Method for manufacturing semiconductor device and semiconductor device manufactured using the method
By using the atomic layer deposition method on the semiconductor layer and increasing the precursor injection pressure, the problem of difficult insulating layer uniformity on the nano-scale semiconductor layer is solved, and the uniformity of the insulating layer and process efficiency are improved.
Patent Information
- Application Number
- CN201910757073.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2018-08-17
- Filing Date
- 2019-08-16
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2039-08-16
AI Technical Summary
There is difficulty in uniformly forming an insulating layer on a nano-scale semiconductor layer, and the prior art is difficult to ensure the uniformity of the insulating layer and shorten the process time and cost.
By using an atomic layer deposition (ALD) method on the semiconductor layer, the injection pressure of the precursor is increased, the adsorption density of the precursor is ensured, thereby improving the uniformity of the insulating layer, and forming an insulating layer with a desired thickness by repeated cycles.
The uniformity of the insulating layer is improved, the number of process cycles is reduced, the process time and cost is shortened, and the uniformity and thickness of the insulating layer is ensured.
Smart Images

Figure CN110838431B_ABST
Abstract
Description
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims priority to and the benefit of Korean Patent Application No. 10-2018-0096142 filed in the Korean Intellectual Property Office on August 17, 2018, the contents of which are incorporated herein by reference in their entirety. Technical Field
[0003] Embodiments of the present disclosure relate to a method for manufacturing a semiconductor device and a semiconductor device manufactured using the method, and more particularly, to a method for manufacturing a semiconductor device that forms a uniform insulating layer on a semiconductor layer by using an atomic layer deposition (ALD) method, and a semiconductor device manufactured by the method. Background Art
[0004] Semiconductor materials having a layered structure are flexible and transparent, and thus are attracting attention as next-generation semiconductor materials. In this case, a thin film such as an insulating layer is uniformly formed on a nano-scale semiconductor layer.
[0005] Atomic layer deposition is a method of sequentially injecting one or more reactants into a reaction chamber and depositing a thin film in atomic layer units by adsorption of each reactant. After the precursor is adsorbed on the substrate surface, the film is formed by surface reactions between other reactants and surface particles. Summary of the invention
[0006] An embodiment of the present disclosure may provide a method for manufacturing a semiconductor device and a semiconductor device manufactured by using the method, wherein the method for manufacturing a semiconductor device may save process time and process cost while ensuring the uniformity of an insulating layer by increasing the injection pressure of a precursor in an atomic layer deposition process for forming an insulating layer on a semiconductor layer.
[0007] A method for manufacturing a semiconductor device according to an exemplary embodiment of the present disclosure includes: forming a semiconductor layer on a substrate in a chamber; and forming an insulating layer on the semiconductor layer; and wherein forming the insulating layer includes: (a) injecting a precursor including a metal into a surface of the semiconductor layer; (b) removing unadsorbed precursors; (c) injecting reactants onto the surface of the semiconductor layer; and (d) removing residual reactants, wherein the semiconductor layer includes a semiconductor material having a layered structure.
[0008] The semiconductor material may include at least one of a transition metal dichalcogenide (TMDC), graphene, and black phosphorus. 2 A chemical formula of , wherein M is one of Mo, W, Zr and Re, and X is one of S, Se and Te.
[0009] The precursor may be injected at a pressure of about 0.01 Torr to about 100 Torr.
[0010] The insulating layer includes M 1 x O a and M 1 x M 2 y O a An oxide represented by one of the following, represented by M 1 x N b The nitride represented by M 1 x O a N b In this case, M 1 and M 2 is a metal, and x>0, y>0, a>0 and b>0.
[0011] The insulating layer may include Al 2 O 3 、ZrO 2 , HfO 2 , Y 2 O 3 ,La 2 O 3 、 2 O.Ta 2 O 5 , MgO, ZnO, TiO 2 , Nb 2 O 5 、SiO 2 , TiN, SiN, HfON, SiON and STO (SrTiO 3 ) at least one of.
[0012] The insulating layer may have a thickness of about 0.5 nm to about 4 nm.
[0013] The insulating layer may include at least one atomic layer.
[0014] The precursor may include the same metal as that included in the insulating layer.
[0015] The precursor may include AlCl 3 、AlMe 3 (trimethylaluminum (TMA)), AlMe 2 Cl、AlMe 2 OiPr、AlEt 3 、Al(OnPr) 3 、Me 3 N:AlH3 、AlMe 2 H, Me 2 EtN:AlH 3 、ZrCl 4 、ZrI 4 、ZrCp 2 Cl 2j 、Zr(OiPr) 2 (dmae (dimethylaminoethanol)) 2 、Zr(OtBu) 4 、Zr(NMe 2 ) 4 、HfCl 4 、HfI 4 、HfCl 2 [N(SiMe 3 ) 2 2 、Hf(OtBu) 4 、Hf(OtBu) 2 (mmp) 2 、Hf(mmp) 4 、Hf(ONEt 2 ) 4 、Hf(NMe 2 ) 4 、Hf(NO 3 ) 4 、YCp 3 、Y(CpMe) 3 、Y(thd) 3 、La(thd) 3 、La[N(SiMe 3 ) 2 3 、TaF 5 、TaCl 5 、TaI 5 、Ta(OEt) 5 、Ta(OEt) 4 (dmae), Ta(NMe 2 ) 5 、Ta(NMe 2 ) 5 、Ta(NEt)(NEt 2 ) 3 、Ta(NEt 2 ) 5 、Ta(NtBu)(tBu 2 pz) 3 、Ta(NtBu)(iPrAMD) 2 NMe 2 、MgCp 2 Mg(thd) 2 、ZnCl 2 、ZnMe 2 、ZnEt 2 、Zn(OAc) 2 、TiCl 4 、TiI 4 、Ti(OMe) 4 、Ti(OiPr) 4 、SiCl 4 、SiCl 3 H、SiCl 2 H 2 、Si(OEt) 4 、HMDSh(hexamethylenediaminethiol), Si(NCO) 4 、MeOSi(NCO) 3 、Si 2 Cl 6 and SiH 4 At least one of .
