A solar cell using an amorphous silicon passivation layer and a method for manufacturing the same

By employing a stepped structure and hydrogen doping of the amorphous silicon passivation layer in the solar cell, the problem of poor surface passivation effect was solved, the cell efficiency was improved, and the effectiveness of current harvesting was ensured.

CN109950352BActive Publication Date: 2024-11-08TONGWEI SOLAR ENERGY (CHENGDU) CO LID
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201910328496.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2019-04-23
Publication Date
2024-11-08
Estimated Expiration
2039-04-23

AI Technical Summary

Technical Problem

Existing solar cells have poor surface passivation, resulting in low cell conversion efficiency, especially at the metal-semiconductor interface where current collection is hindered.

Method used

An amorphous silicon passivation layer is used, which forms a stepped structure of N+-a-Si/Nc-Si/Pc-Si/P+-a-Si or P+-a-Si/Pc-Si/Nc-Si/N+-a-Si. This is combined with the field-effect passivation and chemical passivation effects of hydrogen-doped amorphous silicon to avoid direct contact between the metal electrode and the crystalline silicon.

Benefits of technology

It significantly improves the surface passivation effect of solar cells, reduces the loss of cell efficiency due to surface recombination, and ensures effective current collection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN109950352B_ABST
    Figure CN109950352B_ABST
Patent Text Reader

Abstract

The invention discloses a solar cell using an amorphous silicon passivation layer and a manufacturing method thereof, and belongs to the field of solar cells, and specifically relates to a solar cell with a special passivation layer. The technical scheme comprises a substrate layer, an amorphous silicon layer arranged on the upper and lower sides of the substrate layer, a transparent conductive oxide layer arranged on the amorphous silicon layer, and a metal electrode arranged on the outer surface of the transparent conductive oxide layer; the substrate layer is a P-type single crystal silicon wafer, the amorphous silicon layer comprises a first N-type doping layer and a first P-type doping layer arranged in sequence along the upper and lower surfaces of the P-type single crystal silicon wafer, the first N-type doping layer comprises an N+-a-Si doping layer and an N-c-Si doping layer arranged in sequence from top to bottom, and the first P-type doping layer is a P+-a-Si doping layer; the invention provides a solar cell using an amorphous silicon passivation layer and a manufacturing method thereof, which utilizes the good field effect passivation effect and chemical passivation effect of the hydrogenated doped amorphous silicon layer, can achieve a good surface passivation effect, and improve the cell efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of solar cells, and in particular relates to a solar cell using an amorphous silicon passivation layer and a manufacturing method thereof. Background Art

[0002] The efficiency of traditional crystalline silicon solar cells has increased rapidly in recent years. The market demand and expectations for high-efficiency batteries are getting higher and higher. Various new technologies and new structures have been adopted in the recent production of high-efficiency batteries, such as heterojunction structure (HIT) and tunnel oxide passivation contact (TOPCon) structure.

[0003] The surface recombination of minority carriers accounts for a large proportion of the efficiency loss of solar cells. In various new high-efficiency solar cells, great attention is paid to the surface passivation of solar cells. Generally, the passivation methods are generally divided into two types according to their working principles: chemical passivation and field effect passivation. Chemical passivation reduces surface recombination by saturating the dangling bonds on the surface, and field effect passivation reduces the recombination of minority carriers by establishing an electric field at the surface to repel minority carriers. Hydrogenated silicon nitride film and aluminum oxide film are both commonly used passivation coatings with good passivation effects.

[0004] Existing passivation coatings are usually not specifically doped, and often use the charge characteristics or chemical passivation characteristics of the coating itself in the process to passivate the surface. The passivation effect is still not ideal, especially at the metal-semiconductor contact interface. Silicon nitride and aluminum oxide coatings are not conductive, so they cannot exist at the metal-semiconductor contact position, otherwise it will hinder current collection. The surface recombination of the metal and crystalline silicon contact area will cause a certain loss of the passivation effect of the coating. Summary of the invention

[0005] The purpose of the present invention is to solve the problem that the surface passivation effect of solar cells in the prior art is not good and the conversion efficiency of the cells is not good. A solar cell using an amorphous silicon passivation layer and a manufacturing method thereof are provided. The good field effect passivation effect and chemical passivation effect of the hydrogenated doped amorphous silicon layer are utilized to achieve a good surface passivation effect and improve the cell efficiency.

