Calcium carbonate whisker material and preparation method thereof

By controlling pH stages with magnesium and nitrate ions, and supplementing with calcium hydroxide and nitrate/bicarbonate, the method addresses purity and aspect ratio issues in aragonite calcium carbonate whisker production, enhancing yield and mechanical properties.

CN119082840APending Publication Date: 2024-12-06GUANGXI MODERN VOCATIONAL & TECH COLLEGE
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411228515.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-03
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Existing methods for preparing aragonite calcium carbonate whiskers face challenges in achieving high purity and stable aspect ratio due to quick reaction termination and wastage of crystal form regulators, necessitating improved reaction control and utilization of magnesium ions.

Method used

A method involving controlled pH stages with magnesium and nitrate ions, supplemented by calcium hydroxide and nitrate/bicarbonate solutions, extends the carbonization reaction and promotes whisker growth, resulting in higher aspect ratio and purity.

Benefits of technology

The method enhances the yield and purity of calcium carbonate whiskers by prolonging the reaction and regulating crystal growth, achieving improved mechanical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119082840A_ABST
    Figure CN119082840A_ABST
Patent Text Reader

Abstract

The invention discloses a calcium carbonate whisker material and a preparation method thereof, the preparation method comprises the following steps: mixing a calcium hydroxide suspension and a first crystal form control solution to obtain a mixed solution, heating, and introducing carbon dioxide to obtain a reaction system; and when the pH value of the reaction system reaches a first threshold value, supplementing the calcium hydroxide solution and the second crystal form control solution, keeping the introduction of the carbon dioxide, continuing the reaction until the pH value of the reaction system reaches a second threshold value, stopping the reaction, and collecting to obtain the calcium carbonate whisker material. The calcium hydroxide is supplemented in the later period of the carbonization reaction to prolong the progress of the carbonization reaction, and the second crystal form control solution is supplemented, so that the utilization of the magnesium ion solution and the yield of the calcium carbonate whiskers can be improved, and the aragonite phase whiskers can be promoted to continuously grow along the length direction; therefore, the calcium carbonate whisker with a higher length-diameter ratio is prepared.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of calcium carbonate whisker preparation, in particular to a calcium carbonate whisker material and a preparation method thereof. Background Art

[0002] Aragonite calcium carbonate whisker is a high-purity single crystal material with very good dimensional stability, good bending strength, tensile strength, wear resistance, aspect ratio and thermal stability. It can be used in different materials to enhance the performance of the body, such as plastic filling, friction materials, papermaking, coatings, biomedicine and other industries. And calcium carbonate whisker is expected to replace expensive inorganic whiskers such as potassium titanate and zinc oxide, so the industrial preparation of aragonite calcium carbonate whisker has a good prospect.

[0003] At present, after a long period of research and development, the preparation method and production process of aragonite calcium carbonate whiskers have gradually become mature and streamlined. The main preparation methods include: double decomposition reaction method, urea hydrolysis method, carbonization method, and calcium bicarbonate heating decomposition method. Among them, the carbonization method is currently considered to be the most potential method for large-scale preparation. However, there is no unified understanding of the growth mechanism of calcium carbonate whiskers, especially some details. How to prepare aragonite calcium carbonate whiskers with high purity and stable aspect ratio has always been the focus and difficulty of researchers. Some technologies also provide better methods. For example, CN114959895A discloses an ultra-long calcium carbonate whisker and a preparation method thereof. The preparation method includes mixing a crystal form control solution and a calcium hydroxide suspension, the crystal form control solution includes at least magnesium ions and nitrate ions, and raising the temperature of the mixed solution to 90-110°C; keeping the temperature of the mixed solution constant, and introducing carbon dioxide gas into the mixed solution for reaction. When the pH value of the reaction system decreases, filtering, taking the precipitate, and obtaining calcium carbonate whiskers. This method can obtain calcium carbonate whiskers with a length greater than 90 μm. A hyperbranched three-dimensional structure calcium carbonate whisker and its preparation method and application, the preparation method is to add a crystal form control solution to a calcium hydroxide suspension, the crystal form control agent includes at least magnesium ions and acetate ions, to form a mixed solution, keep the mixed solution at a constant temperature of 80 to 100°C, and introduce carbon dioxide to react. This method can prepare hyperbranched three-dimensional structure calcium carbonate whiskers.