[0016] The semiconductor layer may have a thickness of less than about 1 nm.
[0017] The reactant may be an oxidizing agent.
[0018] The step (a) may include: adsorbing the metal of the precursor to the surface of the semiconductor layer, and the step (c) may include: forming an insulating layer on the surface of the semiconductor layer by a reaction between the metal of the precursor and the reactant.
[0019] A method for manufacturing a semiconductor device according to an exemplary embodiment of the present disclosure includes: forming a semiconductor layer on a substrate in a chamber; and forming an insulating layer on the semiconductor layer, wherein forming the insulating layer includes: (a) injecting a precursor including a metal into a surface of the semiconductor layer; (b) removing unadsorbed precursors; (c) injecting reactants onto the surface of the semiconductor layer; and (d) removing residual reactants, wherein the density of the precursor adsorbed onto the surface of the semiconductor layer is increased by increasing the injection pressure of the precursor, wherein the precursor is injected at a pressure of about 0.1 Torr to about 10 Torr.
[0020] The semiconductor layer may include at least one of a transition metal dichalcogenide (TMDC) having a layered structure, graphene, and black phosphorus.
[0021] The surface roughness of the surface of the semiconductor layer in contact with the insulating layer is approximately 2 nm to 3.2 nm, and the surface roughness can be calculated by calculating multiple absolute values of vertical heights from the center lines of n curves on the surface, calculating the average of the squares of the multiple absolute values, and taking the positive square root of the average.
[0022] The insulating layer may include Al2 O 3 、ZrO 2 , HfO 2 , Y 2 O 3 ,La 2 O 3 、 2 O.Ta 2 O 5 , MgO, ZnO, TiO 2 , Nb 2 O 5 、SiO 2 , TiN, SiN, HfON, SiON and STO (SrTiO 3 ) at least one of.
[0023] The precursor may include AlCl 3 、AlMe 3 (trimethylaluminum (TMA)), AlMe 2 Cl、AlMe 2 OiPr、AlEt 3 、Al(OnPr) 3 、Me 3 N:AlH 3 、AlMe 2 H.Me 2 EtN:AlH 3 、ZrCl 4 , ZrI 4 , ZrCp 2 Cl 2j 、Zr(OiPr) 2 (dmae(dimethylethanolamine)) 2 、Zr(OtBu) 4 、Zr(NMe 2 ) 4 , HfCl 4 , HfI 4 , HfCl 2 [N(SiMe 3 ) 2 ] 2 、Hf(OtBu) 4 、Hf(OtBu) 2 (mmp) 2 、Hf(mmp) 4 、Hf(ONEt 2 ) 4 、Hf(NMe 2 ) 4 、Hf(NO 3 ) 4 , YCp3 , Y(CpMe) 3 , Y(thd) 3 , La(thd) 3 , La[N(SiMe 3 ) 2 3 , TaF 5 , TaCl 5 , TaI 5 , Ta(OEt) 5 , Ta(OEt) 4 (dmae), Ta(NMe 2 ) 5 , Ta(NMe 2 ) 5 , Ta(NEt)(NEt 2 ) 3 , Ta(NEt 2 ) 5 , Ta(NtBu)(tBu 2 pz) 3 , Ta(NtBu)(iPrAMD) 2 NMe 2 , MgCp 2 , Mg(thd) 2 , ZnCl 2 , ZnMe 2 , ZnEt 2 , Zn(OAc) 2 , TiCl 4 , TiI 4 , Ti(OMe) 4 , Ti(OiPr) 4 , SiCl 4 , SiCl 3 H, SiCl 2 H 2 , Si(OEt) 4 , HMDSh (hexamethylenediamine thiol), Si(NCO) 4 , MeOSi(NCO) 3 , Si 2 Cl 6 and SiH 4 and at least one of
[0024] A semiconductor device according to an exemplary embodiment of the present disclosure includes a substrate, a semiconductor layer arranged on the substrate, and an insulating layer arranged on the semiconductor layer, wherein the semiconductor layer includes a semiconductor material having a layered structure, the surface roughness of the surface of the semiconductor layer in contact with the insulating layer is approximately 2 nm to 3.2 nm, and the surface roughness is calculated by calculating multiple absolute values of vertical heights from the center lines of n curves on the surface, calculating an average of the squares of the multiple absolute values, and taking the positive square root of the average.
[0025] The semiconductor layer may include at least one of a transition metal dichalcogenide (TMDC) having a layered structure, graphene, and black phosphorus, wherein the TMDC has MX 2 A chemical formula wherein M is one of Mo, W, Zr and Re, and X is one of S, Se and Te, and the insulating layer may include Al 2 O 3 、ZrO 2 , HfO 2 , Y 2 O 3 ,La 2 O 3 、 2 O.Ta 2 O 5 , MgO, ZnO, TiO 2 , Nb 2 O 5 、SiO 2 , TiN, SiN, HfON, SiON and STO (SrTiO 3 ) at least one of.
[0026] The semiconductor layer may have a thickness of less than about 0.6 nm, and the insulating layer may have a thickness of about 0.5 nm to about 3.5 nm.
[0027] According to the method for manufacturing a semiconductor device disclosed in the present invention, the uniformity of the insulating layer formed by atomic layer deposition on the semiconductor layer can be improved by increasing the injection pressure of the precursor. In addition, the insulating layer can be uniformly deposited using fewer cycles, thereby shortening the process time and process cost. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 , Figure 2 , Figure 3 , Figure 4 and Figure 5 is a cross-sectional view illustrating a method of manufacturing a semiconductor device according to an exemplary embodiment.
[0029] Figure 6 , Figure 7 , Figure 8 , Fig. 9 and Fig.10 is a cross-sectional view illustrating a method of manufacturing a semiconductor device according to an exemplary embodiment.
[0030] Fig.11 , Fig.12 , Fig.13 and Fig.14 are cross-sectional views of various semiconductor devices that may be manufactured by methods according to example embodiments.
[0031] Fig.15 , Fig.16 and Fig.17 are atomic force microscope (AFM) images showing the surface roughness of the semiconductor layer under different precursor injection pressures.
