performed to obtain the tertiary smelting niobium plate; S8, cut into blocks: The tertiary smelting niobium plates are cut into blocks to obtain high-purity smelted niobium blocks.
2. The method for preparing high-purity smelted niobium for high-temperature alloy additives according to claim 1, characterized in that: During the first smelting in step S5 and the second smelting in step S6, the vacuum degree of the furnace chamber is less than or equal to 0.05 Pa, and the smelting power is 350-450 kW.
3. The method for preparing high-purity smelted niobium for high-temperature alloy additives according to claim 1, characterized in that: During the third smelting in step S7, the vacuum degree of the furnace chamber is less than or equal to 0.03 Pa, and the smelting power is 400-450 kW.
4. The method for preparing high-purity smelted niobium for high-temperature alloy additives according to claim 1, characterized in that: In step S1, the purity of the niobium pentoxide is greater than or equal to 99.50%, the purity of the metal aluminum powder is greater than or equal to 99%, the purity of the calcium oxide is greater than or equal to 90%, and the purity of the calcium fluoride is greater than or equal to 99%.
5. The method for preparing high-purity smelted niobium for high-temperature alloy additives according to claim 1, characterized in that: In step S1, the following raw materials are prepared by weight: 100 parts of niobium pentoxide, 38-42 parts of metal aluminum powder, 2-3 parts of calcium oxide, and 3-5 parts of calcium fluoride.
6. The method for preparing high-purity smelted niobium for high-temperature alloy additives according to claim 1, characterized in that: In step S1, the following raw materials are prepared by weight: 100 parts of niobium pentoxide, 40 parts of metal aluminum powder, 2 parts of calcium oxide, and 4 parts of calcium fluoride.
7. The method for preparing high-purity smelted niobium for high-temperature alloy additives according to claim 1, characterized in that: The aluminothermic reduction reaction in step S3 specifically comprises the following steps: S30, pouring the mixed materials into the crucible three times and compacting them respectively; S31, evacuate the reaction chamber to below 20Pa, and then introduce argon gas into the reaction chamber until the pressure in the reaction chamber rises to 0.07-0.065Mpa; S32, igniting to cause the material to undergo aluminothermic reduction reaction, and obtaining a reaction product after the reaction is completed; S33, the reaction product is slowly cooled in the furnace, and then taken out of the furnace and naturally cooled to room temperature; S34, separating the reaction product into slag and gold to obtain niobium aluminum alloy.
8. The method for preparing high-purity smelted niobium for high-temperature alloy additives according to claim 1, characterized in that: The purity of the smelted niobium pad in step S6 is higher than the purity of the first smelted niobium plate; The purity of the high-purity smelted niobium pad in step S7 is higher than the purity of the secondary smelted niobium plate.
9. The method for preparing high-purity smelted niobium for high-temperature alloy additives according to claim 1, characterized in that: In step S2, the mixing time is 3 hours.
10. The method for preparing high-purity smelted niobium for high-temperature alloy additives according to claim 7, characterized in that: In step S32, during the ignition, the ignition wire used includes a conductor made of bare aluminum wire and a spiral wire made of φ0.6-0.8mm nickel-chromium wire.
Citation Information
Cited By
Method for preparing metal tantalum by adopting calcium thermal reduction method
CN120776144A