Method for dephosphorizing and extracting iron from high-phosphorus iron-containing material

Through pre-reduction and multi-stage melting technology, high-phosphorus and iron-containing materials are efficiently dephosphorized and iron-enhancing, solving the problems of low efficiency and insufficient utilization of phosphorus resources in the existing technology, achieving efficient dephosphorization and iron recovery, which is suitable for industrialization application.

CN119144790APending Publication Date: 2024-12-17XI'AN UNIVERSITY OF ARCHITECTURE AND TECHNOLOGY +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411284357.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-13
Publication Date
2024-12-17

AI Technical Summary

Technical Problem

The dephosphorization and iron extraction process of high-phosphorus iron-containing materials in the prior art is low in efficiency, and it is difficult to fully utilize phosphorus resources, resulting in the problem of efficient comprehensive utilization.

Method used

By pre-reducing the high-phosphorus iron-containing material and adding a reducing agent for one melting part, low-phosphorus slag and high-phosphorus molten iron are obtained, and then secondary melting part of the low-phosphorus slag is added with a flux and reducing agent to generate final slag and low phosphorus molten iron, using lime and/or limestone as flux, control temperature and addition amount to achieve efficient dephosphorization and iron recovery.

Benefits of technology

It has achieved the advantages of efficient dephosphorization effect, high iron recovery rate and high phosphorus resource utilization rate. It is suitable for steel production, with simple process and high production efficiency, and is suitable for industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119144790A_ABST
    Figure CN119144790A_ABST
Patent Text Reader

Abstract

The invention relates to the field of ferrous metallurgy, in particular to a dephosphorization and iron extraction method for a high-phosphorus iron-containing material. The dephosphorization and iron extraction method for the high-phosphorus iron-containing material comprises the following steps that after the high-phosphorus iron-containing material is subjected to pre-reduction treatment, a reducing agent is added for primary melt separation, and low-phosphorus slag and high-phosphorus molten iron are obtained; adding a reducing agent and a flux into the low-phosphorus slag for secondary melt separation to obtain final slag and low-phosphorus molten iron; the flux is lime and / or limestone. According to the method, the purposes of efficient dephosphorization and sufficient iron extraction are achieved through the combination of the pre-reduction treatment and the two-stage melting separation process. The dephosphorization efficiency is effectively improved, the quality of molten iron is ensured, and efficient separation and recovery of metal iron are achieved. And the whole technological process is simple, the production efficiency is high, and large-scale industrial utilization of the high-phosphorus iron-containing material can be achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of iron and steel metallurgy, and in particular to a method for dephosphorizing and extracting iron from high-phosphorus iron-containing materials. Background Art

[0002] High-phosphorus iron ore resources are abundant. Although the types of high-phosphorus iron ore in different regions are different and the mineralization ages are different, the mineralization principles are basically the same. Its composition is complex and it is recognized as a difficult-to-select iron ore at home and abroad. High-phosphorus iron ore has a high phosphorus content and phosphorus easily enters the iron, which makes it difficult to separate iron and phosphorus. It is difficult to achieve satisfactory results using traditional mineral processing methods. Therefore, the rational development of high-phosphorus iron ore, its efficient iron extraction and phosphorus removal, and its effective comprehensive utilization are of great strategic significance to alleviate the tight supply of iron ore.

[0003] Researchers have conducted extensive research on the smelting process of high-phosphorus iron ore and have achieved certain results. The main research methods currently include mineral processing, microbial processing, flotation, etc. However, due to the fine particle size of phosphorus minerals in high-phosphorus iron-containing materials and the close relationship between minerals and iron minerals, the existing mineral processing technology cannot efficiently separate iron and phosphorus elements.