[0032] Fig.18 and Fig.19 are AFM images and image diagrams showing the deposition extent of the insulating layer at different pressures. DETAILED DESCRIPTION
[0033] Hereinafter, embodiments of the present disclosure will be described more fully with reference to the accompanying drawings showing exemplary embodiments of the present disclosure. It will be appreciated by those skilled in the art that the exemplary embodiments may be modified in various different ways without departing from the spirit or scope of the present disclosure.
[0034] The drawings and description are to be regarded as illustrative in nature, and not restrictive. Like reference numerals may refer to like elements throughout the specification.
[0035] Since the size and thickness of each configuration shown in the drawings are arbitrarily indicated for better understanding and ease of description, the present disclosure is not limited to what is shown in the drawings, and the thickness of layers, films, panels, regions, etc. may be exaggerated for clarity.
[0036] It will be understood that when an element such as a layer, film, region, or substrate is referred to as being “on” another element, it can be directly on the other element or intervening elements may also be present.
[0037] In the following, reference will be made to Figures 1 to 4 A method for manufacturing a semiconductor device according to an exemplary embodiment is described. Figure 1 , Figure 2 , Figure 3 and Figure 4 is a cross-sectional view illustrating a method of manufacturing a semiconductor device according to an exemplary embodiment.
[0038] Reference Figure 1According to an exemplary embodiment, a substrate including a semiconductor layer 10 is disposed in a chamber, and then a precursor 20 for forming an insulating layer is injected onto the semiconductor layer 10. During the injection of the precursor 20, a metal element 21 of the precursor 20 is adsorbed and thus combined with the surface of the semiconductor layer 10. In this case, some of the precursor 20 may exist without being adsorbed into the surface of the semiconductor layer 10.
[0039] The semiconductor layer 10 according to the exemplary embodiment includes a semiconductor having a layered structure. For example, the semiconductor layer 10 includes at least one of transition metal dichalcogenide (TMDC), graphene, and black phosphorus.
[0040] TMDC is available in the chemical formula MX 2 In the chemical formula, M is one selected from Mo, W, Zr and Re, and X is one selected from S, Se and Te. For example, the chemical formula may be MoS 2 or WSe 2 .
[0041] The precursor 20 according to the exemplary embodiment includes a metal element 21 and at least one ligand 22. The metal element 21 is one selected from Al, Zr, Hf, Y, La, Ta, Mg, Zn, Ti, and Si, but the embodiment is not limited thereto.
[0042] The precursor 20 may include, for example, AlCl 3 、AlMe 3 (trimethylaluminum (TMA)), AlMe 2 Cl、AlMe 2 OiPr、AlEt 3 、Al(OnPr) 3 、Me 3 N:AlH 3 、AlMe 2 H.Me 2 EtN:AlH 3 、ZrCl 4 , ZrI 4 , ZrCp 2 Cl 2j 、Zr(OiPr) 2 (dmae(dimethylethanolamine)) 2 、Zr(OtBu) 4 、Zr(NMe 2 ) 4 , HfCl 4 , HfI 4 , HfCl 2 [N(SiMe 3 ) 2 ]2 、Hf(OtBu) 4 、Hf(OtBu) 2 (mmp) 2 、Hf(mmp) 4 、Hf(ONEt 2 ) 4 、Hf(NMe 2 ) 4 、Hf(NO 3 ) 4 、YCp 3 、Y(CpMe) 3 、Y(thd) 3 、La(thd) 3 、La[N(SiMe 3 ) 2 ] 3 、TaF 5 、TaCl 5 、TaI 5 、Ta(OEt) 5 、Ta(OEt) 4 (dmae)、Ta(NMe 2 ) 5 、Ta(NMe 2 ) 5 、Ta(NEt)(NEt 2 ) 3 、Ta(NEt 2 ) 5 、Ta(NtBu)(tBu 2 pz) 3 、Ta(NtBu)(iPrAMD) 2 NMe 2 、MgCp 2 、Mg(thd) 2 、ZnCl 2 、ZnMe 2 、Znet 2 、Zn(OAc) 2 、TiCl 4 、TiI 4 、Ti(OMe) 4 、Ti(OiPr) 4 、SiCl 4 、SiCl 3 H、SiCl 2 H 2 、Si(OEt) 4 HMDSh (HMDSh) Si(NCO) 4 、MeOSi(NCO) 3 ,Flaw2 Cl 6 and SiH 4 At least one of .
[0043] In this case, OiPr is Oi-Pr, where i-Pr is an isopropyl group -CH(CH 3 ) 2 , OnPr is n-propanol (OnPr), Cp is cyclopentadienyl (C 5 H 5-x R x ), Ot can be ethoxy, tert-butoxy, tert-pentyloxy, etc., mmp is 2,2,6,6-tetramethylheptane-3,5-dione, Nt can be collectively referred to as acylamino (such as ethylmethylamide (NEtMe), dimethylamide (MMe2), diacetylamino (NEt2)), tBu is tert-butoxy, pz is pyrazole, AMD is tetrakis (N,N'-dimethylacetamidine), and Ac is acetylacetonate.
[0044] In this case, according to the exemplary embodiment, the amount of the precursor 20 adsorbed to the semiconductor layer 10 by the metal element 21 of the precursor 20 may be increased by increasing the injection pressure of the precursor 20. Since the amount of the precursor 20 is increased, deposition of an insulating layer to be described below may be caused over a wider area of the surface of the semiconductor layer 10, and uniformity of the insulating layer may be ensured.
[0045] According to an exemplary embodiment, the injection pressure of the precursor 20 has a range of about 0.01 Torr to about 100 Torr, and depending on the embodiment, the range may be up to about 0.1 Torr to about 10 Torr. Figures 15 to 19 The injection pressure of the precursor 20 is described in detail.
[0046] Next, according to an exemplary embodiment, an inert gas is injected into the chamber. The inert gas includes at least one of Ar, N2, and a mixed gas thereof. The injected inert gas is used to remove any precursor 20 that is not adsorbed to the surface of the semiconductor layer 10 and any impurities in the chamber from the chamber.
