Coated knife shaft with diamond abrasive layer and manufacturing method thereof

By forming a diamond abrasive layer and a titanium carbide layer on the cutter shaft, the problem of poor wear resistance of the cutter shaft is solved, achieving high cutting accuracy and long life, while reducing costs and improving anti-fracture capabilities.

CN108214958BActive Publication Date: 2024-10-29JIAXING WORLDIA DIAMOND TOOLS CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN201810181796.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2018-03-06
Publication Date
2024-10-29
Estimated Expiration
2038-03-06

AI Technical Summary

Technical Problem

The cutter shaft has poor wear resistance during the glass cutting process, resulting in reduced cutting accuracy and quality. In addition, the existing PCD cutter shaft has high cost and insufficient anti-breakage capabilities.

Method used

A coated cutter spindle with a diamond abrasive grain layer is used. The diamond abrasive grains are brazed on the cutter spindle body and a titanium carbide layer is formed on its surface. The titanium carbide layer is manufactured using the physical vapor deposition method to enhance the bonding force and strength of the diamond abrasive grains. Wear resistance.

Benefits of technology

It improves the wear resistance and cutting accuracy of the cutter shaft, extends its service life, reduces production costs, and provides higher anti-breakage capabilities and long-lasting high cutting quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN108214958B_ABST
    Figure CN108214958B_ABST
Patent Text Reader

Abstract

The present application provides a coated blade shaft with a diamond abrasive layer, including a blade shaft body and a diamond abrasive layer fixed on the surface of the blade shaft body. The coated blade shaft has a higher holding force on the blade wheel. Compared with ordinary metal blade shafts, the coated blade shaft with a diamond abrasive layer has good wear resistance and a long service life. The blade wheel installed with the coated blade shaft is more stable in cutting glass. The present application also provides a method for manufacturing the above-mentioned coated blade shaft, specifically, brazing a brazing sublayer on the surface of the blade shaft body, and then physically vapor depositing a titanium carbide sublayer on the brazing sublayer. The raw materials used in the method are widely available. The method provided by the present application can be used to uniformly braze diamond abrasives on the surface of the blade shaft body, and can uniformly set a titanium carbide sublayer on the surface of the brazing sublayer. The method is simple and the conditions are mild. The diamond abrasives are firmly and stably in the brazing sublayer and the titanium carbide sublayer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the field of diamond abrasive tools, and specifically relates to a coated cutter shaft with a diamond abrasive layer and a manufacturing method thereof. Background Art

[0002] The knife body used for cutting glass mainly includes a knife wheel, a knife shaft and a knife frame, wherein the knife wheel for cutting is installed on the knife frame through the knife shaft, and the knife shaft is installed on the knife frame. As the knife body moves on the glass surface, the knife wheel rotates around the knife shaft, thereby forming scratches on the glass surface, and then other processing is performed to complete the cutting of the glass.

[0003] The cutter shaft is usually made of hard metal, alloy or PCD material. The glass chips generated in the process of cutting glass will enter the gap between the cutter shaft and the cutter wheel. As the cutter wheel rotates, the glass chips clamped between the cutter shaft and the cutter wheel will wear the metal cutter shaft or PCD cutter shaft, causing the running trajectory of the cutter wheel to deviate from the straight line, thereby reducing the cutting accuracy and cutting quality.

[0004] Therefore, it is urgent to develop a knife shaft with strong wear resistance and low price. Summary of the invention

[0005] In order to solve the problem of poor wear resistance of the blade shaft, the present application provides a coated blade shaft with a diamond abrasive layer, the coated blade shaft includes a blade shaft body and a diamond abrasive layer fixedly arranged on the surface of the blade shaft body, the exposed heights of the diamond abrasives in the diamond abrasive layer are similar, and at least one layer of diamond abrasive layer can be arranged between the diamond abrasive layer and the blade shaft body. The present application also provides a method for preparing the above-mentioned coated blade shaft, the method brazing a brazing sublayer on the blade shaft body, and then preparing a titanium carbide layer on the brazing layer by physical vapor deposition, the method is simple and easy to operate, and has low production cost.