[0006] The technical solution adopted by the present invention is as follows:

[0007] A solar cell using an amorphous silicon passivation layer comprises a base layer, an amorphous silicon layer arranged on the upper and lower sides of the base layer, a transparent conductive oxide layer arranged on the amorphous silicon layer, and a metal electrode arranged on the outer surface of the transparent conductive oxide layer; the base layer is a P-type single crystal silicon wafer, the amorphous silicon layer comprises a first N-type doping layer and a first P-type doping layer arranged in sequence along the upper and lower surfaces of the P-type single crystal silicon wafer, the first N-type doping layer comprises an N+-a-Si doping layer and an Nc-Si doping layer arranged in sequence from top to bottom, and the first P-type doping layer is a P+-a-Si doping layer.

[0008] Furthermore, the base layer is an N-type single crystal silicon wafer, the amorphous silicon layer includes a second P-type doped layer and a second N-type doped layer sequentially arranged along the upper and lower surfaces of the N-type single crystal silicon wafer, the second P-type doped layer includes a P+-a-Si doped layer and a Pc-Si doped layer sequentially arranged from top to bottom, and the second N-type doped layer is a P+-a-Si doped layer.

[0009] Furthermore, both the N+-a-Si doped layer and the P+-a-Si doped layer are hydrogenated doped amorphous silicon layers.

[0010] Furthermore, the thickness of the base layer is 160-200 um.

[0011] Furthermore, the thickness of the amorphous silicon layer is 20-50 nm.

[0012] A method for manufacturing a solar cell using an amorphous silicon passivation layer, wherein the manufacturing process comprises the following steps:

[0013] (1) Cleaning and texturing: The silicon wafer raw material is cleaned and processed into a base layer with a velvet structure.

[0014] (2) Diffusion: The surface of the P-type or N-type silicon wafer substrate layer that has been prepared with a texture is doped with N-type or P-type to form a PN junction.

[0015] (3) Cleaning: Cleaning the P-type or N-type silicon wafer substrate layer after N-type or P-type doping to remove the dead layer and oxide layer formed on the surface during the diffusion process.

[0016] (4) Plating amorphous silicon layer: P-type and N-type doped amorphous silicon layers are deposited on the upper and lower surfaces of the N-type or P-type doped layer, respectively, and hydrogen doping is performed. The thickness of the amorphous silicon layer is 20-50nm, and the doping concentration is 10 20 -10 21 cm -3 .

[0017] (5) TCO layer plating: The amorphous silicon layer in step (4) is electroplated with a TCO layer by using Sputtering or RPD (reactive plasma deposition).

[0018] (6) Preparation of metal electrodes: Metal electrodes are prepared on the TCO layer in step (5) by screen printing, electroplating or smart wires to collect current.

[0019] In summary, due to the adoption of the above technical solution, the beneficial effects of the present invention are:

[0020] In the present invention, the P-type doped and N-type doped amorphous silicon layers are used as passivation coatings, and a step-change structure of N+-a-Si / Nc-Si / Pc-Si / P+-a-Si or P+-a-Si / Pc-Si / Nc-Si / N+-a-Si is formed on the battery structure, forming a good field effect passivation, and the hydrogenated amorphous silicon can also produce a chemical passivation effect on the surface of the crystalline silicon, which can greatly reduce the loss of the battery efficiency caused by the surface recombination. At the same time, the metal electrode has no direct contact with the crystalline silicon, and will not destroy the overall passivation effect of the amorphous silicon layer. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 It is a schematic diagram of the structure of a P-type solar cell panel of the present invention.

[0022] Figure 2 This is a schematic diagram of the structure of an N-type solar cell panel of the present invention.