[0047] Then, according to an exemplary embodiment, Figure 2 As shown in FIG. 1 , the precursor 20 combined with the semiconductor layer 10 remains on the semiconductor layer 10. In this case, the inert gas still remains in the chamber.
[0048] Then, according to an exemplary embodiment, Figure 3 As shown in FIG. 1 , a reactant 50 including a first element 51 and a second element 52 is injected into the chamber. The reactant 50 chemically reacts with the precursor 20 adsorbed to the surface of the semiconductor layer 10 .
[0049] Specifically, according to the exemplary embodiment, a portion of the ligand 22 coupled to the precursor 20 is separated, and the metal element 21 of the precursor 20 and the first element 51 of the reactant 50 react with each other. In addition, the ligand 22 of the precursor 20 and the second element 52 of the reactant 50 chemically react with each other, so that the reaction product 60 can be formed.
[0050] In this case, according to an exemplary embodiment, reactant 50 is a 2 O, O 2 and O 3 In addition, the reactant 50 includes O 2 Plasma, NH 3 Plasma, N 2 or H 2 Plasma and NH 3 At least one of the gases, but the embodiment is not limited thereto. The first element 51 and the second element 52 in the reactant 50 may be the same as or different from each other. The reactant 50 facilitates nucleation of the precursor 20 adsorbed to the semiconductor layer 10.
[0051] Next, according to an exemplary embodiment, an inert gas (such as Ar or N 2 ) removes the unreacted reactants 50 and reaction products 60 from the chamber. Then, as Figure 4 As shown in FIG, only the metal element 21 and the first element 51 adsorbed on the surface of the semiconductor layer 10 remain. In this case, the inert gas may still remain in the chamber.
[0052] Next, refer to Figure 5 According to an exemplary embodiment, by repeatedly performing (a) Figure 1 The precursor 20 is injected, (b) Figure 2 Removal of the unadsorbed precursor 20, (c) Figure 3 The injection of reactants 50 and (d) Figure 4 Any residual reactant 50 is removed to form a uniform insulating layer 80. The repetitive execution from (a) to (d) is one cycle of the ALD method, and the insulating layer 80 having a desired thickness can be formed by repeating the cycle at least once.
[0053] According to an exemplary embodiment, the insulating layer 80 is a thin film having a thickness of about 0.5 nm to about 4 nm depending on a deposition area of the surface of the semiconductor layer 10 .
[0054] exist Figure 5 In the embodiment, according to the exemplary embodiment, the insulating layer 80 includes two atomic layers, but the embodiment is not limited thereto. The insulating layer 80 includes one or more atomic layers. Alternatively, the insulating layer 80 includes a plurality of atomic layers each including a different material.
[0055] According to an exemplary embodiment, the insulating layer 80 is a 1 x O a and M 1 x M 2 y O a An oxide of one of the 1 x N b Nitride or such as M 1 x O a N b In this case, x>0, y>0, a>0 and b>0 are satisfied.
[0056] According to an exemplary embodiment, the insulating layer 80 includes, for example, Al 2 O 3 、ZrO 2 , HfO 2 , Y 2 O 3 ,La 2 O 3 、 2 O.Ta 2 O 5 , MgO, ZnO, TiO 2 , Nb 2 O 5 、SiO 2 , TiN, SiN, HfON, SiON and STO (SrTiO 3 These materials are formed into thin films using an ALD method.
[0057] In an exemplary embodiment, the precursor 20 includes the same metal as the insulating layer 80. That is, when the insulating layer 80 has a metal such as M 1 O a 、M 1 x M 2 y O a 、M 1 N b or M 1 O a N b When the chemical formula is, the metal element 21 of the precursor 20 includes the metal included in the insulating layer 80 (ie, M 1 or M 2 The precursor 20 serves as a metal source for the insulating layer 80 , which causes adsorption of the insulating layer 80 to the surface of the semiconductor layer 10 .
[0058] According to an exemplary embodiment, the uniformity of the insulating layer 80 is determined by the surface roughness (R q ) indicates. The following will refer to Figures 15 to 19 The uniformity and surface roughness R of the insulating layer 80 q The relationship between them is described in detail.
[0059] In the above exemplary embodiment, the precursor 20 and the reactant 50 are injected in an amount of about 1 sccm to about 500 sccm. In addition, in the method for manufacturing a semiconductor device according to the exemplary embodiment, steps (a) to (d) are performed at a temperature of about 100° C. to about 600° C. Depending on the material of the insulating layer 80 to be deposited, steps (a) to (d) are performed at a temperature of about 300° C. to about 500° C. The above-mentioned injection gas amount and process performance temperature are not limited and may vary in other embodiments of the present disclosure.
[0060] In the following, reference will be made to Figures 6 to 10 A method of manufacturing a semiconductor device according to an exemplary embodiment is described. Figure 6 , Figure 7 , Figure 8 , Fig. 9 and Fig.10 is a cross-sectional view showing a method of manufacturing a semiconductor device according to an exemplary embodiment. Figures 6 to 10 In an exemplary embodiment, the insulating layer includes Al 2 O 3 , and the precursor uses AlMe 3 (trimethylaluminum; TMA), and will now Figures 1 to 5 The exemplary embodiments of the present invention are described in more detail. Figures 1 to 5 The parts that are different from the exemplary embodiment of the present invention are described, and the parts whose description is omitted are the same as those of the above-described exemplary embodiment.
[0061] Reference Figure 6 According to an exemplary embodiment, each of the Al element 21' and the methyl group -CH 3 22' as a ligand precursor AlMe 3 (TMA) 20' is injected into the chamber. The injected precursor AlMe 3 20 ′ reacts with hydroxyl groups —OH 30 on the surface of the semiconductor layer 10 . The hydroxyl groups —OH 30 include oxygen ions 31 and hydrogen ions 32 .
[0062] Specifically, according to an exemplary embodiment, the precursor AlMe 325' combines with the oxygen ions 31 of the hydroxyl groups 30 at the surface of the semiconductor layer 10 and is adsorbed to the surface of the semiconductor layer 10. In addition, the precursor AlMe 3 The detached methyl groups 22' of 20' chemically react with the hydrogen ions 32 of the hydroxyl groups 30 at the surface of the semiconductor layer 10 to form a reaction product methane 60'. The chemical reaction formula of this reaction is shown in Chemical Formula 1.