[0004] Patent CN106367554B discloses a method for extracting iron and useful metals from secondary resources and producing slag wool. After being crushed, screened and other treatments, the iron-containing secondary resources are sent to a rotary hearth furnace for pre-reduction treatment. After pre-reduction, they are hot-sent and hot-charged to a primary melting furnace for secondary reduction. Qualified slag is used to produce high-quality slag wool, and unqualified iron-containing slag is returned to the primary melting furnace in a hot state for further melting and reduction treatment. The patent mainly proposes a two-step melting mode, which uses hot slag to produce slag wool while recovering useful metals simultaneously, thereby maximizing resource utilization efficiency and metal recovery rate. Patent CN105861815B discloses a method for dephosphorization and iron extraction of high-phosphorus iron ore, wherein a saturated aqueous solution of CaCl2 is sprayed on the surface of reduced coal and dried, so that the reduced coal is processed into modified reduced coal powder, followed by spraying a saturated aqueous solution of NaCO3 on the surface of high-phosphorus iron ore, grinding after drying, obtaining modified high-phosphorus iron ore powder, mixing the modified reduced coal powder and the modified high-phosphorus iron ore powder, making pellets and drying, and cooling the dried pellets after roasting to obtain pearl iron for dephosphorization and iron extraction. This patent designs unique modification and roasting steps for the dephosphorization demand of high-phosphorus iron ore. The above patent still has high process complexity, large equipment requirements and costs, and still does not solve the technical bottleneck of further efficient utilization of high-phosphorus iron ore at this stage, especially in terms of timely dephosphorization and efficient iron extraction, making it difficult to efficiently and comprehensively utilize high-phosphorus iron ore. Therefore, researching and developing efficient iron extraction and phosphorus removal technology that can realize industrial application is still a technical problem that needs to be solved in the steel production process. Summary of the invention

[0005] Based on the above content, the present invention provides a method for dephosphorizing and extracting iron from high-phosphorus iron-containing materials, aiming to solve the problems of low efficiency and difficulty in fully utilizing phosphorus resources in the dephosphorization and iron-extraction process of high-phosphorus iron-containing materials in the prior art. The present invention performs a pre-reduction treatment on the high-phosphorus iron-containing material, and then adds a reducing agent to perform a primary smelting in a smelting furnace to obtain low-phosphorus slag and high-phosphorus molten iron. Subsequently, a flux and a reducing agent are added to the low-phosphorus slag for a secondary smelting to generate final slag and low-phosphorus molten iron. The present invention has the advantages of good dephosphorization effect, high iron recovery rate, and high phosphorus resource utilization, and is suitable for efficient treatment of high-phosphorus iron-containing materials and comprehensive resource utilization in steel production.

[0006] To achieve the above object, the present invention provides the following solutions:

[0007] The present invention provides a method for dephosphorizing and extracting iron from a high-phosphorus iron-containing material, comprising the following steps:

[0008] Step 1, pre-reducing the high-phosphorus iron-containing material and then adding a reducing agent to perform a smelting separation to obtain low-phosphorus slag and high-phosphorus molten iron;

[0009] Step 2, adding a reducing agent and a flux to the low-phosphorus slag for secondary melting to obtain final slag and low-phosphorus molten iron;

[0010] The flux is lime and / or limestone.

[0011] After the pre-reduction treatment, the metallization rate of the high-phosphorus iron-containing material is 10% to 25%, thereby ensuring the aggregation of phosphorus and iron.

[0012] The present invention does not impose any particular limitation on the specific manner of the pre-reduction treatment, and any pre-reduction treatment manner well known to those skilled in the art may be used.

[0013] After the pre-reduction treatment, the part of the high-phosphorus iron-containing material with a particle size less than 2 mm accounts for 0% to 30% of the mass of the high-phosphorus iron-containing material after the pre-reduction treatment.

[0014] When the flux is a mixture of lime and limestone, the lime and limestone may be mixed in any proportion.

[0015] In a preferred embodiment of the present invention, in step 1, the reducing agent is at least one of coal powder, coke, coke powder, and blue coke, and the particle size is 0.1 to 2 mm.