[0004] At present, the preparation of calcium carbonate whiskers by carbonization requires a large amount of crystal form regulators, but the reaction terminates quickly, resulting in a large amount of crystal form regulators being wasted. It is necessary to provide a corresponding solution. Summary of the invention

[0005] In order to overcome the problems existing in the prior art, the present invention provides a method for preparing a calcium carbonate whisker material, comprising the following steps:

[0006] The calcium hydroxide suspension is mixed with the first crystal form control solution to obtain a mixed solution, and carbon dioxide is introduced into the mixed solution after heating to obtain a reaction system;

[0007] When the pH of the reaction system reaches a first threshold, calcium hydroxide solution and a second crystal form control solution are added, and carbon dioxide is kept flowing to continue the reaction until the pH of the reaction system reaches a second threshold, and the reaction is stopped to collect the calcium carbonate whisker material.

[0008] Furthermore, the first crystal form controlling solution is a magnesium ion solution, the volume ratio of the calcium hydroxide suspension to the magnesium ion solution is 3 to 5:1, and the molar ratio of calcium to magnesium in the mixed solution is 1:1.5 to 2.5;

[0009] The temperature of the mixed solution is raised to 90-110°C.

[0010] The industrial use of carbonization to prepare calcium carbonate whiskers requires the recycling of magnesium ion solutions controlled by crystal form. Magnesium ions are used in large quantities and are equivalent to catalysts in carbonization reactions. After the reaction, the filtered solution is basically a magnesium ion solution, but there is also a calcium carbonate whisker solution after the actual carbonization reaction. Directly using it in the production of calcium carbonate whiskers will seriously affect the purity and aspect ratio of the product. In order to improve the utilization of magnesium ions, prolonging the carbonization reaction is also a solution.

[0011] The present invention studies the growth process of calcium carbonate whiskers and finds that the early stage of the reaction is the main stage for the whiskers to grow into needle-shaped whiskers. However, once the Ca in the system 2+ and OH - ions are exhausted, and the carbonization reaction immediately enters the later stage, that is, the dissolution of magnesium hydroxide and the termination of the carbonization reaction. Therefore. The present invention supplements calcium hydroxide in the later stage of the carbonization reaction to extend the progress of the carbonization reaction, but directly introducing the calcium hydroxide solution will cause crystal distortion and purity reduction. Therefore, the present invention also introduces nitrate as a crystal form regulator, which can not only improve the utilization of magnesium ion solution and increase the output of calcium carbonate whiskers, but also promote the continued growth of aragonite phase whiskers along the length direction, thereby preparing calcium carbonate whiskers with a higher aspect ratio.

[0012] Furthermore, the first threshold refers to a pH of 7.3 to 7.8;

[0013] The second threshold refers to a pH range of 6.8 to 7.1.

[0014] Furthermore, the concentration of the supplementary calcium hydroxide solution is 0.01-0.02 mol / L, and its volume is 0.5-1 times the volume of the initial calcium hydroxide suspension.

[0015] Furthermore, the second crystal form controlling solution is a 0.1-0.5 mol / L nitrate ion solution, and its volume is 0.1-0.3 times the volume of the initial calcium hydroxide suspension.

[0016] The invention shows through a large number of experiments that in the presence of nitrate, introducing a small amount of bicarbonate ions into the reaction system can improve the growth of the crystal form and obtain calcium carbonate whiskers with a higher aspect ratio and more uniformity.

[0017] Furthermore, the second crystal form controlling solution is a mixed solution of 0.1 to 0.5 mol / L nitrate ions and 0.001 to 0.003 mol / L bicarbonate ions.

[0018] Furthermore, the preparation method of the calcium hydroxide suspension is to mix calcium oxide and water at a ratio of 5 to 10 g: 300 to 500 mL, and then perform a digestion reaction at 80 to 100° C. for 1 to 3 hours to obtain the calcium oxide suspension.

[0019] Furthermore, the flow rate of the carbon dioxide introduction is 10 to 30 mL / min.

[0020] It should be noted that the present invention does not impose strict restrictions on the sources of nitrate and bicarbonate. In order not to introduce impurity ions, calcium nitrate, magnesium nitrate, magnesium bicarbonate, calcium bicarbonate, etc. are preferred.

[0021] The present invention also provides a calcium carbonate whisker material, which is prepared by the above-mentioned preparation method.