[0063] Chemical formula 1:
[0064] -OH+Al(CH 3 ) 3 →-O+Al(CH 3 ) 2 +CH 4 .
[0065] In this case, by increasing the precursor AlMe 3 20' injection pressure to increase the adsorption of the precursor AlMe on the surface of the semiconductor layer 10 3 That is, the AlMe precursor adsorbed on the surface of the semiconductor layer 10 3 The number of 25' increases, and thus the insulating layer made therefrom can be formed uniformly.
[0066] Next, according to an exemplary embodiment, Ar or N 2 The inert gas is injected into the chamber to remove the residual precursor AlMe that is not adsorbed on the surface of the semiconductor layer 10. 3 (TMA)20' and the reaction product CH 4 60' of impurities.
[0067] Then, according to an exemplary embodiment, Figure 7 As shown in 3 The portion of 25 ′ that is bonded to the oxygen ions 31 on the surface of the semiconductor layer 10 remains on the semiconductor layer 10 .
[0068] Next, according to an exemplary embodiment, referring to Figure 8 , the reactants H including oxygen (O) 51' and hydrogen (H) 52' 2 O50' is injected into the chamber. The injected reactant H 2 O 50' reacts with the precursor 25' adsorbed to the surface of the semiconductor layer 10. In this case, the precursor 25' includes a compound that separates at least one methyl group 22' from the Al element 21'.
[0069] Specifically, according to an exemplary embodiment, the methyl group 22' is separated from the precursor 25', and the Al element 21' of the precursor 25' and the reactant H 2O 50' and oxygen 51' react with each other, so that the hydroxyl group 30 is combined with the Al element 21'. In addition, according to an exemplary embodiment, the methyl group 22' separated from the precursor 25' reacts with the reactant H 2 O 50' and hydrogen 52' react to form reaction product 60'. Reaction product 60' may be CH 4 , CH 3 or C 2 H 6 The chemical reaction formula of this reaction is chemical formula 2.
[0070] Chemical formula 2:
[0071] Al(CH 3 ) 2 +H 2 O→AlOH+CH 4 +CH 3 .
[0072] Next, the unreacted reactant H 2 O 50' and the reaction product CH 4 60' By injecting Ar or N into the chamber 2 of inert gas and removed from the chamber.
[0073] Then, according to an exemplary embodiment, Fig. 9 As shown in FIG. 8 , the insulating layer 80 ′ is formed to include Al elements 21 ′, oxygen 51 ′, and hydroxyl groups 30 combined with oxygen ions 31 at the surface of the semiconductor layer 10 .
[0074] According to an exemplary embodiment, repeatedly performing Figure 6 AlMe 3 20' injection, Figure 7 AlMe 3 20' removal and Figure 8 The reactant H 2 O 50' is implanted, so that a uniform Al 2 O 3 Insulation layer 80', such as Fig. 9 as shown in .
[0075] Using the above ALD method to form Al 2 O 3 The reaction of the insulating layer 80' can be represented by the reaction formula of Chemical Formula 3. In this case, H 2 Not present Fig. 9 Shown in.
[0076] Chemical formula 3:
[0077] 2Al(CH 3 ) 2 +3H 2 O→Al 2 O 3 +4CH 4 +H 2 .
[0078] Reference Fig.10 According to an exemplary embodiment, by repeatedly performing a cycle exceeding a predetermined number of times, Al 2 O 3 The insulating layer 80' is formed to a desired thickness. Fig.10 In, Al 2 O 3 The insulating layer 80' includes two Al 2 O 3 Atomic layer, but the embodiment is not limited thereto. 2 O 3 The insulating layer 80' may include one or more Al 2 O 3 Molecular layer.
[0079] According to an exemplary embodiment, Al 2 O 3 The insulating layer 80 ′ is a thin film having a thickness of about 0.5 nm to about 3.5 nm.
[0080] In addition, according to an exemplary embodiment, Al 2 O 3 The insulating layer 80' may be a single layer or have multiple layers. Figures 6 to 10 In the exemplary embodiment, the insulating layer 80 ′ includes Al 2 O 3 , but the embodiment is not limited thereto. The insulating layer 80' may include a plurality of layers each including a different material. For example, the insulating layer 80' may have a 2 O 3 The layers include HfO 2 The multiple layers are formed by the layers.
[0081] In the following, reference will be made to Figures 11 to 14 A semiconductor device according to an exemplary embodiment is described. Fig.11 , Fig.12 , Fig.13 and Fig.14 are cross-sectional views of various semiconductor devices that may be manufactured by methods according to example embodiments.
[0082] Fig.11 is a cross-sectional view of a semiconductor device having a bottom-gate structure in which a gate electrode is arranged below a semiconductor layer.
[0083] according to Fig.11 The semiconductor device of the exemplary embodiment includes a substrate 110 , a buffer layer 120 , a first gate electrode 124 , a first gate insulating layer 141 , a semiconductor layer 131 , a source electrode 133 , and a drain electrode 135 .
[0084] According to example embodiments, the substrate 110 may include glass or a transparent material including Si as a main component. However, embodiments are not limited thereto, and the substrate 110 may include various materials such as transparent plastic or metal.
[0085] According to an exemplary embodiment, the buffer layer 120 is disposed on the substrate 110. The buffer layer 120 prevents impurity ions from diffusing into the semiconductor device and prevents moisture or air from penetrating into the semiconductor device, and planarizes a surface of the semiconductor device.
[0086] According to an exemplary embodiment, the first gate electrode 124 is disposed on the buffer layer 120. The first gate insulating layer 141 includes silicon nitride (SiN x ) or silicon oxide (SiO x ) and is disposed on the first gate electrode 124. The semiconductor layer 131 includes a semiconductor material having a layered structure and is disposed on the first gate insulating layer 141. The semiconductor layer 131 includes at least one of transition metal dichalcogenide (TMDC), graphene, black phosphorus, and the like.