[0016] In a preferred embodiment of the present invention, in step 1, the amount of reducing agent added is 2% to 4% by mass of the high-phosphorus iron-containing material.

[0017] In the present invention, the reducing agent in step 1 mainly plays the role of providing a reducing atmosphere; excessive addition of reducing agent will lead to a significant increase in the basicity of the slag; the slag becomes viscous and the fluidity is reduced, which will affect the separation effect of the iron ore and the slag. During the melting process, when the amount of reducing agent added is too high, it will react with the iron oxide in the high-phosphorus iron ore to form highly basic iron silicate. The occurrence of this side reaction will not only consume part of the reducing agent, but also reduce the output of iron, increase the amount of slag, and affect the recovery rate of molten iron.

[0018] In a preferred embodiment of the present invention, in step 1, the temperature of the first melting is 1400°C to 1550°C.

[0019] In a preferred embodiment of the present invention, the residual carbon content in the low-phosphorus slag is 0.2% to 0.6%.

[0020] The present invention does not impose any particular limitation on the time of the first smelting. The smelting time varies depending on the type of furnace, size of blast furnace, etc. Therefore, the present invention does not impose any particular limitation on the time of the first smelting. It is sufficient to control the residual carbon content in the low-phosphorus slag obtained after the first smelting to be 0.2% to 0.6%.

[0021] In the present invention, the primary melting temperature needs to be higher than the secondary melting temperature because the material in the primary melting is a solid high-phosphorus iron-containing material, while the material in the secondary melting is a molten material.

[0022] The temperature of the first melting is too high: it will cause the slag to be too fluid and too thin, making it difficult to separate the slag from the iron. Although the migration speed of phosphorus is accelerated, the slag-iron interface is blurred, and phosphorus may not be able to effectively enter the molten iron, resulting in unstable phosphorus removal effect.

[0023] The temperature of the first melting is too low: it will lead to insufficient reduction reaction during the melting process, reduce the reduction rate of phosphorus, and make it difficult to migrate from the slag to the molten iron. Therefore, the phosphorus content in the molten iron is insufficient and cannot meet the target requirements.

[0024] In a preferred embodiment of the present invention, in step 2, the reducing agent is at least one of coal powder, coke, coke powder, and blue coke, and the particle size is 4 to 10 mm.

[0025] The reason why the particle size of the reducing agent is limited to the above parameter range during the first and second smelting is: the high-phosphorus iron-containing material during the first smelting is solid, and adding small particles of reducing agent to the solid material can allow the reducing agent to enter the solid high-phosphorus iron-containing material; while in the second smelting, the material is molten, and at this time, choosing a reducing agent with larger particles can allow the reducing agent to be suspended in the slag. At this time, if a reducing agent with smaller particles is selected, the reducing agent will float on the surface of the molten material, resulting in poor reaction effect.

[0026] In a preferred embodiment of the present invention, in step 2, the amount of reducing agent added is 8% to 20% of the mass of the low-phosphorus slag.

[0027] In the present invention, the reason why the amount of reducing agent added in step 2 is limited to the above parameter range is to control the basicity of the secondary smelting. If the basicity is too low, the separation between slag and iron is insufficient, resulting in an increase in the amount of iron remaining in the slag, reducing the recovery rate of molten iron and affecting the smelting effect. If the basicity is too high, the CaO content is high, and the amount of slag generated will also increase. Too much slag not only increases the difficulty and cost of slag treatment, but also reduces smelting efficiency.

[0028] In a preferred embodiment of the present invention, the content of the part with a particle size of 3 to 8 mm in the flux is 80% to 100wt%, and the content of the part with a particle size greater than 8 mm is 0% to 20wt%; the amount of flux added is such that the basicity of the final slag is 1.6 to 1.9.

[0029] The reason why the particle size of the flux is limited to the above parameter range is that in the molten material, the reducing agent can be suspended and dispersed in the slag instead of floating on the upper surface or sinking to the bottom.