[0022] The invention also provides application of the calcium carbonate whisker material in concrete mortar, plastic filling and friction material.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] The present invention supplements calcium hydroxide in the later stage of the carbonization reaction to prolong the progress of the carbonization reaction, and is supplemented with a second crystal form control solution, which can not only improve the utilization of the magnesium ion solution and the yield of the calcium carbonate whiskers, but also promote the continued growth of the aragonite phase whiskers along the length direction, thereby preparing the calcium carbonate whiskers with a higher aspect ratio. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0026] Figure 1The X-ray diffraction patterns of calcium carbonate whiskers prepared in the embodiments of the present invention and the comparative examples are shown;

[0027] Figure 2 The scanning electron microscope image of the calcium carbonate whisker prepared in Example 1 of the present invention is shown;

[0028] Figure 3 The scanning electron microscope image of the calcium carbonate whisker prepared in Example 2 of the present invention is shown;

[0029] Figure 4 The scanning electron microscope image of the calcium carbonate whisker prepared in Example 3 of the present invention is shown;

[0030] Figure 5 The scanning electron microscope image of the calcium carbonate whisker prepared in Example 4 of the present invention is shown;

[0031] Figure 6 The scanning electron microscope image of the calcium carbonate whisker prepared in Comparative Example 1 of the present invention is shown;

[0032] Figure 7 The scanning electron microscope image of the calcium carbonate whisker prepared in Comparative Example 2 of the present invention is shown. DETAILED DESCRIPTION

[0033] The endpoints and any values ​​of the ranges disclosed in the present invention are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more numerical ranges, which should be regarded as specifically disclosed in the present invention.

[0034] The following will be combined with the specific embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0035] Example 1

[0036] A method for preparing a calcium carbonate whisker material, comprising the following steps:

[0037] Step 1, 5.6g of calcium oxide was mixed with 400mL of water and heated to 90°C for digestion reaction for 2.5h to obtain a calcium hydroxide suspension with a total calcium molar amount of 0.1mol; 40.6g of magnesium chloride hexahydrate was mixed with 100mL of water and stirred at 200rpm for 15min to form a magnesium chloride solution with a total magnesium molar amount of 0.2mol; calcium hydroxide was dissolved in water to prepare a 0.015mol / L calcium hydroxide solution; calcium nitrate tetrahydrate was dissolved in water to prepare a 0.2mol / L calcium nitrate solution with a nitrate ion of 0.4mol / L;

[0038] Step 2, at a rotation speed of 300 rpm, 400 mL of calcium hydroxide suspension and 100 mL of magnesium chloride solution were mixed to obtain a mixed solution, and the temperature of the mixed solution was raised to 90° C., the temperature and the rotation speed were maintained, and carbon dioxide was introduced at a flow rate of 15 mL / min to obtain a reaction system. When the pH of the reaction system was 7.6, 300 mL of calcium hydroxide solution and 100 mL of calcium nitrate solution were added, and carbon dioxide was continued to be introduced at a flow rate of 15 mL / min until the pH of the reaction system dropped to 7.0, the reaction was stopped, and the precipitate was washed with water after filtering, and then transferred to a 100° C. constant temperature oven for drying for 8 h to obtain a calcium carbonate whisker material.

[0039] Example 2

[0040] A method for preparing a calcium carbonate whisker material, comprising the following steps:

[0041] Step 1, 5.6g of calcium oxide was mixed with 400mL of water and heated to 90°C for digestion reaction for 2.5h to obtain a calcium hydroxide suspension with a total calcium molar amount of 0.1mol; 40.6g of magnesium chloride hexahydrate was mixed with 100mL of water and stirred at 200rpm for 15min to form a magnesium chloride solution with a total magnesium molar amount of 0.2mol; calcium hydroxide was dissolved in water to prepare a 0.015mol / L calcium hydroxide solution; calcium nitrate tetrahydrate and calcium bicarbonate were dissolved in water to prepare a mixed solution of 0.4mol / L nitrate and 0.001mol / L bicarbonate;

[0042] Step 2, at a rotation speed of 300 rpm, 400 mL of calcium hydroxide suspension was mixed with 100 mL of magnesium chloride solution to obtain a mixed solution, and the temperature of the mixed solution was raised to 90 ° C., the temperature and the rotation speed were maintained, and carbon dioxide was introduced at a flow rate of 15 mL / min to obtain a reaction system. When the pH of the reaction system was 7.6, 300 mL of calcium hydroxide solution, 100 mL of a mixed solution of 0.4 mol / L nitrate and 0.001 mol / L bicarbonate were added, and carbon dioxide was continued to be introduced at a flow rate of 15 mL / min until the pH of the reaction system dropped to 7.0, the reaction was stopped, and the precipitate was washed with water after filtering, and then transferred to a 100 ° C constant temperature oven for drying for 8 h to obtain a calcium carbonate whisker material.