[0006] The purpose of the present application is to provide a coated blade shaft with a diamond abrasive layer, the coated blade shaft comprising: a blade shaft body 1 and a diamond abrasive layer 2 arranged on the surface of the blade shaft body 1, the diamond abrasive layer 2 comprising a brazing sublayer 21 brazed on the blade shaft body 1, a titanium carbide sublayer 22 arranged on the brazing sublayer 21 by physical vapor deposition, and diamond abrasives 23 embedded in the brazing sublayer 21 and the titanium carbide sublayer 22, the outer ends of the diamond abrasives 23 extending out of the titanium carbide sublayer 22.

[0007] In one feasible manner, the particle size of the diamond abrasive 23 is 5 to 50 μm, the particle size tolerance range is ±2 μm, the length L1 of the diamond abrasive 23 extending out of the brazing sublayer 21 is 40% to 60% of the thickness D of the diamond abrasive layer 2, and the thickness D of the diamond abrasive layer 2 is the distance from the outer end of the diamond abrasive 23 to the side of the brazing sublayer 21 close to the arbor body 1.

[0008] In one achievable manner, the outer diameter of the coated cutter shaft is 0.77-0.79 mm, wherein the outer diameter of the coated cutter shaft is measured by the diameter of the largest circumscribed circle where the outer ends of the diamond abrasive particles are located.

[0009] In one achievable manner, the brazing material used to manufacture the brazing sublayer 21 is selected from a copper-based alloy solder containing active elements, a silver-based alloy solder containing active elements, and a nickel-based alloy solder containing active elements, and the active elements include titanium and chromium.

[0010] Due to the high hardness of diamond abrasive grains, after the cutter wheel is installed on the coated cutter shaft, the glass chips generated during the glass cutting process can enter the gaps between the diamond abrasive grains. As the cutter wheel rotates continuously, the glass chips are crushed into glass chips with smaller particle sizes by the diamond abrasive grains. Compared with a simple metal cutter shaft, an alloy cutter shaft or a PCD cutter shaft, the crushed glass chips cause little wear on the diamond abrasive grains. In addition, most of the glass chips will be discharged from the cutter wheel hole, so that the glass chips generated by cutting the glass will not hinder the rotation of the cutter wheel. Therefore, the use of the coated cutter shaft provided by the present application can provide long-lasting high cutting accuracy and excellent cutting quality in the process of cutting glass.

[0011] Since there are partially exposed diamond abrasives in the diamond brazing layer, and the friction coefficient between the diamond abrasives and the cutter wheel is greater than the friction coefficient between the ordinary metal cutter shaft and the cutter wheel, the coated cutter shaft provided in the embodiment of the present application has a higher holding force on the cutter wheel, and. The titanium carbide sublayer further strengthens the bonding strength between the brazing material and the diamond abrasives, and enhances the holding force of the brazing material on the diamond abrasives, so that the diamond abrasives are embedded more firmly in the brazing sublayer and are not easy to fall off. At the same time, compared with ordinary metal cutter shafts, alloy cutter shafts or PCD cutter shafts, the coated cutter shaft with a diamond abrasive layer has good wear resistance and a long service life, and the cutter wheel installed with the coated cutter shaft is more stable in cutting glass; compared with the PCD (polycrystalline diamond) cutter shaft, the coated cutter shaft provided in the embodiment of the present application is low in price and has high anti-fracture ability.

[0012] In one practicable manner, multiple layers of the diamond abrasive grain layer 2 may be provided on the surface of the arbor body 1 .