[0030] In a preferred embodiment of the present invention, the temperature of the secondary melting is 1350°C to 1500°C.

[0031] The present invention does not impose any particular limitation on the time of the secondary melting and separation, and the melting and separation time commonly used in the art may be adopted.

[0032] In the present invention, the temperature of the secondary melting is limited to the above parameter range because: since slag adjustment is performed during the first melting and the basicity becomes higher, the melting temperature during the secondary melting is lower; if the temperature of the secondary melting is too low, it will not be in a molten state in the secondary melting furnace and ultimately cannot be melted.

[0033] The basicity of the final slag is controlled to be 1.6 to 1.9 during the secondary melting. The present invention uses the amount of flux added to control the basicity of the final slag. Basicity = calcium oxide / silicon dioxide mass ratio.

[0034] The present invention uses an innovative method of pre-reduction and multi-stage melting to remove phosphorus and extract iron from high-phosphorus iron ore, filling the gap in the prior art. The proposed process is more convenient to operate and has achieved significant improvements in dephosphorization efficiency and iron recovery rate, which not only solves the problem of high-phosphorus iron ore resource utilization, but also provides a new idea for low-cost, high-efficiency industrial applications.

[0035] The present invention discloses the following technical effects:

[0036] (1) The method for dephosphorizing and extracting iron from a high-phosphorus iron-containing material of the present invention achieves the purpose of efficient dephosphorization and sufficient iron extraction by combining a pre-reduction treatment with a two-stage melting process. The present invention effectively improves the dephosphorization efficiency, ensures the quality of molten iron, and realizes efficient separation and recovery of metallic iron. The overall process is simple and the production efficiency is high, which can realize large-scale industrial utilization of high-phosphorus iron-containing materials.

[0037] (2) By adopting the technical solution provided by the present invention, the obtained high-phosphorus molten iron can be further converted into phosphate fertilizer, while the low-phosphorus molten iron can be directly used in the normal steelmaking process. This reduces the energy waste in the production process, improves the economic efficiency of the process, and provides more significant benefits for industrial application. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0039] Figure 1 The figure is a schematic diagram of the process flow of the method for dephosphorizing and extracting iron from high-phosphorus iron-containing materials of the present invention. DETAILED DESCRIPTION

[0040] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0041] It should be understood that the terms described in the present invention are only for describing a particular embodiment and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. The intermediate value in any stated value or stated range, and each smaller range between any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0042] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0043] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present invention description and examples are exemplary only.

[0044] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0045] The embodiment of the present invention is carried out on the basis of conventional treatment of high-phosphorus iron-containing materials in the prior art, and the dephosphorization effect is improved by the innovative methods of pre-reduction and multi-stage melting; the conventional method for treating high-phosphorus iron-containing materials in the prior art is a reduction-magnetic separation process, and a product with an iron grade of 90.01% and a phosphorus content of 0.129% is obtained. However, the iron loss in the process is large and the dephosphorization rate is low, which is not an ideal method for treating high-phosphorus iron ore. The reason may be that the process of reducing Fe2O3 to Fe3O4 is difficult to control, and it is easy to be over-reduced to FeO, resulting in poor magnetic separation effect, and the reduction temperature is low, which cannot destroy the oolitic structure of the ore, and the hematite and apatite are still closely connected, and it is not easy to separate iron and phosphorus.

[0046] The method for dephosphorizing and extracting iron from high-phosphorus iron-containing materials provided by the present invention first performs a pre-reduction treatment on the high-phosphorus iron-containing materials, and then effectively separates the high-phosphorus molten iron from the low-phosphorus slag through primary smelting and secondary smelting, and finally obtains low-phosphorus molten iron and final slag. The method has the advantages of significant dephosphorization effect and high molten iron recovery rate, effectively reduces energy consumption, improves economic benefits, and provides a feasible technical path for the industrial utilization of high-phosphorus iron-containing materials.