[0023] Markings in the figure: 1-base layer, 2-amorphous silicon layer, 3-transparent conductive oxide layer, 4-metal electrode, 5-first N-type doping layer, 6-first P-type doping layer, 7-N+-a-Si doping layer, 8-Nc-Si doping layer, 10-second P-type doping layer, 11-second N-type doping layer. DETAILED DESCRIPTION

[0024] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0025] A solar cell using an amorphous silicon passivation layer comprises a substrate layer 1, an amorphous silicon layer 2 arranged on the upper and lower sides of the substrate layer 1, a transparent conductive oxide layer 3 arranged on the outer surface of the amorphous silicon layer 2, and a metal electrode 4 arranged on the outer surface of the transparent conductive oxide layer 3; the substrate layer 1 is a P-type single crystal silicon wafer, the amorphous silicon layer 2 comprises a first N-type doping layer 5 and a first P-type doping layer 6 arranged in sequence along the upper and lower surfaces of the P-type single crystal silicon wafer, the first N-type doping layer 5 comprises an N+-a-Si doping layer 7, an Nc-Si doping layer 8 and a N+-a-Si doping layer 9 arranged in sequence from top to bottom Doping layer 8, the first P-type doping layer 6 is a P+-a-Si doping layer; the P-type doped and N-type doped amorphous silicon layers are used as passivation coatings, and a step-change structure of N+-a-Si / Nc-Si / Pc-Si / P+-a-Si or P+-a-Si / Pc-Si / Nc-Si / N+-a-Si is formed on the battery structure, forming a good field effect passivation, and hydrogenated amorphous silicon can also produce a chemical passivation effect on the surface of crystalline silicon, which can greatly reduce the loss of surface recombination to battery efficiency. At the same time, the metal electrode has no direct contact with the crystalline silicon, and will not destroy the overall passivation effect of the amorphous silicon layer.

[0026] Preferably, the base layer 1 is an N-type single crystal silicon wafer, and the amorphous silicon layer 2 includes a second P-type doping layer 10 and a second N-type doping layer 11 arranged in sequence along the upper and lower surfaces of the N-type single crystal silicon wafer, the second P-type doping layer 10 includes a P+-a-Si doping layer and a Pc-Si doping layer arranged in sequence from top to bottom, and the second N-type doping layer is an N+-a-Si doping layer.

[0027] Preferably, the N+-a-Si doped layer and the P+-a-Si doped layer are both hydrogenated doped amorphous silicon layers.

[0028] Preferably, the thickness of the base layer is 160-200 um.

[0029] Preferably, the amorphous silicon layer has a thickness of 20-50 nm.

[0030] A method for manufacturing a solar cell using an amorphous silicon passivation layer as claimed in any one of claims 1 to 5, characterized in that the manufacturing process comprises the following steps:

[0031] (1) Cleaning and texturing: The silicon wafer raw material is cleaned and processed into a base layer with a velvet structure. After cleaning, the original silicon wafer is prepared with a special velvet structure to increase the light absorption rate. The velvet structure includes but is not limited to pyramid and inverted pyramid shapes.

[0032] (2) Diffusion: The surface of the P-type or N-type silicon wafer substrate layer that has been textured is doped with N-type or P-type to form a PN junction. The surface of the P-type or N-type silicon wafer substrate layer that has been textured is doped with N-type or P-type to form a PN junction. The doping methods include but are not limited to liquid source high temperature diffusion and ion implantation.

[0033] (3) Cleaning: Cleaning the P-type or N-type silicon wafer substrate layer after N-type or P-type doping to remove the dead layer and oxide layer formed on the surface during the diffusion process.

[0034] (4) Plating amorphous silicon layer: P-type and N-type doped amorphous silicon layers are deposited on the upper and lower surfaces of the N-type or P-type doped layer, respectively, and hydrogen doping is performed. The thickness of the amorphous silicon layer is 20-50nm, and the doping concentration is 10 20 -10 21 cm -3 , ensuring a good passivation effect. The thickness of the amorphous silicon layer cannot be too thick, so as not to absorb too much incident light and affect the battery efficiency. The deposition method includes but is not limited to PECVD (plasma enhanced chemical vapor deposition) and Cat-CVD (catalytic chemical vapor deposition).

[0035] (5) Plating TCO layer: The TCO layer is a transparent conductive oxide layer. It can collect carriers by utilizing its good conductivity. Its good light transmittance can ensure that most incident light can be used to generate photogenerated carriers. The thickness is 30-80nm. The amorphous silicon layer in step (4) is electroplated with the TCO layer by sputtering or RPD (reactive plasma deposition).