[0013] The present application also provides a method for manufacturing the above-mentioned coated knife shaft, the method comprising:

[0014] Step 1, pre-treating the blade shaft body 1 to remove grease and other dirt on the surface, and evenly mixing the diamond abrasive grains and the brazing material to obtain a mixture;

[0015] Step 2, installing the blade shaft body 1 processed in step 1 in a brazing mold, with a gap between the blade shaft body 1 and the brazing mold, and adding the mixture prepared in step 1 into the gap;

[0016] Step 3, in an aerobic environment, heating the mold installed with the blade shaft body 1 and the brazing material obtained in step 2;

[0017] Step 4, in an oxygen-free environment, such as in a vacuum furnace, further heating the workpiece obtained in step 3;

[0018] Step 5, using physical vapor deposition to produce a titanium carbide sublayer on the surface of the workpiece obtained in step 4;

[0019] Step 6, removing the titanium carbide deposited on the surface of the diamond abrasive grains in the workpiece obtained in step 5, so that the diamond abrasive grains extending out of the titanium carbide sublayer are partially exposed, and the outer diameter of the obtained coated tool shaft is uniform.

[0020] In one achievable manner, the weight ratio of diamond abrasive grains to brazing material is 1:(3-30).

[0021] In one achievable manner, in step 3, the mold obtained in step 2 and equipped with the blade shaft body (1) and the brazing material is heated to 50° C. to 150° C. and kept at this temperature for 5 to 10 minutes.

[0022] In one achievable manner, in step 4, the workpiece obtained in step 3 is further heated to 800° C. to 1100° C., and is kept at this temperature for 10 seconds to 60 seconds.

[0023] In one practicable manner, after completing steps 1 to 6, steps 1 to 6 are continued on the surface of the diamond abrasive layer to obtain a coated blade shaft having multiple layers of diamond abrasive layers.

[0024] Since diamond has a greater hardness, the wear resistance of the coated blade shaft provided in the present application is significantly improved, and the diamond abrasives can crush the glass chips clamped between the coated blade shaft and the blade wheel into smaller fragments, thereby making the cutting smoother and further reducing the wear of the coated blade shaft by the glass chips, thereby improving the cutting accuracy and cutting quality.

[0025] The method for manufacturing the aforementioned coated arbor provided in the present application uses raw materials from a wide range of sources. The method provided in the present application can be used to evenly braze diamond abrasive grains on the surface of the arbor body, and can evenly set a titanium carbide sublayer on the surface of the brazing sublayer. The method is simple and the conditions are mild. The diamond abrasive grains are firmly and stably located in the brazing sublayer and the titanium carbide sublayer.

[0026] The embodiment of the present application achieves brazing through the chemical reaction between diamond abrasives and brazing material. At the same time, the brazing sublayer further improves the bonding strength between the diamond abrasives and the brazing sublayer, reducing the risk of diamond abrasives falling off during use, thereby achieving the high-precision production requirements of the coated knife shaft process and reducing the production cost of the coated knife shaft. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 A cross-sectional view of a coated knife shaft having a diamond abrasive layer provided in an embodiment of the present application;

[0028] Figure 2 A cross-sectional view of another coated blade shaft having a diamond abrasive layer provided in an embodiment of the present application.

[0029] Description of Reference Numerals

[0030] 1-shaft body, 2-diamond abrasive grain layer, 21-brazing sublayer, 22-titanium carbide sublayer, 23-diamond abrasive grains. DETAILED DESCRIPTION

[0031] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0032] The present invention is described in detail below.

[0033] Figure 1 A cross-sectional view of a coated blade shaft with a diamond abrasive layer provided in an embodiment of the present application, please refer to Figure 1 The coated blade shaft comprises: a blade shaft body 1 and a diamond abrasive layer 2 arranged on the surface of the blade shaft body 1.