[0047] The process flow diagram of the method for dephosphorizing and extracting iron from high-phosphorus iron-containing materials of the present invention is as follows: Figure 1 shown.

[0048] The technical solutions described in the present invention, unless otherwise specified, are all conventional solutions in the art, and the reagents or raw materials used, unless otherwise specified, are purchased from commercial channels or have been disclosed.

[0049] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0050] Example 1

[0051] A method for smelting high-phosphorus iron-containing material comprises the following steps:

[0052] The high-phosphorus iron-containing material is subjected to a pre-reduction treatment. The metallization rate of the high-phosphorus iron-containing material after the pre-reduction treatment is 12.31%, and the portion with a particle size of less than 2 mm accounts for 13.64% (that is, the portion with a particle size of less than 2 mm in the high-phosphorus iron-containing material after the pre-reduction treatment is 13.64wt%). Coke accounting for 2% of the mass of the high-phosphorus iron-containing material is added, and the coke particle size does not exceed 0.5mm. The material is sent to a smelting furnace for a smelting. The temperature of the first smelting is set to 1550°C. After the first smelting is completed, low-phosphorus slag and high-phosphorus molten iron are obtained. The residual carbon content in the low-phosphorus slag is 0.26wt%. The low-phosphorus slag obtained after the first melting is added with coke accounting for 10% of the mass of the low-phosphorus slag, and the coke particle size does not exceed 8mm. At the same time, limestone with a particle size of 3-8mm accounting for 85% (that is, the part of the limestone with a particle size of 3-8mm contains 85wt%) is added as a flux for secondary melting. At this time, the basicity of the final slag is controlled to be 1.75, and the melting temperature is 1400℃. After the secondary melting, the final slag and low-phosphorus molten iron are obtained.

[0053] The phosphorus content of the high-phosphorus hot metal obtained in this embodiment is 0.717%, and the phosphorus content of the low-phosphorus hot metal is 0.093%.

[0054] Example 2

[0055] A method for smelting high-phosphorus iron-containing material comprises the following steps:

[0056] The high-phosphorus iron-containing material is subjected to a pre-reduction treatment. After the pre-reduction treatment, the metallization rate of the high-phosphorus iron-containing material is 19.31%, and the proportion of the part with a particle size less than 2 mm is 18.33%. Coke accounting for 3% of the mass of the high-phosphorus iron-containing material is added, and the coke particle size does not exceed 0.5 mm. It is sent to a smelting furnace for a first smelting. The temperature of the first smelting is set to 1500°C. After the first smelting, low-phosphorus slag and high-phosphorus molten iron are obtained, and the residual carbon content in the low-phosphorus slag is 0.40wt%. The low-phosphorus slag obtained after the first smelting is added with coke accounting for 12% of the mass of the low-phosphorus slag, and the coke particle size does not exceed 8mm. At the same time, limestone with a particle size of 3 to 8 mm and a proportion of 89% is added as a flux for a second smelting. At this time, the basicity of the final slag is controlled to be 1.80, and the smelting temperature is 1450°C. After the second smelting, the final slag and low-phosphorus molten iron are obtained.

[0057] The phosphorus content of the high-phosphorus hot metal obtained in this embodiment is 0.776%, and the phosphorus content of the low-phosphorus hot metal is 0.083%.

[0058] Example 3

[0059] A method for smelting high-phosphorus iron-containing material comprises the following steps:

[0060] The high-phosphorus iron-containing material is pre-reduced, and the metallization rate of the high-phosphorus iron-containing material after the pre-reduction treatment is 21.11%, and the part with a particle size less than 2mm accounts for 19.41%. Coke accounting for 3% of the mass of the high-phosphorus iron-containing material is added, and the coke particle size does not exceed 0.5mm. It is sent to a smelting furnace for a first smelting. The temperature of the first smelting is set to 1550℃. After the first smelting, low-phosphorus slag and high-phosphorus molten iron are obtained, and the residual carbon content in the low-phosphorus slag is 0.38wt%. The low-phosphorus slag obtained after the first smelting is added with coke accounting for 15% of the mass of the low-phosphorus slag, and the coke particle size does not exceed 8mm. At the same time, limestone with a particle size of 3 to 8mm and a proportion of 90% is added as a flux for a second smelting. At this time, the basicity of the final slag is controlled to be 1.85, and the smelting temperature is 1450℃. After the second smelting, the final slag and low-phosphorus molten iron are obtained.