[0043] Example 3

[0044] A method for preparing a calcium carbonate whisker material, comprising the following steps:

[0045] Step 1, 5.6g of calcium oxide was mixed with 400mL of water and heated to 90°C for digestion reaction for 2.5h to obtain a calcium hydroxide suspension with a total calcium molar amount of 0.1mol; 40.6g of magnesium chloride hexahydrate was mixed with 100mL of water and stirred at 200rpm for 15min to form a magnesium chloride solution with a total magnesium molar amount of 0.2mol; calcium hydroxide was dissolved in water to prepare a 0.015mol / L calcium hydroxide solution; calcium nitrate tetrahydrate and calcium bicarbonate were dissolved in water to prepare a mixed solution of 0.4mol / L nitrate and 0.002mol / L bicarbonate;

[0046] Step 2, at a rotation speed of 300 rpm, 400 mL of calcium hydroxide suspension was mixed with 100 mL of magnesium chloride solution to obtain a mixed solution, and the temperature of the mixed solution was raised to 90 ° C., the temperature and the rotation speed were maintained, and carbon dioxide was introduced at a flow rate of 15 mL / min to obtain a reaction system. When the pH of the reaction system was 7.6, 300 mL of calcium hydroxide solution, 100 mL of a mixed solution of 0.4 mol / L nitrate and 0.002 mol / L bicarbonate were added, and carbon dioxide was continued to be introduced at a flow rate of 15 mL / min until the pH of the reaction system dropped to 7.0, the reaction was stopped, and the precipitate was washed with water after filtering, and then transferred to a 100 ° C constant temperature oven for drying for 8 h to obtain a calcium carbonate whisker material.

[0047] Example 4

[0048] A method for preparing a calcium carbonate whisker material, comprising the following steps:

[0049] Step 1, 5.6g of calcium oxide was mixed with 400mL of water and heated to 90°C for digestion reaction for 2.5h to obtain a calcium hydroxide suspension with a total calcium molar amount of 0.1mol; 40.6g of magnesium chloride hexahydrate was mixed with 100mL of water and stirred at 200rpm for 15min to form a magnesium chloride solution with a total magnesium molar amount of 0.2mol; calcium hydroxide was dissolved in water to prepare a 0.015mol / L calcium hydroxide solution; calcium nitrate tetrahydrate and calcium bicarbonate were dissolved in water to prepare a mixed solution of 0.4mol / L nitrate and 0.003mol / L bicarbonate;

[0050] Step 2, at a rotation speed of 300 rpm, 400 mL of calcium hydroxide suspension was mixed with 100 mL of magnesium chloride solution to obtain a mixed solution, and the temperature of the mixed solution was raised to 90 ° C., the temperature and the rotation speed were maintained, and carbon dioxide was introduced at a flow rate of 15 mL / min to obtain a reaction system. When the pH of the reaction system was 7.6, 300 mL of calcium hydroxide solution, 100 mL of a mixed solution of 0.4 mol / L nitrate and 0.003 mol / L bicarbonate were added, and carbon dioxide was continued to be introduced at a flow rate of 15 mL / min until the pH of the reaction system dropped to 7.0, the reaction was stopped, and the precipitate was washed with water after filtering, and then transferred to a 100 ° C constant temperature oven for drying for 8 h to obtain a calcium carbonate whisker material.