[0034] The blade shaft body 1 can be any blade shaft used to mount a blade wheel on a blade holder in the prior art. For example, the blade shaft body 1 can be Figure 1The blade shaft shown includes a coaxial and integrally formed cone and cylinder, and the outer diameter of the blade shaft body 1 is slightly smaller than the outer diameter of the ordinary blade shaft, so that after the diamond abrasive layer is provided on the surface of the blade shaft body, the outer diameter of the coated blade shaft is equivalent to the outer diameter of the ordinary blade shaft. In this application, the outer diameter of the coated blade shaft refers to the outer diameter of the part around which the blade wheel rotates, for example, Figure 1 For the coated blade shaft shown, the outer diameter of the coated blade shaft refers to the outer diameter of the cylindrical part of the coated blade shaft.

[0035] In one practicable manner, the arbor body 1 can be made of materials such as steel, iron or alloy.

[0036] The diamond abrasive layer 2 includes a brazing sublayer 21 brazed on the arbor body 1, a titanium carbide sublayer 22 disposed on the brazing sublayer 21 by physical vapor deposition, and diamond abrasives 23 embedded in the brazing sublayer 21 and the titanium carbide sublayer 22, wherein the outer ends of the diamond abrasives 23 extend out of the titanium carbide sublayer 22.

[0037] In one feasible manner, the particle size of the diamond abrasive grains 23 is 5 μm to 50 μm, and the particle size tolerance range is ±2 μm. Under different cutting requirements, the amount and particle size of glass chips generated by cutting glass are different. Therefore, diamond abrasive grains with different particle sizes can be used as fillers for the diamond abrasive layer for different cutting requirements. However, for the same coated arbor, the particle size of the selected diamond abrasive grains is relatively uniform. For example, if diamond abrasive grains with a particle size of 5 μm are selected, diamond abrasive grains with a particle size range of 5 ± 2 μm can be selected, thereby ensuring that the height of the diamond abrasive grains set on the surface of the arbor body is uniform, and the distribution of the diamond abrasive grains on the arbor body is also relatively uniform.

[0038] In an achievable manner, the length L1 of the diamond abrasive grains 23 extending out of the brazing sublayer 21 is 40% to 60% of the thickness D of the diamond abrasive grain layer 2, and the thickness D of the diamond abrasive grain layer 2 is the distance between the outer end of the diamond abrasive grains 23 and the side of the brazing sublayer 21 close to the blade shaft body 1. If the length L1 of the diamond abrasive grains 23 extending out of the brazing sublayer 21 is less than 40% of the thickness D of the diamond abrasive grain layer 2, the portion of the diamond abrasive grains exposed in the titanium carbide sublayer is too small to clearly reflect the effect of the diamond abrasive grains; if the length L1 of the diamond abrasive grains 23 extending out of the brazing sublayer 21 is greater than 60% of the thickness D of the diamond abrasive grain layer 2, the diamond abrasive grains 23 are not stable in the brazing sublayer 21, which may cause the diamond abrasive grains to fall off during the process of cutting glass, thereby causing the outer diameter of the coated blade shaft to be uneven, thereby reducing the cutting accuracy and cutting quality.

[0039] In one achievable manner, the outer diameter of the coated cutter shaft is 0.77-0.79 mm, wherein the outer diameter of the coated cutter shaft is measured by the diameter of the largest circumscribed circle where the outer ends of the diamond abrasive particles are located. For different cutter wheels, coated cutter shafts with different outer diameters can be used. The outer diameter of the coated cutter shaft provided in the present application is 0.77 mm to 0.79 mm, which can ensure the normal use of the cutter wheel and fully reflect the effect of the diamond abrasive particles during use.

[0040] In the present application, the thickness ratio of the brazing sublayer 21 to the titanium carbide sublayer 22 is not limited, and can be a thickness ratio that can be achieved in the prior art. For example, the thickness of the brazing sublayer is 0.01 mm to 0.1 mm, and the thickness of the titanium carbide sublayer is 0.5 μm to 5 μm.