[0087] According to an exemplary embodiment, the semiconductor layer 131 has a thickness less than about 1 nm. In particular, when the semiconductor layer 131 includes a transition metal dichalcogenide (TMDC), the thickness of the semiconductor layer 131 is less than about 0.6 nm.
[0088] According to example embodiments, the semiconductor layer 131 is formed by one of a chemical vapor deposition (CVD) process, a plasma enhanced chemical vapor deposition (PECVD) process, an atomic layer deposition (ALD) process, and a sputtering process.
[0089] According to example embodiments, the source electrode 133 and the drain electrode 135 are disposed on the semiconductor layer 131 .
[0090] According to an exemplary embodiment, the interlayer insulating layer 160 is disposed on the source electrode 133 and the drain electrode 135. The interlayer insulating layer 160 covers some exposed portions of the semiconductor layer 131. The interlayer insulating layer 160 protects the semiconductor layer 131.
[0091] The interlayer insulating layer 160 according to the exemplary embodiment includes a high dielectric material, and as described above, may be formed by the ALD method.
[0092] According to the exemplary embodiment, the semiconductor layer 131 includes a semiconductor material having a layered structure and having a nano-sized thickness, and thus is easily damaged. In addition, the semiconductor layer 131 has high surface stability and has no dangling bonds, so it may not adsorb the precursor onto its surface.
[0093] When using the atomic layer deposition method, the semiconductor device according to the exemplary embodiment receives a high precursor injection pressure, and thus may uniformly form the interlayer insulating layer 160 without damaging a shadow portion of the semiconductor layer 131 .
[0094] In the following, Figure 12 to Figure 14 In the Fig.11 Features of the exemplary embodiments differ from those of the exemplary embodiments described above, and parts of the description are omitted.
[0095] Fig.12 is a cross-sectional view of a semiconductor device having a double gate structure in which two gate electrodes are included in one semiconductor device.
[0096] Fig.12 The exemplary embodiment further includes a second gate electrode 125 and a second gate insulating layer 142 .
[0097] According to an exemplary embodiment, the interlayer insulating layer 160 is disposed on the semiconductor layer 131. In the present exemplary embodiment, the semiconductor layer 131 includes a channel region, a source region, and a drain region, and the source region and the drain region may be doped with n-type or p-type impurities.
[0098] According to an exemplary embodiment, the second gate electrode 125 is disposed on the interlayer insulating layer 160. The second gate insulating layer 142 is disposed on the second gate electrode 125. In addition, the second gate insulating layer 142 and the interlayer insulating layer 160 have contact holes penetrating therethrough. The source electrode 133 and the drain electrode 135 are electrically connected to the source region and the drain region of the semiconductor layer 131, respectively, through the contact holes.
[0099] In this case, the interlayer insulating layer 160 may be uniformly formed without damaging the shadow portion of the semiconductor layer 131 using the atomic layer deposition method according to the exemplary embodiment.
[0100] Fig.13 is a cross-sectional view of a semiconductor device having a top gate structure in which a gate electrode is arranged above a semiconductor layer.
[0101] exist Fig.13In the exemplary embodiment of the present invention, the semiconductor layer 131 is disposed on the buffer layer 120. The first gate insulating layer 141, the first gate electrode 124 and the interlayer insulating layer 160 are sequentially disposed on the semiconductor layer 131. The interlayer insulating layer 160 includes a contact hole. The source electrode 133 and the drain electrode 135 are electrically connected to the source region and the drain region of the semiconductor layer 131, respectively, through the contact holes.
[0102] In this case, the first gate insulating layer 141 may be uniformly formed without damaging the shadow portion of the semiconductor layer 131 using the atomic layer deposition method according to example embodiments.
[0103] Fig.14 Is with Fig.13 A cross-sectional view of a semiconductor device with the same top-gate structure, wherein the insulating layer has multiple layers.
[0104] Fig.14 The exemplary embodiment further includes a second gate insulating layer 142. The second gate insulating layer 142 is disposed on the first gate insulating layer 141. The first gate insulating layer 141 and the second gate insulating layer 142 include different materials. In the exemplary embodiment, the gate insulating layer is a double layer, but the embodiment is not limited thereto, and the gate insulating layer may include three or more layers.
[0105] In this case, the first gate insulating layer 141 may be uniformly formed without damaging the shadow portion of the semiconductor layer 131 using the atomic layer deposition method according to example embodiments.
[0106] According to an exemplary embodiment, since the second gate insulating layer 142 is arranged on the first gate insulating layer 141, unlike the first gate insulating layer 141 on the semiconductor layer 131, the second gate insulating layer 142 can be formed not only by the ALD method but also by a chemical vapor deposition (CVD) process, a low pressure chemical vapor deposition (LPCVD) process, etc.
[0107] In the following, reference is made to Figures 15 to 17 , the uniformity of an insulating layer formed by using an ALD method under different precursor injection pressures will be described. Fig.15 , Fig.16 and Fig.17 is an atomic force microscope (AFM) image depicting the surface roughness of the semiconductor layer under different precursor injection pressures. Hereinafter, the surface roughness is calculated by a root mean square method of calculating the average value of values obtained by squaring the original values and then taking the positive square root of the average value.
[0108] More specifically, according to an exemplary embodiment, Figures 15 to 17Figures 1 and 2 are AFM images of the precursor injection pressures at 0.05 Torr, 0.5 Torr, and 2.5 Torr when the ALD process was performed for 9 cycles. In this case, the semiconductor layer includes MoS 2 , the insulating layer includes Al 2 O 3 , and the precursor includes AlMe 3 (TMA). In the figure, the bright part indicates Al 2 O 3 The dark part indicates the deposition area of Al 2 O 3 non-deposition area.
[0109] Reference Fig.15 When the precursor is injected at an injection pressure of 0.05 Torr, the Al 2 O 3 Deposited only on MoS 2 On some parts of the surface of the semiconductor layer. 2 O 3 is formed unevenly at the surface of the semiconductor layer, and the surface roughness R q Measured to be 2nm.