[0051] Comparative Example 1

[0052] A method for preparing a calcium carbonate whisker material, comprising the following steps:

[0053] Step 1, 5.6g of calcium oxide was mixed with 400mL of water and heated to 90°C for digestion reaction for 2.5h to obtain a calcium hydroxide suspension with a total calcium molar amount of 0.1mol; 40.6g of magnesium chloride hexahydrate was mixed with 100mL of water and stirred at 200rpm for 15min to form a magnesium chloride solution with a total magnesium molar amount of 0.2mol;

[0054] Step 2: At a rotation speed of 300 rpm, 400 mL of calcium hydroxide suspension and 100 mL of magnesium chloride solution are mixed to obtain a mixed solution, and at the same time, the temperature of the mixed solution is raised to 90° C., the temperature and the rotation speed are maintained, and carbon dioxide is introduced at a flow rate of 15 mL / min to obtain a reaction system. When the pH of the reaction system drops to 7.0, the reaction is stopped. After filtering, the precipitate is washed with water, and then transferred to a constant temperature oven at 100° C. for drying for 8 hours to obtain a calcium carbonate whisker material.

[0055] Comparative Example 2

[0056] A method for preparing a calcium carbonate whisker material, comprising the following steps:

[0057] Step 1, 5.6g of calcium oxide was mixed with 400mL of water and heated to 90°C for digestion reaction for 2.5h to obtain a calcium hydroxide suspension with a total calcium molar amount of 0.1mol; 40.6g of magnesium chloride hexahydrate was mixed with 100mL of water and stirred at 200rpm for 15min to form a magnesium chloride solution with a total magnesium molar amount of 0.2mol; calcium hydroxide was dissolved in water to prepare a 0.015mol / L calcium hydroxide solution;

[0058] Step 2, at a rotation speed of 300 rpm, 400 mL of calcium hydroxide suspension and 100 mL of magnesium chloride solution were mixed to obtain a mixed solution, and the temperature of the mixed solution was raised to 90° C., the temperature and the rotation speed were maintained, and carbon dioxide was introduced at a flow rate of 15 mL / min to obtain a reaction system. When the pH of the reaction system was 7.6, 300 mL of calcium hydroxide solution was added, and carbon dioxide was continued to be introduced at a flow rate of 15 mL / min until the pH of the reaction system dropped to 7.0, the reaction was stopped, and the precipitate was washed with water after filtering, and then transferred to a 100° C. constant temperature oven for drying for 8 h to obtain a calcium carbonate whisker material.

[0059] Test Case

[0060] The phase composition and lattice parameters of the calcium carbonate whisker materials prepared in the embodiments of the present invention and the comparative examples were tested by X-ray diffraction. Figure 1 As shown. It can be seen that the prepared calcium carbonate whisker material mainly has two phases of aragonite phase and calcite phase. The content of aragonite calcium carbonate whiskers was calculated using the following formula:

[0061]

[0062] Wherein, X is the mass fraction of aragonite calcium carbonate whiskers, i.e., the purity of aragonite calcium carbonate whiskers; a is the integrated intensity of the strongest peak of the aragonite phase; I c is the integrated intensity of the strongest peak of the calcite phase. The calculation results are shown in Table 1.

[0063] Table 1 Purity results of aragonite calcium carbonate whiskers

[0064] purity(%) Example 1 97.3 Example 2 98.2 Example 3 99.5 Example 4 96.1 Comparative Example 1 96.8 Comparative Example 2 56.4

[0065] It can be seen from the test results in Table 1 that, for the aragonite crystal orientation type of calcium carbonate whiskers, Example 3 of the present invention has the highest purity, while Comparative Example 2 has the lowest. This is because without adding nitrate as a control, the generated aragonite calcium carbonate whiskers are largely transformed into calcite.

[0066] The microscopic morphology of the calcium carbonate whiskers prepared in Examples 1 to 4 of the present invention and Comparative Examples 1 to 2 was also observed using a scanning electron microscope, and the results were: Figure 2 to Figure 7 As shown. Figure 2 , Figure 6 , Figure 7 It can be seen that the addition of calcium hydroxide in the later stage of the carbonization reaction can prolong the carbonization reaction. However, in Comparative Example 2 where no nitrate is added for regulation, an obvious calcite configuration appears. Figure 2The morphology of Example 1 shows that the present invention can prepare calcium carbonate whiskers with high purity and good morphology by improving the conventional preparation method of calcium carbonate whiskers, strictly controlling the pH of the reaction, and adding nitrate for regulation. Figure 2 to Figure 5 , it can be seen that the addition of bicarbonate can further regulate the calcium carbonate whiskers.