[0041] In an achievable manner, the brazing sublayer 21 is disposed on the surface of the arbor body by brazing. Specifically, the method includes:

[0042] Step 1, pre-treating the blade shaft body 1 to remove surface grease and other dirt, and evenly mixing diamond abrasive grains with brazing material to obtain a mixture.

[0043] In one achievable manner, the brazing material used to manufacture the brazing sublayer 21 is selected from one of a copper-based alloy solder containing active elements, a silver-based alloy solder containing active elements, and a nickel-based alloy solder containing active elements, wherein the active elements include titanium and chromium, and may also include other chemically active elements, such as manganese and tin. The present application utilizes the titanium element in the brazing material to react chemically with diamond abrasive grains during the brazing process to generate titanium carbide in the brazing sublayer 21. Since the generated titanium carbide has a strong interaction force with the diamond abrasive grains, the diamond abrasive grains can be firmly embedded in the brazing sublayer 21.

[0044] In one practicable manner, the brazing material used in the present application is in granular form so as to be mixed with diamond abrasive particles and to be convenient for use in a brazing mold.

[0045] In one achievable manner, the weight ratio of diamond abrasive grains to brazing material is 1:(3-30). Since the inner diameter of the mold used for brazing in the present application is not adjustable, once the particle size of the diamond abrasive grains is selected, the density of the diamond abrasive grains embedded in the coated arbor can be adjusted by adjusting the weight ratio of the diamond abrasive grains to the brazing material. Specifically, increasing the weight ratio of the brazing material reduces the distribution density of the diamond abrasive grains, and reducing the weight ratio of the brazing material increases the distribution density of the diamond abrasive grains.

[0046] Step 2, installing the blade shaft body 1 processed in step 1 in a brazing mold, there is a gap between the blade shaft body 1 and the brazing mold, and adding the mixture prepared in step 1 into the gap.

[0047] In one achievable manner, the present application selects a brazing material having a particle size close to that of the selected diamond abrasive particles, so that the brazing material and the diamond abrasive particles can be mixed more fully and evenly.

[0048] In one feasible method, the inner hole shape of the mold is similar to the outer shape of the blade shaft body, with the only difference being that the size of the inner hole of the mold is slightly larger than the size of the blade shaft body, so that after the blade shaft body is installed in the mold, a gap can be formed between the blade shaft body and the inner wall of the mold.

[0049] Further, after the blade shaft body is installed in the mold, the blade shaft body is coaxial with the mold, so that the distance between the blade shaft body and the inner wall of the mold is equal, so that the thickness of the brazing layer formed on the surface of the blade shaft body is uniform. Optionally, the distance between the blade shaft body and the inner wall of the mold is slightly larger than the particle size of the diamond abrasive grains, so that the diamond abrasive grains can be evenly distributed between the blade shaft body and the inner wall of the mold, and will not be mostly clamped at the top of the gap due to the excessively large particle size.

[0050] Step 3, in an aerobic environment, heating the mold installed with the blade shaft body 1 and the brazing material obtained in step 2.

[0051] In one practicable manner, the mold mounted with the blade shaft body 1 and the brazing material obtained in step 2 is heated to 50° C. to 150° C. and kept at this temperature for 5 to 10 minutes.

[0052] This step is performed in an oxygen environment, and the low-melting-point material in the brazing material is melted at the above temperature and reacts with oxygen to form oxides, thereby sintering the diamond abrasive grains to the surface of the arbor body 1.

[0053] Step 4, in an oxygen-free environment, continue to heat the workpiece obtained in step 3.

[0054] In one achievable manner, in step 4, the workpiece obtained in step 3 is further heated to 800°C to 1100°C and kept at this temperature for 10s to 60s. Under the above temperature conditions, the high melting point substance in the brazing material melts and is evenly coated on the surface of the blade shaft body 1. After the heat preservation, the workpiece is cooled to complete the brazing of the diamond abrasive grains.