[0110] Surface roughness represents the micro-deformation formed by the protrusions and depressions at the surface. In general, the surface roughness can be calculated by a curve representing a vertical section of the surface to be measured. The surface roughness can be calculated as the arithmetic mean of the absolute values of the vertical heights from the center line representing the average value of the curve to n curves (here, n>0). In this exemplary embodiment, the surface roughness is calculated by the root mean square method as described above.
[0111] Reference Fig.16 According to an embodiment, when the precursor is injected at an injection pressure of 0.5 Torr, the bright part is Fig.15 That is to say, it is determined that Al 2 O 3 It was observed that when the implantation pressure increased from 0.05 Torr to 0.5 Torr, the Al deposited 2 O 3 The area of the surface of the semiconductor layer gradually increases. In this case, as Al 2 O 3 The deposition increases, the convexities and concavities on the surface increase, and the surface roughness R q Measured to be 4.1 nm.
[0112] Reference Fig.17 According to an embodiment, when the precursor is injected at an injection pressure of 2.5 Torr, Al 2 O 3Deposited on almost every area of the surface of the semiconductor layer. Fig.15 and Fig.16 In contrast, Al is densely formed on the surface of the semiconductor layer. 2 O 3 , and it can be determined that the most uniform thin insulating layer is formed. In this case, the surface roughness R q Measured to be 3.2nm.
[0113] exist Figures 15 to 17 As the precursor injection pressure increases, the surface roughness R q Increases and then decreases, where the cycle is repeated the same number of times. This is because during the process of depositing the insulating layer to gradually cover the surface of the semiconductor layer, the convexity and concavity of the surface increase with repeated cycles until the non-deposition area of the insulating layer is larger than the deposition area, and then the convexity and concavity of the surface decrease as the deposition area grows beyond the non-deposition area. Accordingly, in Figures 15 to 17 Surface roughness R q It increases from 2nm to 4.1nm and then decreases to 3.2nm.
[0114] In this case, since the injection amount of the precursor is proportional to the product of the injection pressure and the injection time of the precursor, Fig.17 The injection pressure is 2.5 Torr, but when the injection pressure increases above 2.5 Torr, the surface roughness R q Reduced to 3.2nm or smaller.
[0115] In the following, reference is made to Fig.18 and Fig.19 , will be described in Figures 15 to 17 The exemplary embodiment cycles the uniformity of the insulation layer under different pressures at different cycles. Fig.18 and Fig.19 are AFM images and image diagrams showing the deposition extent of the insulating layer at different pressures.
[0116] More specifically, Fig.18 and Fig.19 An AFM image and an image diagram are shown when the atomic layer deposition method is performed at 15 cycles and the injection pressure of the precursor is 0.05 Torr and 0.5 Torr, respectively.
[0117] In the following, only Figures 15 to 17 Features different from those of the exemplary embodiments are described below, and parts of the description are omitted following the above-described exemplary embodiments.
[0118] Reference Fig.18 According to an embodiment, when the precursor is injected at an injection pressure of 0.05 Torr, Al 2 O 3Deposited only on a portion of the surface of the semiconductor layer. Fig.18 The lower image in the figure is obtained by using a specific analysis method Fig.18 The Al2O3 layer on the surface of the semiconductor layer is extracted from the AFM image at the top image. 2 O 3 The deposition area was measured to be 65%.
[0119] Reference Fig.19 According to an embodiment, when the precursor is injected at an injection pressure of 0.5 Torr, Al 2 O 3 Deposited over almost the entire surface area of the semiconductor layer. Fig.18 Compared with the deposition area, the deposition area increases. In the surface of the semiconductor layer, Al 2 O 3 The deposition area was measured to be 90%, and therefore, with an injection pressure of 0.05 Torr Fig.18 In contrast, the insulating layer may be uniformly formed at the surface of the semiconductor layer.
[0120] When compared Figures 15 to 17 Exemplary embodiments and Fig.18 and Fig.19 In the exemplary embodiment, since the number of cycles of the atomic layer deposition method is small, it can be determined that the high precursor injection pressure saturates the uniformity of the insulating layer. That is, when the injection pressure of the precursor according to the exemplary embodiment is increased, the insulating layer can be uniformly deposited with fewer cycles, thereby reducing the process time and process cost.
[0121] exist Fig.19 In an exemplary embodiment, when the atomic layer deposition method is repeated for 15 cycles, a precursor injection pressure of about 0.5 Torr enables the deposition area to reach about 90%, and thus the insulating layer can be uniformly formed. As the number of cycles increases, the precursor injection pressure that can ensure uniformity in the insulating layer can be reduced, and specifically, when the atomic layer deposition method is performed for about 50 cycles, the precursor injection pressure can be about 0.1 Torr. Therefore, the precursor injection pressure according to the exemplary embodiment can have a range from about 0.01 Torr to 100 Torr, and depending on the exemplary embodiment, the range can be between about 0.1 Torr and about 10 Torr.
[0122] According to an embodiment, the thin layered semiconductor material has high mobility, high on / off current ratio and high stability, and is also flexible and transparent. When the semiconductor layer includes a semiconductor material having a layered structure, a thin insulating layer can be formed on the semiconductor layer. Therefore, a thin film can be formed by an atomic layer deposition process using a precursor.
[0123] Since the insulating layer according to the exemplary embodiment has a thickness scale in the order of atomic layer units, the insulating layer may include a high-k material for dielectric constant and capacitance.
[0124] However, the layered semiconductor material has a stable surface, and thus chemical bonding cannot be easily ensured between the surface of the semiconductor layer and the precursor, and accordingly, a uniform insulating layer may not be formed on the semiconductor layer.
[0125] Generally, when an insulating layer is formed on a layered semiconductor layer, damage to the semiconductor layer may be caused or an unnecessary intermediate layer may be introduced.
[0126] However, in one embodiment, increasing the injection pressure of the precursor increases the bonding of the precursor to the surface of the semiconductor layer without damaging the semiconductor layer. Accordingly, the precursor, which is a source for forming the insulating layer, is uniformly formed on the surface of the semiconductor layer, and the uniformity of the insulating layer formed thereby can be improved. In addition, since the injection amount of the precursor increases with the injection pressure of the precursor, it is possible to use fewer atomic layer deposition cycles to deposit the insulating layer, thereby shortening the process time and process cost.