[0067] The average aspect ratio of the calcium carbonate whiskers was calculated based on the scanning electron microscope characterization results; the quality of the calcium carbonate whiskers obtained in other embodiments and comparative examples was compared with that in comparative example 1, and the results are shown in Table 2.

[0068] Table 2 Average aspect ratio and yield ratio results

[0069]

[0070]

[0071] It can also be seen from the results in Table 2 that the present invention can increase the yield of calcium carbonate whiskers by supplementing calcium hydroxide in the later stage of the carbonization reaction, and can also improve the aspect ratio of the calcium carbonate whisker material. This is due to the appropriate pH control and the introduction of nitrate and bicarbonate to better adjust the reaction.

[0072] Application Examples

[0073] 5 kg of calcium carbonate whiskers prepared in the embodiments of the present invention and the comparative example were respectively put into a mixer, mixed with 225 kg of cement, 1350 kg of river sand, 220 kg of water, and 100 kg of fly ash, and stirred at 80 rpm for 10 min to obtain mortar. The compressive strength of the mortar was tested with reference to the standard JGJ / T70 2009 "Standard for Test Methods of Basic Properties of Building Mortar", and the results are shown in Table 3.

[0074] Table 3 Compressive strength of mortar

[0075] Compressive strength(MPa) Example 1 11.8 Example 2 13.2 Example 3 14.9 Example 4 11.1 Comparative Example 1 10.6 Comparative Example 2 9.8 No calcium carbonate whiskers 7.8

[0076] It can be seen from the test results in Table 3 that the calcium carbonate whiskers prepared in the embodiment of the present invention can be applied to cement mortar to improve the strength of the mortar.

[0077] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a calcium carbonate whisker material, characterized in that, The steps are as follows, The calcium hydroxide suspension is mixed with the first crystal form control solution to obtain a mixed solution, and carbon dioxide is introduced into the mixed solution after heating to obtain a reaction system; When the pH of the reaction system reaches a first threshold, calcium hydroxide solution and a second crystal form control solution are added, and carbon dioxide is kept flowing to continue the reaction until the pH of the reaction system reaches a second threshold, and the reaction is stopped to collect the calcium carbonate whisker material.

2. the preparation method of calcium carbonate whisker material according to claim 1, is characterized in that, The first crystal form control solution is a magnesium ion solution, the volume ratio of the calcium hydroxide suspension to the magnesium ion solution is 3 to 5:1, and the molar ratio of calcium to magnesium in the mixed solution is 1:1.5 to 2.5; The temperature of the mixed solution is raised to 90-110°C.

3. the preparation method of calcium carbonate whisker material according to claim 1 is characterized in that, The first threshold refers to a pH of 7.3 to 7.8; The second threshold refers to a pH range of 6.8 to 7.

1.

4. The preparation method of calcium carbonate whisker material according to claim 1, wherein The concentration of the supplementary calcium hydroxide solution is 0.01-0.02 mol / L, and its volume is 0.5-1 times the volume of the initial calcium hydroxide suspension.

5. The preparation method of calcium carbonate whisker material according to claim 4, wherein The second crystal form controlling solution is a 0.1-0.5 mol / L nitrate ion solution, and its volume is 0.1-0.3 times the volume of the initial calcium hydroxide suspension.

6. The preparation method of calcium carbonate whisker material according to claim 5, wherein The second crystal form controlling solution is a mixed solution of 0.1 to 0.5 mol / L nitrate ions and 0.001 to 0.003 mol / L bicarbonate ions.

7. The preparation method of calcium carbonate whisker material according to claim 1, wherein The preparation method of the calcium hydroxide suspension is as follows: calcium oxide and water are mixed at a ratio of 5 to 10 g: 300 to 500 mL, and then the mixture is subjected to a digestion reaction at 80 to 100° C. for 1 to 3 hours to obtain the calcium oxide suspension.

8. The method for preparing a calcium carbonate whisker material according to any one of claims 1 to 7, characterized in that: The flow rate of the carbon dioxide introduction is 10 to 30 mL / min.

9. A calcium carbonate whisker material, characterized in that: The preparation method is described in any one of claims 1 to 8.

10. Use of the calcium carbonate whisker material according to claim 9 in concrete mortar, plastic filling and friction material.

Citation Information

Cited By

  • Ultra-light heat insulation coating and preparation method thereof

    CN120041018A