[0055] Step 4 is performed in an oxygen-free environment to prevent the brazing material and diamond from coming into contact with oxygen to cause an oxidation reaction, thereby maintaining the single-substance state of the brazing material. More importantly, it is to prevent the diamond from coming into contact with oxygen under high temperature conditions to generate carbon dioxide, thereby maintaining the integrity of the shape of the diamond abrasive grains.

[0056] In this step, the oxygen-free environment may be, for example, a vacuum furnace.

[0057] In one achievable manner, the titanium carbide sublayer 22 is disposed on the brazing sublayer 21 by physical vapor deposition (PVD).

[0058] Physical vapor deposition is a film manufacturing method that uses physical forms such as evaporation or sputtering under vacuum conditions to convert solid materials into atomic, molecular or ionic gas phase substances and then deposits these energy-carrying evaporated particles onto the surface of a substrate or part to form a film layer.

[0059] The method of manufacturing the TiC sublayer by PVD method in the embodiment of the present application is as follows: an arc is discharged on the Ti target in a vacuum furnace, and the metal Ti is ionized to generate Ti ions; at the same time, methane or C2H2 gas is introduced into the furnace chamber, and under the action of the tungsten wire discharge, the diamond abrasive grains are ionized to generate C ions. The Ti ions and C ions are attracted by the place where the bias voltage exists (specifically the placement position of the knife shaft body and the surface of the brazing sublayer in the embodiment of the present application), and move. TiC is generated on the surface of the brazing sublayer, and as the arc is continuously discharged, the amount of TiC generated gradually increases, thereby forming a TiC sublayer with a preset thickness on the surface of the brazing layer.

[0060] In the embodiment of the present application, a TiC sublayer is provided on the brazing sublayer to further improve the bonding force between the brazing material and the diamond abrasive by increasing the number of TiC molecules on the surface of the brazing sublayer, and to make the total thickness of the brazing sublayer and the titanium carbide sublayer more uniform.

[0061] Figure 2 Another coated blade shaft provided in the embodiment of the present application is provided in combination with Figure 2 , a plurality of diamond abrasive grain layers 2 are arranged on the surface of the blade shaft body 1. For example, Figure 2 The coated blade shaft shown includes two layers of diamond abrasive grains, wherein the diamond abrasive grain layer close to the blade shaft body is the first diamond abrasive grain layer, and the diamond abrasive grain layer away from the blade shaft body is the second diamond abrasive grain layer.

[0062] The thickness of the first diamond abrasive grain layer may be the same as or different from the thickness of the second diamond abrasive grain layer, and the particle sizes of the diamond abrasive grains embedded in the first diamond abrasive grain layer and the diamond abrasive grains embedded in the second diamond abrasive grain layer may be the same as or different.

[0063] As the coated blade shaft is continuously used, the second diamond abrasive grain layer on the surface of the coated blade shaft may fall off and expose the first diamond abrasive grain layer, thereby increasing the service life of the coated blade shaft. Moreover, if the outer diameter of the blade shaft body is smaller than the outer diameter of the preset blade shaft body, the outer diameter of the preset blade shaft body can be increased by adding the first diamond abrasive grain layer, so that the outer diameter of the prepared coated blade shaft can reach the target outer diameter.

[0064] Due to the high hardness of diamond abrasive grains, after the cutter wheel is installed on the coated cutter shaft, the glass chips generated during the glass cutting process can enter the gaps between the diamond abrasive grains. As the cutter wheel rotates continuously, the glass chips are crushed into glass chips with smaller particle sizes by the diamond abrasive grains. Compared with a simple metal cutter shaft, the crushed glass chips cause little wear on the diamond abrasive grains. In addition, most of the glass chips will be discharged from the cutter wheel hole, so that the glass chips generated by cutting the glass will not hinder the rotation of the cutter wheel. Therefore, the use of the coated cutter shaft provided by the present application can provide long-lasting high cutting accuracy and excellent cutting quality in the process of cutting glass.