[0127] While embodiments of the present disclosure have been described in connection with what are presently considered to be practical exemplary embodiments, it is to be understood that the embodiments of the present disclosure are not limited to the exemplary embodiments, but, on the contrary, are intended to cover various modifications and equivalent arrangements included within the spirit and scope of the appended claims.
Claims
1. A method for manufacturing a semiconductor device, include: forming a semiconductor layer on a substrate in a chamber; as well as forming an insulating layer on the semiconductor layer, Wherein, forming the insulating layer comprises: (a) injecting a precursor comprising a metal and at least one ligand into the surface of the semiconductor layer, wherein the precursor reacts with hydroxyl groups on the surface of the semiconductor layer; (b) removing the precursor that is not adsorbed on the semiconductor layer, wherein only the portion of the precursor that is bound to the oxygen ion of the hydroxyl group remains on the semiconductor layer; (c) injecting a reactant onto the surface of the semiconductor layer, wherein the reactant includes a first element and a second element; and (d) removing residual reactants, wherein only the metal and the first element adsorbed on the surface of the semiconductor layer remain, wherein the ligand is separated from the precursor, the metal of the precursor and the first element of the reactant react with each other, and the ligand of the precursor and the second element of the reactant react with each other to form a reaction product, Wherein, the semiconductor layer comprises a semiconductor material having a layered structure, and Wherein, the surface roughness of the surface of the semiconductor layer in contact with the insulating layer is 2 nm to 3.2 nm under different precursor injection pressures.
2. The method for manufacturing a semiconductor device according to claim 1, in, The semiconductor material comprises at least one of a transition metal dichalcogenide, graphene and black phosphorus, wherein the transition metal dichalcogenide has MX 2 A chemical formula of , wherein M is one of Mo, W, Zr and Re, and X is one of S, Se and Te.
3. The method for manufacturing a semiconductor device according to claim 1, in, The precursor is injected at a pressure of 0.01 torr to 100 torr.
4. The method for manufacturing a semiconductor device according to claim 1, in, The insulating layer comprises M 1 x O a and M 1 x M 2 y O a An oxide represented by one of the following, represented by M 1 x N b The nitride represented by M 1 x O a N b At least one of the nitrogen oxides represented by Among them, M 1 and M 2 is a metal, and x>0, y>0, a>0 and b>0.
5. The method for manufacturing a semiconductor device according to claim 4, in, The insulating layer includes Al 2 O 3 、ZrO 2 , HfO 2 , Y 2 O 3 ,La 2 O 3 、 2 O.Ta 2 O 5 , MgO, ZnO, TiO 2 , Nb 2 O 5 、SiO 2 , TiN, SiN, HfON, SiON and SrTiO 3 At least one of .
6. The method for manufacturing a semiconductor device according to claim 1, in, The insulating layer has a thickness of 0.5 nm to 4 nm.
7. The method for manufacturing a semiconductor device according to claim 1, in, The insulating layer includes at least one atomic layer.
8. The method for manufacturing a semiconductor device according to claim 1, in, The precursor includes the same metal as a metal included in the insulating layer.
9. The method for manufacturing a semiconductor device according to claim 8, in, AlCl 3 、AlMe 3 、AlMe 2 Cl、AlMe 2 OiPr、AlEt 3 、Al(OnPr) 3 ,I 3 N:AlH 3 、AlMe 2 H、Me 2 EtN:AlH 3 、ZrCl 4 、ZrI 4 、ZrCp 2 Cl 2j 、Zr(OiPr) 2 (dmae) 2 、Zr(OtBu) 4 、Zr(NMe 2 ) 4 、HfCl 4 、HfI 4 、HfCl 2 [N(SiMe 3 ) 2 ] 2 、Hf(OtBu) 4 、Hf(OtBu) 2 (mmp) 2 、Hf(mmp) 4 、Hf(ONEt 2 ) 4 、Hf(NMe 2 ) 4 、Hf(NO 3 ) 4 、YCp 3 、Y(CpMe) 3 、Y(thd) 3 、La(thd) 3 、La[N(SiMe 3 ) 2 ] 3 、TaF 5 、TaCl 5 、TaI 5 、Ta(OEt) 5 、Ta(OEt) 4 (dmae)、Ta(NMe 2 ) 5 、Ta(NMe 2 ) 5 、Ta(NEt)(NEt 2 ) 3 , Ta(NEt 2 ) 5 , Ta(NtBu)(tBu 2 pz) 3 , Ta(NtBu)(iPrAMD) 2 NMe 2 , MgCp 2 , Mg(thd) 2 , ZnCl 2 , ZnMe 2 , ZnEt 2 , Zn(OAc) 2 , TiCl 4 , TiI 4 , Ti(OMe) 4 , Ti(OiPr) 4 , SiCl 4 , SiCl 3 H, SiCl 2 H 2 , Si(OEt) 4 , HMDSh, Si(NCO) 4 , MeOSi(NCO) 3 , Si 2 Cl 6 and SiH 4 at least one of 10. The method for manufacturing a semiconductor device according to claim 1, in, The semiconductor layer has a thickness of less than 1 nm.
11. The method for manufacturing a semiconductor device according to claim 1, in, The reactant is an oxidizing agent.
12. The method for manufacturing a semiconductor device according to claim 1, in, Step (a) comprises: adsorbing the metal of the precursor onto the surface of the semiconductor layer, and Step (c) comprises: The insulating layer is formed on the surface of the semiconductor layer by a reaction between the metal of the precursor and the reactant.
13. The method for manufacturing a semiconductor device according to claim 1, in, increasing the density of the precursor adsorbed to the surface of the semiconductor layer by increasing the injection pressure of the precursor, and The precursor is injected at a pressure of 0.1 torr to 10 torr.
14. The method for manufacturing a semiconductor device according to claim 1, in, The surface roughness is calculated by calculating a plurality of absolute values of vertical heights from center lines of n curves on the surface, calculating an average of squares of the plurality of absolute values, and taking a positive square root of the average. 15 . A semiconductor device manufactured by the method of manufacturing a semiconductor device according to claim 1 .