[0036] (6) Preparation of metal electrodes: Prepare metal electrodes on the TCO layer to collect current. The electrode and TCO have good ohmic contact. The metal electrodes are prepared on the TCO layer in step (5) by screen printing, electroplating or smart wires to collect current.

[0037] Example 1

[0038] A solar cell using an amorphous silicon passivation layer comprises a substrate layer 1, an amorphous silicon layer 2 arranged on the upper and lower sides of the substrate layer 1, a transparent conductive oxide layer 3 arranged on the outer surface of the amorphous silicon layer 2, and a metal electrode 4 arranged on the outer surface of the transparent conductive oxide layer 3; the substrate layer 1 is a P-type single crystal silicon wafer, the amorphous silicon layer 2 comprises a first N-type doping layer 5 and a first P-type doping layer 6 arranged in sequence along the upper and lower surfaces of the P-type single crystal silicon wafer, the first N-type doping layer 5 comprises an N+-a-Si doping layer 7, an Nc-Si doping layer 8 and a N+-a-Si doping layer 9 arranged in sequence from top to bottom Doping layer 8, the first P-type doping layer 6 is a P+-a-Si doping layer; the P-type doped and N-type doped amorphous silicon layers are used as passivation coatings, and a step-change structure of N+-a-Si / Nc-Si / Pc-Si / P+-a-Si or P+-a-Si / Pc-Si / Nc-Si / N+-a-Si is formed on the battery structure, forming a good field effect passivation, and hydrogenated amorphous silicon can also produce a chemical passivation effect on the surface of crystalline silicon, which can greatly reduce the loss of surface recombination to battery efficiency. At the same time, the metal electrode has no direct contact with the crystalline silicon, and will not destroy the overall passivation effect of the amorphous silicon layer.

[0039] Example 2

[0040] On the basis of Example 1, the base layer 1 is an N-type single crystal silicon wafer, the amorphous silicon layer 2 includes a second P-type doping layer 10 and a second N-type doping layer 11 arranged in sequence along the upper and lower surfaces of the N-type single crystal silicon wafer, the second P-type doping layer 10 includes a P+-a-Si doping layer and a Pc-Si doping layer arranged in sequence from top to bottom, and the second N-type doping layer is an N+-a-Si doping layer.

[0041] Example 3

[0042] On the basis of Example 2, the N+-a-Si doping layer and the P+-a-Si doping layer are both hydrogenated doped amorphous silicon layers.

[0043] Example 4

[0044] Based on the above embodiment, a method for manufacturing a solar cell using an amorphous silicon passivation layer is provided, wherein the manufacturing process comprises the following steps:

[0045] (1) Cleaning and texturing: The silicon wafer raw material is cleaned and processed into a base layer with a velvet structure. After cleaning, the original silicon wafer is prepared with a special velvet structure to increase the light absorption rate. The velvet structure includes but is not limited to pyramid and inverted pyramid shapes.

[0046] (2) Diffusion: The surface of the P-type or N-type silicon wafer substrate layer that has been textured is doped with N-type or P-type to form a PN junction. The surface of the P-type or N-type silicon wafer substrate layer that has been textured is doped with N-type or P-type to form a PN junction. The doping methods include but are not limited to liquid source high temperature diffusion and ion implantation.

[0047] (3) Cleaning: Cleaning the P-type or N-type silicon wafer substrate layer after N-type or P-type doping to remove the dead layer and oxide layer formed on the surface during the diffusion process.

[0048] (4) Plating amorphous silicon layer: P-type and N-type doped amorphous silicon layers are deposited on the upper and lower surfaces of the N-type or P-type doped layer, respectively, and hydrogen doping is performed. The thickness of the amorphous silicon layer is 30nm and the doping concentration is 10 20 cm -3 , to ensure a good passivation effect. The thickness of the amorphous silicon layer cannot be too thick, so as not to absorb too much incident light and affect the battery efficiency. Deposition method PECVD (plasma enhanced chemical vapor deposition).