[0065] Since there are partially exposed diamond abrasive grains in the diamond brazing layer, and the friction coefficient between the diamond abrasive grains and the cutter wheel is greater than the friction coefficient between the ordinary metal cutter shaft and the cutter wheel, the coated cutter shaft provided in the embodiment of the present application has a higher holding force on the cutter wheel, and the titanium carbide sublayer further strengthens the bonding strength between the brazing material and the diamond abrasive grains, and enhances the holding force of the brazing material on the diamond abrasive grains, so that the diamond abrasive grains are embedded more firmly in the brazing sublayer and are not easy to fall off. At the same time, compared with ordinary metal cutter shafts, the coated cutter shaft with a diamond abrasive grain layer has good wear resistance and a long service life, and the cutter wheel installed with the coated cutter shaft is more stable in cutting glass; compared with PCD (polycrystalline diamond) cutter shafts, the coated cutter shaft provided in the embodiment of the present application is low in price and has high anti-fracture ability.

[0066] The present application also provides a method for manufacturing the aforementioned coated knife shaft, the method comprising:

[0067] Step 1, pre-treating the blade shaft body 1 to remove grease and other dirt on the surface, and evenly mixing the diamond abrasive grains and the brazing material to obtain a mixture;

[0068] Step 2, installing the blade shaft body 1 processed in step 1 in a brazing mold, with a gap between the blade shaft body 1 and the brazing mold, and adding the mixture prepared in step 1 into the gap;

[0069] Step 3, in an aerobic environment, heating the mold installed with the blade shaft body 1 and the brazing material obtained in step 2;

[0070] Step 4, in an oxygen-free environment, continuing to heat the workpiece obtained in step 3;

[0071] Step 5, using physical vapor deposition to produce a titanium carbide sublayer on the surface of the workpiece obtained in step 4;

[0072] Step 6, removing the titanium carbide deposited on the surface of the diamond abrasive grains in the workpiece obtained in step 5, so that the diamond abrasive grains extending out of the titanium carbide sublayer are partially exposed, and the outer diameter of the obtained coated tool shaft is uniform.

[0073] The specific implementation of steps 1 to 4 of the present method can refer to the aforementioned description of the manufacturing process of the brazing sub-layer, which will not be repeated here.

[0074] The specific implementation of step 5 of the present method can refer to the above description of the manufacturing process of the titanium carbide sublayer, which will not be repeated here.

[0075] In step 6 of the method, the titanium carbide deposited on the surface of the diamond abrasive grains may be removed by using a grinding tool to expose the diamond abrasive grain bodies.

[0076] In one achievable manner, steps 1 to 6 are continuously performed on the surface of the diamond abrasive grain layer to obtain a coated blade shaft having multiple layers of diamond abrasive grain layers.

[0077] The method for manufacturing the aforementioned coated arbor provided in the present application uses raw materials from a wide range of sources. The method provided in the present application can be used to evenly braze diamond abrasive grains on the surface of the arbor body, and can evenly set a titanium carbide sublayer on the surface of the brazing sublayer. The method is simple and the conditions are mild. The diamond abrasive grains are firmly and stably located in the brazing sublayer and the titanium carbide sublayer.

[0078] The embodiment of the present application achieves brazing through the chemical reaction between diamond abrasives and brazing material. At the same time, the brazing sublayer further improves the bonding strength between the diamond abrasives and the brazing sublayer, reducing the risk of diamond abrasives falling off during use, thereby achieving the high-precision production requirements of the coated knife shaft process and reducing the production cost of the coated knife shaft.

[0079] The present application is described in detail above in conjunction with specific implementation methods and exemplary examples, but these descriptions cannot be understood as limiting the present application. Those skilled in the art understand that, without departing from the spirit and scope of the present application, a variety of equivalent replacements, modifications or improvements can be made to the technical solution of the present application and its implementation methods, all of which fall within the scope of the present application. The scope of protection of the present application shall be subject to the attached claims.