[0061] The phosphorus content of the high-phosphorus hot metal obtained in this embodiment is 0.833%, and the phosphorus content of the low-phosphorus hot metal is 0.076%.

[0062] The phosphorus content of the low-phosphorus molten iron prepared by the embodiment of the present invention can reflect the dephosphorization effect of the present invention; the low-phosphorus molten iron prepared by the present invention can directly meet the requirements of normal smelting and can be smelted in the normal steelmaking smelting process area; the high-phosphorus molten iron obtained by one smelting can be processed and dephosphorized to prepare phosphate fertilizer, etc.

[0063] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A method for dephosphorizing and extracting iron from high-phosphorus iron-containing materials, It is characterized in that The following steps are involved: Step 1, pre-reducing the high-phosphorus iron-containing material and then adding a reducing agent to perform a smelting separation to obtain low-phosphorus slag and high-phosphorus molten iron; Step 2, adding a reducing agent and a flux to the low-phosphorus slag for secondary melting to obtain final slag and low-phosphorus molten iron; The flux is lime and / or limestone.

2. The method for dephosphorizing and extracting iron from high-phosphorus iron-containing materials according to claim 1, It is characterized in that After the pre-reduction treatment is completed, the metallization rate of the high-phosphorus iron-containing material is 10% to 25%.

3. The method for dephosphorizing and extracting iron from high-phosphorus iron-containing materials according to claim 1, It is characterized in that In step 1, the reducing agent is at least one of coal powder, coke, coke powder, and blue coke, and the particle size is 0.1 to 2 mm.

4. The method for dephosphorizing and extracting iron from high-phosphorus iron-containing materials according to claim 1, It is characterized in that In step 1, the amount of reducing agent added is 2% to 4% of the mass of the high-phosphorus iron-containing material.

5. The method for dephosphorizing and extracting iron from high-phosphorus iron-containing materials according to claim 1, It is characterized in that In step 1, the temperature of the first melting is 1400°C to 1550°C.

6. The method for dephosphorizing and extracting iron from high-phosphorus iron-containing materials according to claim 1, It is characterized in that The residual carbon content in low-phosphorus slag is 0.2% to 0.6%.

7. The method for dephosphorizing and extracting iron from high-phosphorus iron-containing materials according to claim 1, It is characterized in that In step 2, the reducing agent is at least one of coal powder, coke, coke powder, and semi-coke, and the particle size is 4 to 10 mm.

8. The method for dephosphorizing and extracting iron from high-phosphorus iron-containing materials according to claim 1, It is characterized in that In step 2, the amount of reducing agent added is 8% to 20% of the mass of the low-phosphorus slag.

9. The method for dephosphorizing and extracting iron from high-phosphorus iron-containing materials according to claim 1, It is characterized in that The content of the part with a particle size of 3 to 8 mm in the flux is 80% to 100wt%, and the content of the part with a particle size greater than 8 mm is 0% to 20wt%; the amount of flux added is such that the basicity of the final slag is 1.6 to 1.

9.

10. The method for dephosphorizing and extracting iron from high-phosphorus iron-containing materials according to claim 1, It is characterized in that The temperature of the secondary melting is 1350℃~1500℃.

Citation Information

Cited By

  • Phosphorus-containing waste liquid treatment and phosphorus removal agent regeneration synchronous device system

    CN224677931U