[0049] (5) Plating TCO layer: The TCO layer is a transparent conductive oxide layer. It can collect carriers by utilizing its good conductivity. Its good light transmittance can ensure that most incident light can be used to generate photogenerated carriers. The thickness is 50nm. The amorphous silicon layer in step (4) is electroplated with the TCO layer by sputtering.

[0050] (6) Preparation of metal electrodes: Prepare metal electrodes on the TCO layer to collect current. The electrode and TCO have good ohmic contact. Smart wires are used to prepare metal electrodes on the TCO layer in step (5) to collect current.

[0051] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A solar cell using an amorphous silicon passivation layer, characterized in that: The invention comprises a base layer (1), an amorphous silicon layer (2) arranged on the upper and lower sides of the base layer (1), a transparent conductive oxide layer (3) arranged on the outer surface of the amorphous silicon layer (2), and a metal electrode (4) arranged on the outer surface of the transparent conductive oxide layer (3); the base layer (1) is a P-type single crystal silicon wafer; the amorphous silicon layer (2) comprises a first N-type doping layer (5) and a first P-type doping layer (6) arranged in sequence along the upper and lower surfaces of the P-type single crystal silicon wafer; the first N-type doping layer (5) comprises an N+-a-Si doping layer (7) and an Nc-Si doping layer (8) arranged in sequence from top to bottom; the first P-type doping layer (6) is a P+-a-Si doping layer; N+-a-Si / Nc-Si / Pc-Si / P+-a-Si are formed on the battery structure; the N+-a-Si doping layer and the P+-a-Si doping layer are both hydrogenated doped amorphous silicon layers; the doping concentration is 10 20 -10 21 cm -3 .

2. A solar cell using an amorphous silicon passivation layer, characterized in that: The invention comprises a base layer (1), an amorphous silicon layer (2) arranged on the upper and lower sides of the base layer (1), a transparent conductive oxide layer (3) arranged on the outer surface of the amorphous silicon layer (2), and a metal electrode (4) arranged on the outer surface of the transparent conductive oxide layer (3); the base layer (1) is an N-type single crystal silicon wafer; the amorphous silicon layer (2) comprises a second P-type doping layer (10) and a second N-type doping layer (11) arranged in sequence along the upper and lower surfaces of the N-type single crystal silicon wafer; the second P-type doping layer (10) comprises a P+-a-Si doping layer and a Pc-Si doping layer arranged in sequence from top to bottom; the second N-type doping layer is an N+-a-Si doping layer; a step-change structure of P+-a-Si / Pc-Si / Nc-Si / N+-a-Si is formed on the battery structure; the N+-a-Si doping layer and the P+-a-Si doping layer are both hydrogenated doped amorphous silicon layers; the doping concentration is between 10 20 -10 21 cm -3 .

3. A solar cell using an amorphous silicon passivation layer as claimed in claim 1 or 2, characterized in that: The thickness of the base layer is 160-200 μm.

4. A solar cell using an amorphous silicon passivation layer as claimed in claim 1 or 2, characterized in that: The thickness of the amorphous silicon layer is 20-50 nm.

5. A method for manufacturing a solar cell using an amorphous silicon passivation layer according to any one of claims 1 to 4, characterized in that: The manufacturing process includes the following steps: (1) Cleaning and texturing: The silicon wafer raw material is cleaned and processed into a base layer with a velvet structure; (2) Diffusion: N-type or P-type doping is performed on the surface of the P-type or N-type silicon wafer substrate layer after the texture is prepared to form a PN junction; (3) Cleaning: Cleaning the P-type or N-type silicon wafer substrate layer after N-type or P-type doping to remove the dead layer and oxide layer formed on the surface during the diffusion process; (4) Plating an amorphous silicon layer: depositing a P-type and N-type doped amorphous silicon layer on the upper and lower surfaces of the N-type or P-type doped layer, respectively, and performing hydrogenation doping. The thickness of the amorphous silicon layer is 20-50 nm; (5) TCO layer plating: the amorphous silicon layer in step (4) is electroplated with a TCO layer by sputtering or reactive plasma deposition; (6) Preparation of metal electrodes: Metal electrodes are prepared on the TCO layer in step (5) by screen printing or electroplating to collect current.