Claims

1. A coated knife shaft with a diamond abrasive layer, characterized in that: include: A knife shaft body (1) and a diamond abrasive grain layer (2) arranged on the surface of the knife shaft body (1), wherein the diamond abrasive grain layer (2) comprises a brazing sublayer (21) brazed on the knife shaft body (1), a titanium carbide sublayer (22) arranged on the brazing sublayer (21) by physical vapor deposition, and diamond abrasive grains (23) embedded in the brazing sublayer (21) and the titanium carbide sublayer (22), wherein the outer ends of the diamond abrasive grains (23) are The diamond abrasive grains (23) extend out of the titanium carbide sublayer (22); wherein the particle size of the diamond abrasive grains (23) is 5 to 50 μm, the particle size tolerance range is ±2 μm, the length L1 of the diamond abrasive grains (23) extending out of the brazing sublayer (21) is 40% to 60% of the thickness D of the diamond abrasive grain layer (2), and the thickness D of the diamond abrasive grain layer (2) is the distance between the outer end of the diamond abrasive grains (23) and the side of the brazing sublayer (21) close to the blade shaft body (1); Multiple layers of diamond abrasive grain layers (2) are arranged on the surface of the blade shaft body (1).

2. The coated knife shaft according to claim 1, characterized in that: The outer diameter of the coated knife shaft is 0.77-0.79 mm, wherein the outer diameter of the coated knife shaft is measured by the diameter of the largest circumscribed circle where the outer ends of the diamond abrasive particles are located.

3. The coated knife shaft according to any one of claims 1 or 2, characterized in that: The solder used to manufacture the soldering sublayer (21) is selected from a copper-based alloy solder containing active elements, a silver-based alloy solder containing active elements, and a nickel-based alloy solder containing active elements, and the active elements include titanium and chromium.

4. A method for manufacturing the coated blade shaft according to any one of claims 1 to 3, characterized in that: The method comprises: Step 1, pre-treating the blade shaft body (1) to remove grease and other dirt on the surface, and evenly mixing diamond abrasive grains and brazing material to obtain a mixed material; Step 2, installing the blade shaft body (1) processed in step 1 in a brazing mold, wherein there is a gap between the blade shaft body (1) and the brazing mold, and adding the mixture prepared in step 1 into the gap; Step 3, in an aerobic environment, heating the mold installed with the blade shaft body (1) and the brazing material obtained in step 2; Step 4, in an oxygen-free environment, continuing to heat the workpiece obtained in step 3; Step 5, using physical vapor deposition to produce a titanium carbide sublayer on the surface of the workpiece obtained in step 4; Step 6, removing the titanium carbide deposited on the surface of the diamond abrasive in the workpiece obtained in step 5, so that the diamond abrasive protruding from the titanium carbide sublayer is partially exposed, and the outer diameter of the obtained coated knife shaft is uniform; wherein in step 1, the weight ratio of the diamond abrasive to the brazing material is 1:(3-30); In step 3, the mold obtained in step 2 and equipped with the blade shaft body (1) and the brazing material is heated to 50° C. to 150° C. and kept at this temperature for 5 to 10 minutes; In step 4, the workpiece obtained in step 3 is further heated to 800° C. to 1100° C. and kept at this temperature for 10s to 60s; After completing steps 1 to 6, continue to perform steps 1 to 6 on the surface of the diamond abrasive grain layer to obtain a coated blade shaft having multiple layers of diamond abrasive grain layers.

Citation Information

Patent Citations

  • Abrasive-bladed multiple cutting wheel assembly

    CN1229709A

  • Radial polycrystalline diamond bearing for spiral drilling rig transmission shaft

    CN201915843U

  • Surface enhanced polycrystalline diamond composite cutters

    US5833021A

  • Abrasive tool with knurled surface

    US5997597A